High-entropy doped niobium pentoxide nanoparticles, and methods of making and using the same
By using high-entropy-doped niobium pentoxide nanoparticles, the problems of insufficient electronic conductivity and energy storage sites in niobium-based oxide anode materials have been solved, achieving high rate performance and high specific capacity, making them suitable for high-power energy storage devices.
Patent Information
- Application Number
- CN202511602666.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-11-04
AI Technical Summary
Traditional niobium-based oxide anode materials have low electronic conductivity and insufficient energy storage sites, resulting in significant polarization effects at high rates, making it difficult to meet the requirements of high-power and high-safety lithium-ion batteries.
High-entropy doped niobium pentoxide nanoparticles are used, and Fe, Co, Ni, Cr and Al elements are doped to form a stable solid solution structure, which enhances electronic conductivity and lithium-ion diffusion rate. The preparation methods include hydrothermal method and sintering process.
It achieves high rate performance and high specific capacity. The nanoparticles retain 88% of their capacity at 10 C rate, and the lithium-ion diffusion coefficient is improved by two orders of magnitude, making it suitable for high-power energy storage devices.
Smart Images

Figure CN121361834B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery materials and electrochemical technology, specifically relating to a high-entropy doped niobium pentoxide nanoparticle, its preparation method, and its application. Background Technology
[0002] High-power lithium-ion batteries (fast charge / discharge) are increasingly in demand in fields such as high-speed drones, consumer electronics, new energy vehicles, and military equipment. Although traditional graphite anode lithium-ion batteries perform well in most scenarios, their slow electrochemical kinetics, poor rate performance, and safety hazards caused by lithium dendrites at the interface make them unsuitable for the demands of high-power, high-safety lithium-ion batteries. Therefore, Li4Ti5O4 batteries with a working potential range of 1-2 V (vs. Li+ / Li) are being developed. 12 Lithium has attracted much attention due to its ability to effectively avoid the risk of dendrite formation, but its 175 mAh g⁻¹... -1 Its low theoretical capacity limits its large-scale application.
[0003] In recent years, products with high specific capacity (>200 mAh g) have been developed. -1 Niobium-based oxides (such as T-Nb₂O₅ and TiNb₂O₇) have become a research hotspot. Among them, orthorhombic T-Nb₂O₅ exhibits exceptionally fast energy storage characteristics, with its lithium-ion intercalation rate increasing almost linearly with the scan rate, and has been applied in various energy storage device research. The crystal structure of T-Nb₂O₅ is exceptionally complex, consisting of an open framework structure formed by tilted NbO₆ octahedra and NbO₇ pentagonal bipyramidal structures, providing quasi-two-dimensional continuous channels for ion transport, enabling the material to achieve high-rate performance. However, the practical application of T-Nb₂O₅ still faces key challenges. First, its intrinsic electronic conductivity is low, leading to significant polarization effects at high rates, severely limiting the improvement of power density. Second, its limited bulk diffusion channels and energy storage sites prevent its capacity from reaching the level of graphite. Although carbon composites have increased the conductivity by several orders of magnitude, alleviating the electron transport limitation, they cannot overcome the bottleneck of bulk ion diffusion kinetics. The applicant's previous research showed that doping Co into T-Nb2O5 improved the electronic conductivity of T-Nb2O5 and excited Nb. 4+ / Nb 3+ The redox reaction improves the rate performance and specific capacity of the material. However, the results show that when the doping concentration is greater than 2%, impurity phases appear in T-Nb2O5, making it difficult to maintain the quasi-two-dimensional lithium-ion migration channels of Nb2O5. The high-entropy (HE) strategy, as a special doping method, can construct a stable host crystal structure by introducing multiple elements to increase the entropy value, showing significant effectiveness in enhancing the stability of layered cathode oxides and improving the conductivity of solid electrolytes. This provides a new approach for achieving high-concentration doped T-Nb2O5. Summary of the Invention
[0004] In view of the defects of low electronic conductivity and insufficient energy storage sites of existing fast-charging niobium-based oxide anode materials, the present invention provides a high-entropy doped niobium pentoxide nanoparticle and its preparation method and application, so as to realize precise occupation of Nb sites by doping atoms without causing phase separation, and simultaneously improve the electronic conductivity, lithium ion diffusion rate and specific capacity of the material, solving the core contradiction that the fast-charging performance and capacity of traditional niobium-based materials cannot be achieved simultaneously.
