A fluorescent glass-ceramic, a method for preparing the same and a light emitting device
By combining zinc borosilicate glass powder with blue-green phosphor, a dense fluorescent glass ceramic was prepared, which solved the problems of low luminous efficiency and poor reliability of sky-blue LED devices and achieved a high-efficiency and stable sky-blue luminous effect.
Patent Information
- Application Number
- CN202511276504.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-09-08
AI Technical Summary
Existing azure LED devices suffer from low luminous efficiency, high cost, and poor reliability. In particular, colloidal yellowing at high temperatures leads to accelerated light decay and color coordinate drift, making it difficult to operate stably at high power.
By combining zinc borosilicate glass powder with blue-green phosphor and precisely controlling the ratio of glass powder to phosphor, a dense fluorescent glass ceramic is formed during low-temperature co-firing. Combined with a nanoparticle coating layer, the stability of the phosphor and the light conversion efficiency are ensured, thus achieving sky-blue luminescence.
It achieves efficient light conversion and accurate azure emission, improving the reliability and stability of the device, especially maintaining long-term luminescence performance in high temperature and high humidity environments, and reducing light decay and color coordinate drift.
Smart Images

Figure CN121318142B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of luminescent materials technology, and in particular to a fluorescent glass ceramic, its preparation method, and a luminescent device. Background Technology
[0002] Existing azure LED (light-emitting diode) devices mostly use azure LED chips, but they suffer from problems such as low luminous efficiency and high cost. Although the organic encapsulation solution of LED chip + phosphor + glue has a significant cost advantage, the glue is prone to yellowing when the device temperature is high, which leads to accelerated light decay, difficulty in effective heat dissipation, and causes thermal quenching of phosphor and color coordinate drift. This results in poor reliability and low power consumption. Summary of the Invention
[0003] This application provides a fluorescent glass ceramic, its preparation method, and a light-emitting device. The fluorescent glass ceramic prepared in this application has high reliability and can be applied to high-power light emission. The light-emitting device combined with a specific light source can achieve a precise sky-blue light emission effect. Its color coordinates based on the CIE1931 chromaticity diagram are located within a specific quadrilateral area, making it very suitable for fields such as sky-blue indicator lights for automotive assisted driving and autonomous driving.
[0004] In a first aspect, embodiments of this application provide a fluorescent glass-ceramic, comprising glass powder and phosphor; the glass powder comprises zinc borosilicate glass powder; the zinc borosilicate glass powder comprises the following components in molar percentage: 5%~20% SiO2, 10%~35% B2O3, 20%~65% ZnO, 0.3%~15% P2O5, 2%~20% RO, and 0.1%~15% R2O, wherein RO is selected from at least one of MgO, CaO, SrO, and BaO, and R2O is selected from at least one of Li2O, Na2O, and K2O; the phosphor comprises a blue-green phosphor; the blue-green phosphor has an emission peak wavelength of 480~510 nm; based on the total mass of the glass powder and the phosphor, the mass percentage of the glass powder is 30%~80%, and the mass percentage of the phosphor is 20%~70%.
[0005] In the above technical solution, zinc borosilicate glass powder serves as the matrix. Its specific composition and ratio ensure that the glass has a low softening point and good chemical stability, enabling densification at a relatively low sintering temperature and preventing damage to the phosphor during co-firing. The blue-green phosphor allows it to be effectively excited by common blue or near-ultraviolet LED chips, emitting blue-green light. When mixed with the emitted light from the light source, it achieves sky-blue emission. By adjusting the ratio of glass powder to phosphor, co-firing ensures no damage and balances the mechanical strength, light transmittance, and fluorescence conversion efficiency of the fluorescent glass ceramic, resulting in both good reliability and efficient light conversion, achieving precise sky-blue emission.
[0006] In some embodiments, the blue-green phosphor includes M a D b E c :xEu 2+ or BaSi2O2N2:Eu 2+ One of the following, wherein: M includes at least one of Sr, Ba, Ca, Mg, and Zn; D includes Al; E includes O; 3.7≤a≤4.3, 12≤b≤16, 22≤c≤28, and 0.01≤x≤0.5.