[0005] In order to achieve the above purpose, the present invention provides a high-entropy doped niobium pentoxide nanoparticle, and the chemical formula of the high-entropy doped niobium pentoxide nanoparticle is Nb 1-x Fe a Co e Ni i Cr j Al k O2, where x=a+e+i+j+k, 0.04≤x≤0.06, 0<a<1, 0<e<1, 0<i<1, 0<j<1, 0<k<1; it has an orthorhombic crystal system with a space group of P2 / m, the doped metals occupy Nb sites in an atomically dispersed manner, the cell parameter c-axis is extended to 0.41 nm; and the size of the nanoparticle is 50-200 nm. Further, the discharge capacity of the nanoparticle at a 100 C rate is not less than 156 mAh g -1 , and the lithium ion diffusion coefficient is 10 -8 -10 -10 cm 2 / s.
[0006] Further, the value of x is 0.05; The present invention also provides a preparation method of the above high-entropy doped niobium pentoxide nanoparticle, which comprises the following steps: (1) Dissolving a niobium source, an iron source, a cobalt source, a nickel source, a chromium source and an aluminum source in N,N-dimethylformamide or ethanol to form a metal mixed solution A; (2) Dissolving an organic ligand in N,N-dimethylformamide or ethanol to form a ligand solution B; (3) Mixing the solution A and the solution B uniformly to prepare a precursor solution; (4) Placing the precursor solution in a hydrothermal reaction kettle, reacting at 160-220°C for 6-24 hours, and after the reaction is completed, performing centrifugation, washing and drying to obtain a precursor; (5) Sintering the precursor under a protective atmosphere to obtain the high-entropy doped niobium pentoxide nanoparticle.
[0007] Furthermore, the niobium source is niobium pentachloride; the iron source is ferric chloride or ferric nitrate; the cobalt source is cobalt chloride or cobalt nitrate; the nickel source is nickel chloride or nickel nitrate; the chromium source is chromium chloride or chromium nitrate; and the aluminum source is aluminum chloride or aluminum nitrate.
[0008] Furthermore, the organic ligand is terephthalic acid; and the molar ratio of the organic ligand to the niobium source is (2-5):1.
[0009] Further, in step (1), the molar volume ratio of the niobium source to N,N-dimethylformamide or ethanol is 1 mmol : (15-23) mL; in step (2), the molar volume ratio of the organic ligand to N,N-dimethylformamide or ethanol is 1 mmol : (1-1.6) mL.
[0010] Furthermore, in step (5), the sintering is carried out by heating to 700-800°C at a heating rate of 2-5°C / min, holding at that temperature for 3-6 hours, and then cooling to room temperature.
[0011] The present invention also provides a lithium-ion battery anode material comprising the above-mentioned high-entropy doped niobium pentoxide nanoparticles.
[0012] The present invention also provides a lithium-ion battery, wherein the negative electrode adopts the above-mentioned lithium-ion battery negative electrode material; the battery retains a capacity of not less than 88% after 1000 cycles at a 10 C rate, and the volume change rate is less than 1.5%.
[0013] The beneficial effects of this invention are: 1) The innovative preparation process of this invention achieves atomic-level precise doping: through pentavalent niobium ions (Nb... 5+ ) and ferric ions (Fe 3+ ), trivalent aluminum ions (Al 3+ ), divalent cobalt ions (Co) 2+ ), divalent nickel ions (Ni 2+ ), trivalent chromium ions (Cr 3 + Under the synergistic coordination regulated by terephthalic acid ligands, a precursor solution with uniform metal ion distribution was formed. HE-Nb₂O₅ nanoparticles (50-200 nm) obtained after heat treatment exhibit the following characteristics: 1) Multiple dopant ions occupy Nb lattice sites at the atomic level, forming a stable solid solution structure (no impurity phase peaks in XRD); 2) The high entropy effect causes Li₂O₅ to undergo a process where... + The diffusion channels are expanded (the interplanar spacing increases by 5%); 3) Through the synergistic effect of multi-metal electrons, the electronic conductivity is improved, achieving a high specific capacity of 280 mAh / g and a capacity retention of 88% at 10 C rate.