[0007] In the above technical solution, the physicochemical properties of the blue-green phosphor are stable and will not be damaged when co-fired with glass powder. It can be excited by the light emitted by the light source and emit blue-green light. By controlling its composition parameters, it is possible to obtain blue-green light with high brightness, good color purity, excellent stability and better thermal quenching performance. When mixed with the light emitted by the light source, the color coordinates of the light-emitting device can be precisely adjusted to the area required for sky blue, thus achieving sky blue light emission.
[0008] In some embodiments, D further includes at least one of B, Ga, or In, and E further includes at least one of F, Cl, Br, or I.
[0009] In the above technical solution, by doping elements and adjusting the proportions, the tunable spectral range is further expanded, the environmental adaptability is improved, the interaction between phosphor and glass powder is weakened when the phosphor is co-fired with glass powder, efficiency loss is reduced, and its luminescence performance is better maintained. While ensuring spectral accuracy, the long-term stability of luminescence is improved.
[0010] In some embodiments, the blue-green phosphor includes Sr 4-x Al 14 O 25 :xEu 2+ , where 0.02≤x≤0.3.
[0011] In the above technical solution, the phosphor exhibits stable physical and chemical properties, maintaining the integrity of its crystal structure and luminescent properties during sintering, thus ensuring that the final fluorescent glass-ceramic possesses high light conversion efficiency and reliability. The blue-green phosphor, upon excitation, produces characteristic blue-green fluorescence emission, with its spectral energy distribution highly overlapping with the azure color gamut. By mixing with light emitted from the light source, the color coordinates of the entire device's emitted light can be effectively and precisely anchored within the azure standard region.
[0012] In some embodiments, the phosphor further includes a green phosphor; the green phosphor satisfies at least one of the following conditions: (1) The emission peak wavelength of the green phosphor is 510~540 nm; (2) Green phosphors include β-Sialon:Eu 2+ AlON:Mn 2+ Lu3(Al,Ga)5O 12 :Ce 3+ Or (Ba,Sr)2SiO4:Eu 2+ Any one of them.
[0013] In the above technical solution, the synergistic effect of green phosphor and blue-green phosphor allows for further fine-tuning of the overall emission spectrum of the fluorescent glass ceramic, enabling precise design of the final device's emission color to meet specific requirements in different application scenarios. Green phosphor exhibits good thermal stability at relatively low sintering temperatures on zinc borosilicate glass substrates, effectively reducing thermal quenching and degradation of the phosphor during sintering. By adjusting the types and ratios of blue-green and green phosphors, accurate sky-blue emission can be achieved while maintaining the long-term reliability of the light-emitting device under high-temperature and high-humidity environments.
[0014] In some embodiments, the phosphor surface is coated with powder; the powder satisfies at least one of the following conditions: (1) The powder includes any one of aluminum oxide, silicon oxide, titanium dioxide, magnesium oxide, zinc oxide or boron nitride; (2) The particle size of the powder is 20~200 nm.
[0015] In the above technical solution, the nanoparticle coating layer (thickness of 80~500 nm) has high chemical inertness and thermal stability, which can form a dense physical barrier on the surface of phosphor particles. When co-sintered with glass powder at low temperature, it can effectively block the ion (especially alkali metal ion) in the glass matrix from eroding the phosphor, so that the phosphor can maintain high luminous efficiency and emission spectrum characteristics, and improve the thermal stability and service life of fluorescent glass ceramics.
[0016] Secondly, embodiments of this application provide a method for preparing fluorescent glass ceramics, comprising the following steps: mixing glass powder and phosphor powder and pressing them into shape, and then sintering them; based on the total mass of glass powder and phosphor powder, the mass percentage of glass powder is 30%~80%, and the mass percentage of phosphor powder is 20%~70%.
[0017] In the above technical solution, the glass powder fully melts and flows during sintering, forming a continuous, dense, and highly transparent glass matrix. This matrix effectively coats and protects the phosphor particles, ensuring uniform dispersion of the phosphor within the glass matrix, thereby obtaining a fluorescent glass-ceramic with uniform luminescence. The resulting glass-ceramic combines the density and chemical stability of glass with the rigidity of ceramics, significantly improving thermal stability, resistance to moisture erosion, and mechanical strength.
[0018] In some embodiments, sintering satisfies at least one of the following conditions: (1) The sintering temperature is 400~700 ℃; (2) The sintering time is 10 min to 2 h; (3) The sintering pressure is 1~20 MPa.
[0019] In the above technical solution, the sintering temperature ensures that the glass powder can fully soften and melt, obtaining sufficient fluidity to wet the phosphor particles, fill the voids, and form a dense and continuous glass matrix, minimizing the damage to the phosphor caused by high-temperature thermal effects. The sintering time ensures that the above melting, flow, and preliminary densification processes can be completed, reducing the significant thermal degradation of the phosphor caused by prolonged exposure to high temperatures, which would lead to a sharp decline in luminous efficiency and thermal stability. During the preparation process, because the phosphor has a higher volume ratio and the glass powder, acting as an inorganic binder, has a lower volume ratio, the density and strength of the fluorescent glass-ceramic can be improved by applying certain pressure during sintering.
[0020] Thirdly, embodiments of this application provide a light-emitting device, including a light source and the fluorescent glass ceramic described above or the fluorescent glass ceramic prepared by the above method, wherein the emission peak wavelength of the light source is 380~410 nm; or the emission peak wavelength of the light source is 430~460 nm.
[0021] In the above technical solution, the emission spectrum of the light source matches the excitation spectrum of the phosphor contained in the fluorescent glass ceramic, and can be efficiently absorbed by the phosphor in the fluorescent glass ceramic, thereby exciting the phosphor to emit light. The final emitted light of the light-emitting device is composed of the unabsorbed residual excitation light and the fluorescence emitted by the phosphor under stimulation, together achieving sky-blue light emission.
[0022] In some embodiments, the color coordinates of the emitted light from the light-emitting device in the CIE 1931 chromaticity diagram are located within a quadrilateral region bounded by points A (0.012, 0.495), B (0.200, 0.400), C (0.200, 0.320), and D (0.040, 0.320).
[0023] In the above technical solution, the color coordinates are limited to a specific quadrilateral area, ensuring that the light emitted by the light-emitting device is an accurate sky blue color. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 An optical microscope image of a fluorescent glass-ceramic provided in Embodiment 6 of this application; Figure 2 The coordinate position of a light-emitting device in the CIE1931 chromaticity diagram provided in this application. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0027] Currently, most azure LED devices use azure LED chips, but they suffer from low luminous efficiency and high cost. While the organic encapsulation solution of LED chip + phosphor + adhesive has a significant cost advantage, the adhesive is prone to yellowing under high-temperature operating conditions, leading to accelerated light decay. It also hinders effective heat dissipation, causing the phosphor to experience thermal quenching and color coordinate shift, ultimately resulting in decreased device reliability and difficulty in stable operation at high power.
[0028] To address the aforementioned technical problems, this application provides a fluorescent glass-ceramic, comprising glass powder and phosphor; the glass powder comprises zinc borosilicate glass powder; the zinc borosilicate glass powder comprises the following components in molar percentage: 5%~20% SiO2, 10%~35% B2O3, 20%~65% ZnO, 0.3%~15% P2O5, 2%~20% RO, and 0.1%~15% R2O, wherein RO is selected from at least one of MgO, CaO, SrO, and BaO, and R2O is selected from at least one of Li2O, Na2O, and K2O; the phosphor comprises a blue-green phosphor; the blue-green phosphor has an emission peak wavelength of 480~510 nm; based on the total mass of the glass powder and the phosphor, the mass percentage of the glass powder is 30%~80%, and the mass percentage of the phosphor is 20%~70%. By precisely controlling the mass ratio of the glass matrix to the phosphor, the phosphor is not damaged during the co-firing process. The resulting fluorescent glass ceramic has good mechanical strength, optical transmittance and fluorescence conversion efficiency. When matched with a suitable light source, it can achieve high-efficiency light conversion and precise sky-blue emission.