[0014] 2) This invention innovatively develops orthorhombic high-entropy doped Nb₂O₅ materials, achieving performance breakthroughs through the synergistic effect of multiple metal ions. Regarding electronic structure modulation, the co-doping of five transition metals (Fe, Co, Ni, Cr, and Al) significantly alters the local electronic environment of Nb, simultaneously activating Nb. 5+ / Nb 4+ / Nb 3+ Multi-electron redox reactions increased the theoretical capacity by more than 40% (from 202 mAh / g to 280 mAh / g); in terms of ion transport kinetics, high-entropy-induced lattice distortion reduced the lithium-ion migration barrier from 0.78 eV to 0.52 eV. + Compared to undoped samples, the diffusion coefficient is significantly higher; the unique solid solution structure retains 92.3% capacity retention and has a volume change rate of <1.5% after 1000 cycles at a high rate of 10 C. These properties make it an ideal anode material for next-generation fast-charging lithium-ion batteries, particularly suitable for fast-charging systems for electric vehicles and high-power energy storage devices.
[0015] 3) The preparation process of this invention has significant industrialization advantages. It adopts a one-step hydrothermal method combined with a controllable sintering process, which has low energy consumption. No toxic solvents are involved in the whole process, which is in line with the twelve principles of green chemistry. The morphology of the product can be precisely controlled by adjusting the ligand / metal ratio and solvothermal temperature. The batch stability is better than that of the sol-gel method, which has the conditions for large-scale production. Attached Figure Description
[0016] Figure 1 These are a) XRD patterns and b) magnified XRD patterns of HE-Nb2O5 nanoparticles prepared in Example 1; Figure 2 These are atomic-level HAADF-STEM images (a) of HE-Nb2O5 nanoparticles prepared in Example 1, and atomic-level HAADF-STEM images (e) of undoped niobium pentoxide (Nb2O5) nanoparticles. Figure 3 These are atomic-level HAADF-STEM and EDS mapping images of HE-Nb2O5 and Nb2O5 nanoparticles prepared in Example 1. Figure 4 The following are the a) UV-Vis diffuse reflectance spectra of HE-Nb2O5 and Nb2O5 nanoparticles prepared in Example 1; and the b) photon energy and (αhv) of these nanoparticles. 2 Relationship curve; Figure 5 The CV curve of the material prepared in Example 1 as an electrode material in a lithium-ion half-cell is shown. Figure 6This is a rate performance diagram of the material prepared in Example 1 as an electrode material in a lithium-ion half-cell at different current densities. Figure 7 The material prepared in Example 1 is used as an electrode material in a long-cycle performance diagram of a lithium-ion half-cell at a current density of 10 C; Figure 8 The lithium-ion diffusion coefficient of the material prepared in Example 1 as an electrode material in a lithium-ion half-cell; Figure 9 The XPS spectra of the material prepared in Example 1 as an electrode material in a lithium-ion half-cell under different charge and discharge conditions are shown. Detailed Implementation
[0017] To make the technical solutions and advantages of the present invention clearer, the present invention and its beneficial effects will be described in further detail below with reference to specific embodiments and accompanying drawings. However, the embodiments of the present invention are not limited thereto. For ease of understanding, the present invention will be described more comprehensively and meticulously below with reference to the accompanying drawings and preferred embodiments. However, the scope of protection of the present invention is not limited to the following specific embodiments.
[0018] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0019] Unless otherwise specified, all reagents and raw materials used in this invention are commercially available products or products that can be prepared by known methods.
[0020] To better understand the present invention, the following embodiments further illustrate the content of the present invention, but the content of the present invention is not limited to the following embodiments.
[0021] In this invention, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0022] Example 1 A method for preparing HE-Nb2O5 nanoparticles includes the following steps: 1) Dissolve 1.9 mmol niobium pentachloride, 0.02 mmol aluminum nitrate nonahydrate, 0.02 mmol cobalt nitrate nonahydrate, 0.02 mmol chromium nitrate nonahydrate, 0.02 mmol ferric nitrate nonahydrate and 0.02 mmol nickel nitrate hexahydrate in 35 mL of ethanol and mix well to obtain mixed solution A; 2) Dissolve 5 mmol of terephthalic acid in 35 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 70 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 200℃ and react for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0023] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain HE-Nb2O5 nanoparticles.