[0029] In some embodiments of this application, the blue-green phosphor includes M a D b E c :xEu 2+ or BaSi2O2N2:Eu 2+ One of the following, wherein: M includes at least one of Sr, Ba, Ca, Mg, and Zn; D includes Al; E includes O; 3.7 ≤ a ≤ 4.3, 12 ≤ b ≤ 16, 22 ≤ c ≤ 28, and 0.01 ≤ x ≤ 0.5. Specifically, x can be a value within the range of 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.2, 0.3, 0.4, 0.5, or any two of these. As an example, the blue-green phosphor includes Sr... 4- x Al 14 O 25 :xEu 2+ Where 0.02 ≤ x ≤ 0.3. For example, x can be a value within the range of 0.02, 0.04, 0.06, 0.08, 0.1, 0.14, 0.18, 0.22, 0.26, 0.3, or any two of these ranges. When x satisfies the above range, the blue-green phosphor exhibits excellent long-term stability, with significantly reduced light decay rate and color coordinate shift, ensuring that the final fluorescent glass ceramic has high light conversion efficiency and reliability.
[0030] In some embodiments of this application, D further includes at least one of B, Ga, or In, and E further includes at least one of F, Cl, Br, or I. By doping elements and adjusting their proportions, the tunable spectral range can be further expanded, environmental adaptability can be improved, and the decrease in phosphor luminescence efficiency during sintering can be reduced, thereby improving the long-term stability of luminescence while ensuring spectral accuracy.
[0031] In some embodiments of this application, the phosphor further includes a green phosphor; the green phosphor includes β-Sialon:Eu 2+ AlON:Mn 2+ Lu3(Al,Ga)5O 12 :Ce 3+ Or (Ba,Sr)2SiO4:Eu 2+The emission peak wavelength of the green phosphor is 510–540 nm, for example, it can be a value within the range of 510 nm, 515 nm, 520 nm, 525 nm, 530 nm, 535 nm, 540 nm, or any two of these. When the emission peak wavelength of the green phosphor meets the above range, its emission spectrum can achieve good matching with the emission spectrum of the light source and the emission spectrum of the blue-green phosphor, and the color coordinates of the resulting sky-blue emission can more accurately fall into the target area.
[0032] In some embodiments of this application, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 30% to 80%, and the mass percentage of blue-green phosphor is 20% to 70%.
[0033] In some embodiments of this application, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 30% to 80%, the mass percentage of blue-green phosphor is 10% to 40%, and the mass percentage of green phosphor is 10% to 30%.
[0034] Of course, in some embodiments of this application, to prevent the phosphor from being corroded and contaminated by ions (especially alkali metal ions) in the glass matrix during low-temperature co-sintering with glass powder, nanoparticles are coated on the surface of the phosphor; the powder includes any one of alumina, silicon dioxide, titanium dioxide, magnesium oxide, zinc oxide, or sodium boron nitride. The particle size of the powder is 20~200 nm, for example, it can be a value within the range of 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, or any two of these values.
[0035] In some embodiments of this application, the preparation method of fluorescent glass-ceramics includes the following steps: mixing glass powder and phosphor powder and pressing them into shape, followed by sintering; based on the total mass of glass powder and phosphor powder, the mass percentage of glass powder is 30%~80%, and the mass percentage of phosphor powder is 20%~70%. The prepared glass-ceramics combine the density and chemical stability of glass with the rigidity of ceramics, significantly improving thermal stability, resistance to moisture erosion, and mechanical strength.
[0036] Specifically, in this step, the sintering temperature is 400~700 ℃, for example, it can be a value within the range of 400 ℃, 450 ℃, 500 ℃, 550 ℃, 600 ℃, 650 ℃, 700 ℃, or any combination thereof. When the sintering temperature meets the above range, the glass powder can melt and flow, achieving effective coating of phosphor particles, while reducing the degree of phosphor degradation.
[0037] In some embodiments of this application, the sintering time is 10 min to 2 h, for example, it can be a value within the range of 10 min, 0.5 h, 1 h, 1.5 h, 2 h, or any two of these. When the sintering time meets the above range, the glass powder can be fully melted and flowed to form a dense, non-porous, continuous matrix, which then physically and chemically wets the phosphor particles, forming a firmly bonded interface.
[0038] In addition, in some embodiments of this application, the emission spectrum of the azure light-emitting device is close to that of a monochromatic spectrum. The amount of phosphor used in the preparation process is relatively large. Since the volume ratio of phosphor is large, the volume ratio of glass powder acting as an inorganic binder is small. In order to ensure the density and strength of the final fluorescent glass, a certain pressure is used in the sintering process to greatly improve the density and strength of the fluorescent glass. The sintering pressure is 1~20 MPa, for example, it can be a value within the range of 1 MPa, 2 MPa, 4 MPa, 6 MPa, 8 MPa, 10 MPa, 12 MPa, 14 MPa, 16 MPa, 18 MPa, 20 MPa or any two of them.
[0039] In some embodiments of this application, the light-emitting device includes a light source and the aforementioned fluorescent glass ceramic. The emission peak wavelength of the light source is 380~410nm, for example, it can be a value within the range of 380 nm, 382 nm, 385 nm, 390 nm, 395 nm, 400 nm, 405 nm, 410 nm, or any combination thereof. When the emission peak wavelength of the light source meets the above range, it can be efficiently absorbed by the phosphor and converted into a highly pure azure fluorescence. Furthermore, the emitted light of the light source is in the violet light region, which is insensitive to the human eye, and does not participate in the final color synthesis, ensuring that the emitted light is an accurate azure light.
[0040] In some embodiments of this application, the light-emitting device includes a light source and the aforementioned fluorescent glass-ceramic. The emission peak wavelength of the light source is 430~460nm, for example, it can be a value within the range of 430 nm, 435 nm, 440 nm, 445 nm, 450 nm, 455 nm, 460 nm, or any combination thereof. When the emission peak wavelength of the light source meets the above range, it can efficiently excite the phosphor to emit light. The partially transmitted blue light mixes with the light emitted by the phosphor and together displays a sky-blue color, which helps to improve the light color stability and long-term service life of the light-emitting device.
[0041] In some embodiments of this application, the color coordinates of the light emitted by the light-emitting device lie within the quadrilateral region enclosed by points A (0.012, 0.495), B (0.200, 0.400), C (0.200, 0.320), and D (0.040, 0.320) in the CIE 1931 chromaticity diagram, such as... Figure 2 As shown, the luminous color represented within this quadrilateral area is the azure color described in this application.
[0042] The following are definitions of terms used in this application: Emission peak wavelength: This refers to the wavelength at which the luminescence intensity of a luminescent material, such as a phosphor, quantum dot, semiconductor, or a light-emitting device reaches its maximum value in its emission spectrum. It represents the most dominant luminescent color of the material or device.
[0043] The CIE 1931 chromaticity diagram, developed by the International Commission on Illumination (CIE) in 1931, is a standard colorimetric system for quantitatively describing color and is a fundamental tool for characterizing color in color science and industry. By transforming the human eye's perception of different wavelengths of light into mathematical coordinates, the CIE 1931 chromaticity diagram achieves a precise definition and visual representation of color.
[0044] The present application will be further described in detail below with reference to the embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available products, and the devices or equipment used are all purchased from conventional market sales channels. In the specific embodiments of this application, the light source is an LED chip, and the LED device bracket is 2016.
[0045] Using an Oswell M330-M100 optical microscope with coaxial light as the light source, the microstructure of fluorescent glass-ceramic slides was observed and photographed. For example... Figure 1 The image shown is an optical microstructure image of the fluorescent glass-ceramic of Embodiment 6 of this application, wherein the continuous matrix is glass and the spherical particles are Lu3(Al,Ga)5O. 12 :Ce 3+ Green phosphor, rod-shaped particles are BaSi2O2N2:Eu 2+ Blue-green fluorescent powder.
[0046] The emission spectrum of the light-emitting device was tested using the HASS2000 LED photoelectric testing system from Yuanfang Optoelectronics. The color coordinates of the light-emitting device were obtained through its supporting software, and the color coordinate positions were marked on the CIE1931 chromaticity diagram.
[0047] Example 1 Fluorescent glass ceramics, including glass powder and phosphor; Zinc borosilicate glass powder comprises the following components in molar percentage: 10% SiO2, 25% B2O3, 45% ZnO, 10% P2O5, 5% MgO, and 5% Li2O. The phosphor is Sr4Al 14 O 25 Eu 2+The emission peak wavelength is 490 nm. The phosphor surface is coated with alumina powder with a particle size of 100 nm and the coating layer formed by the powder is about 300 nm thick. Based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 40% and the mass percentage of phosphor is 60%.
[0048] Preparation method of fluorescent glass ceramics: glass powder and fluorescent powder are mixed and pressed into shape, and then sintered at a temperature of 500 ℃ for 1 h and a sintering pressure of 2 MPa.
[0049] The sintered fluorescent glass-ceramic ingot is sliced, ground, and polished to obtain a fluorescent glass-ceramic substrate with a thickness of 0.15 mm. The fluorescent glass-ceramic substrate is then cut to obtain a fluorescent glass-ceramic sheet with a length × width of 1 mm × 1 mm. The fluorescent glass-ceramic sheet is then mounted on the light-emitting surface of an LED chip to obtain an LED lamp that emits sky-blue light. The emission peak wavelength of the LED chip is 450 nm.
[0050] Example 2 The difference from Example 1 is that the zinc borosilicate glass powder includes the following components in molar percentage: 10% SiO2, 25% B2O3, 45% ZnO, 10% P2O5, 5% CaO, and 5% Na2O.
[0051] Example 3 The difference from Example 1 is that the zinc borosilicate glass powder includes the following components in molar percentage: 15% SiO2, 20% B2O3, 33% ZnO, 12% P2O5, 10% CaO, and 10% Na2O.
[0052] Example 4 The difference from Example 1 is that the zinc borosilicate glass powder includes the following components in molar percentage: 15% SiO2, 20% B2O3, 33% ZnO, 12% P2O5, 10% MgO, and 10% Li2O.
[0053] Example 5 The difference from Example 1 is that, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 50%; the phosphor is Sr4Al. 14 O 25 Eu 2+ and β-Sialon:Eu 2+ Among them, Sr4Al 14 O 25 Eu 2+ The emission peak wavelength is 490 nm, and the mass percentage is 40%; β-Sialon:Eu2+ The emission peak wavelength is 530 nm, and the mass percentage is 10%.
[0054] Example 6 The difference from Example 1 is that, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 50%; the phosphor is BaSi2O2N2:Eu. 2+ and Lu3(Al,Ga)5O 12 :Ce 3+ Among them, BaSi2O2N2:Eu 2+ The emission peak wavelength is 485 nm, and the mass percentage content is 30%; Lu3(Al,Ga)5O 12 :Ce 3+ The emission peak wavelength is 525 nm, and the mass percentage is 20%.
[0055] Example 7 The difference from Example 1 is that, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 30% and the mass percentage of phosphor is 70%.
[0056] Example 8 The difference from Example 1 is that, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 80% and the mass percentage of phosphor is 20%.
[0057] Example 9 The difference from Example 1 is that the phosphor surface is coated with alumina powder with a particle size of 20 nm and the coating layer formed by the powder is about 100 nm thick.
[0058] Example 10 The difference from Example 1 is that the phosphor surface is coated with alumina powder with a particle size of 200 nm and the coating layer formed by the powder is about 400 nm thick.
[0059] Example 11 The difference from Example 1 is that the phosphor surface is coated with boron nitride powder with a particle size of 20 nm and the coating layer formed by the powder is about 80 nm thick.
[0060] Example 12 The difference from Example 1 is that the phosphor surface is coated with boron nitride powder with a particle size of 200 nm and the coating layer formed by the powder is about 500 nm thick.
[0061] Example 13 The difference from Example 1 is that in the fluorescent glass preparation method, the sintering temperature is 700 ℃, the sintering time is 10 min, and the sintering pressure is 1 MPa.
[0062] Example 14 The difference from Example 1 is that in the fluorescent glass preparation method, the sintering temperature is 400 ℃, the sintering time is 2 h, and the sintering pressure is 20 MPa.
[0063] Example 15 The difference from Example 1 is that the LED chip emission peak wavelength is 380 nm.
[0064] Example 16 The difference from Example 1 is that the emission peak wavelength of the LED chip is 410 nm.
[0065] Example 17 The difference from Example 1 is that the emission peak wavelength of the LED chip is 430 nm.
[0066] Example 18 The difference from Example 1 is that the LED chip emission peak wavelength is 460 nm.
[0067] Comparative Example 1 The LED chip is made of non-fluorescent glass ceramic with an emission peak wavelength of 495 nm. The LED device bracket is made of 2016, and the encapsulation adhesive is silicone.
[0068] Comparative Example 2 Phosphor: BaSi2O2N2:Eu with an emission peak wavelength of 485 nm 2+ And Lu3(Al,Ga)5O with an emission peak wavelength of 525 nm 12 :Ce 3+ .
[0069] LED chip: emission peak wavelength is 450 nm.
[0070] Phosphors and LED chips are combined to form a light-emitting device. The LED device bracket is 2016, and silicone is used as the encapsulating adhesive.
[0071] Comparative Example 3 The difference from Example 1 is that, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 20% and the mass percentage of phosphor is 80%.
[0072] Comparative Example 4 The difference from Example 1 is that, based on the total mass of glass powder and phosphor, the mass percentage of glass powder is 90% and the mass percentage of phosphor is 10%.
[0073] Test methods The light-emitting devices of Examples 1-18 and Comparative Examples 1-4 were tested to measure the color coordinates, luminous flux, light decay and color drift Dxy at 85 °C and 85% humidity for 1000 hours under the test current / voltage of 500 mA / 3 V.
[0074] The test results of Examples 1-18 and Comparative Examples 1-4 are shown in Table 1.
[0075] Table 1 Test results for each embodiment and comparative example
[0076] A comparison of Examples 1-18 and Comparative Examples 1-2 shows that although the light-emitting devices of Examples 1-18 and Comparative Examples 1-2 all emit azure light based on the CIE 1931 chromaticity diagram within a specific quadrilateral region, the luminous flux, 1000-hour light decay, and color drift of Examples 1-18 are superior to those of Comparative Examples 1-2. This indicates that the fluorescent glass ceramic of this application absorbs the light emitted by the LED chip more effectively, resulting in higher light conversion efficiency and less light loss. In particular, Examples 5 and 6, which use a mixed phosphor scheme, further enhance the luminous flux, significantly outperforming the silicone encapsulation scheme of Comparative Example 2. In high-temperature and high-humidity (85℃, 85% humidity) environments, the fluorescent glass ceramic, as an encapsulation material, exhibits better thermal stability and moisture resistance. Its dense inorganic structure effectively blocks water vapor and oxygen, protecting the phosphor from corrosion, thereby greatly improving the lifespan and reliability of the light-emitting device. In addition, the fluorescent glass-ceramic device of this application exhibits very stable color performance during long-term aging. This is due to the fact that the phosphor is firmly sintered in a stable glass matrix, avoiding color drift problems caused by the yellowing of silicone due to aging or the separation of phosphor from the encapsulation material.
[0077] By comparing Examples 1, 7, and 8 with Comparative Examples 3-4, it can be seen that the light-emitting devices of Examples 1, 7, and 8, based on the CIE 1931 chromaticity diagram, all have color coordinates within a specific quadrilateral region, emitting azure light and exhibiting good performance. However, the light-emitting devices of Comparative Examples 3-4, based on the CIE 1931 chromaticity diagram, do not have color coordinates within the specific quadrilateral region and cannot emit accurate azure light. Furthermore, the mass ratio of glass powder to phosphor is crucial for ensuring the overall performance of the light-emitting device. In Comparative Example 3, the glass powder content is too low, preventing the glass matrix from completely encapsulating the phosphor, resulting in reduced protection and increased light decay and color drift. In Comparative Example 4, the glass powder content is too high and the phosphor content is too low, leading to a significant decrease in luminous flux.
[0078] Through the comparison of the above embodiments and comparative examples, it can be clearly seen that the light-emitting device composed of fluorescent glass ceramic and a specific light source can provide an accurate sky blue light emission effect and has obvious advantages in terms of luminous efficiency and long-term light decay performance. By optimizing the ratio of glass powder to phosphor and adopting mixed phosphor and other technical solutions, the luminous efficiency, reliability and color stability of the light-emitting device can be further improved.
[0079] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A fluorescent glass-ceramic, characterized in that, It includes glass powder and phosphor; the glass powder and phosphor are mixed and pressed into shape, and then sintered; the sintering temperature is 400~700 ℃; The glass powder is zinc borosilicate glass powder; the zinc borosilicate glass powder is composed of the following components in molar percentage: 5%~20%SiO2, 10%~35%B2O3, 20%~65%ZnO, 0.3%~15%P2O5, 2%~20%RO, 0.1%~15%R2O, wherein RO is selected from at least one of MgO, CaO, SrO, and BaO, and R2O is selected from at least one of Li2O, Na2O, and K2O; The phosphor is composed of blue-green phosphor and green phosphor; the emission peak wavelength of the blue-green phosphor is 480~510 nm. Based on the total mass of the glass powder and the phosphor, the mass percentage of the glass powder is 30%~80%, the mass percentage of the blue-green phosphor is 10%~40%, and the mass percentage of the green phosphor is 10%~30%. The green phosphor satisfies at least one of the following conditions: (1) The emission peak wavelength of the green phosphor is 510~540 nm; (2) The green phosphor includes β-Sialon:Eu 2+ AlON:Mn 2+ Lu3(Al,Ga)5O 12 :Ce 3+ Or (Ba,Sr)2SiO4:Eu 2+ Any one of them.
2. The fluorescent glass-ceramic according to claim 1, characterized in that, The blue-green phosphor includes M a D b E c :xEu 2+ or BaSi2O2N2:Eu 2+ One of them, Wherein: M includes at least one of Sr, Ba, Ca, Mg, and Zn; D includes Al; E includes O; 3.7≤a≤4.3, 12≤b≤16, 22≤c≤28, 0.01≤x≤0.
5.
3. The fluorescent glass-ceramic according to claim 2, characterized in that, D also includes at least one of B, Ga, or In, and E also includes at least one of F, Cl, Br, or I.
4. The fluorescent glass-ceramic according to claim 2, characterized in that, The blue-green phosphor includes Sr 4- x Al 14 O 25 :xEu 2+ , where 0.02≤x≤0.
3.
5. The fluorescent glass-ceramic according to claim 1, characterized in that, The phosphor is coated with powder; the powder satisfies at least one of the following conditions: (1) The powder includes any one of aluminum oxide, silicon oxide, titanium dioxide, magnesium oxide, zinc oxide or boron nitride; (2) The particle size of the powder is 20~200 nm.
6. A method for preparing a fluorescent glass-ceramic as described in any one of claims 1 to 5, characterized in that, The process includes the following steps: mixing glass powder and phosphor, pressing them into shape, and then sintering them; the sintering temperature is 400~700 ℃; the phosphor is composed of blue-green phosphor and green phosphor; based on the total mass of the glass powder and the phosphor, the mass percentage of the glass powder is 30%~80%, the mass percentage of the blue-green phosphor is 10%~40%, and the mass percentage of the green phosphor is 10%~30%.
7. The method for preparing fluorescent glass-ceramics according to claim 6, characterized in that, The sintering satisfies at least one of the following conditions: (1) The sintering time is 10 min to 2 h; (2) The sintering pressure is 1~20 MPa.
8. A light-emitting device, characterized in that, The light source includes a fluorescent glass ceramic prepared by the method of any one of claims 1 to 5 or any one of claims 6 to 7, wherein the emission peak wavelength of the light source is 380 to 410 nm; or the emission peak wavelength of the light source is 430 to 460 nm.
9. The light-emitting device according to claim 8, characterized in that, The color coordinates of the emitted light from the light-emitting device in the CIE1931 chromaticity diagram are located within the quadrilateral area enclosed by points A (0.012, 0.495), B (0.200, 0.400), C (0.200, 0.320), and D (0.040, 0.320).
Citation Information
Patent Citations
Full-spectrum borosilicate fluorescent glass and preparation method thereof
CN110698073A
Cyan fluorescent glass, preparation method thereof and full-spectrum LED device thereof
CN111003933A