[0024] Figure 1 The images show a) XRD patterns and b) magnified XRD patterns of HE-Nb2O5 and pure Nb2O5 nanoparticles prepared in this embodiment. The XRD patterns show that the phase of the high-entropy doped niobium pentoxide nanoparticles is Nb2O5, and the diffraction peaks correspond to the orthogonal Nb2O5 standard card, with no other impurity phases. The magnified XRD patterns show that the (001) diffraction peak of the high-entropy doped niobium pentoxide is shifted to a lower angle (Δ2θ=0.15°), indicating that high-entropy doping expands the interlayer spacing (d value increases by 0.2 Å).
[0025] Figure 2 These are a) TEM and b) atomic-level HAADF-STEM images of HE-Nb₂O₅ and pure Nb₂O₅ nanoparticles prepared in this embodiment. The TEM images show that both samples exhibit a nanoparticle morphology with a particle size of 50-100 nm. HAADF-STEM imaging reveals that HE-Nb₂O₅ and pure Nb₂O₅ exhibit clear (001) lattice fringes, with interplanar spacings of 4.1 Å and 3.9 Å, respectively. This indicates that high-entropy doping widens the interlayer spacing by 0.2 Å. Notably, the relatively dark-contrast atoms (yellow dashed lines) in the Nb layer indicate that multi-element doping occupies Nb sites.
[0026] Figure 3This is an atomic-level HAADF-STEM and EDS mapping image of the HE-Nb2O5 nanoparticles prepared in this embodiment. High-resolution STEM-EDS elemental surface scanning confirms that the five elements Fe, Co, Ni, Cr, and Al are atomically uniformly distributed in the high-entropy doped Nb2O5, with no elemental segregation.
[0027] Figure 4 The UV-Vis diffuse reflectance spectra and photon energies (αhv) of HE-Nb2O5 and pure Nb2O5 nanoparticles prepared in this embodiment are shown. 2 Relationship curves. Compared with undoped niobium pentoxide, high-entropy-doped niobium pentoxide exhibits stronger light absorption characteristics in the wavelength range of 400-1500 nm. Calculations show that the band gap of high-entropy-doped niobium pentoxide is only 2.75 eV, lower than that of undoped niobium pentoxide (3.15 eV), indicating that high-entropy doping effectively improves the intrinsic conductivity of the material.
[0028] The high-entropy doped niobium pentoxide nanoparticles (70 mg) prepared in Example 1 were used as the negative electrode active component. They were mixed with acetylene black conductive agent (20 mg) and polyvinylidene fluoride binder (10 mg) at a mass ratio of 7:2:1. 1 mL of N-methylpyrrolidone solvent was added, and the mixture was stirred thoroughly to form a homogeneous slurry. This slurry was then coated onto a copper foil current collector and dried at 70°C to obtain the working electrode. The electrode sheet was subsequently cut to a size of 0.78 cm. 2 The circular electrodes were assembled into a CR2032 type button half-cell for electrochemical performance testing in a glove box environment with strictly controlled moisture and oxygen content, using a lithium metal sheet as the counter electrode, Celgard 2400 as the separator, and 1M LiPF6 / EC:DMC (1:1 v / v) as the electrolyte.
[0029] Figure 5 The CV curves of the lithium-ion half-cell prepared in this application example are shown in the 1-3V range. Compared to the pure Nb₂O₅ system, the non-Faraday and faradaic current response in the lithium-ion half-cell prepared in this application example are increased by 2 times, indicating a significant improvement in its electrochemical reactivity. The significant peak pairs of 1.56 / 1.83V and 2.04 / 1.77V for Nb₂O₅ correspond to Nb 5+ / Nb 4+ The redox process. The 2.04 / 1.77V redox peaks of HE-Nb₂O₅ significantly weakened, and a new broad peak pair at 1.37 / 1.5V appeared, revealing the low valence state of niobium (Nb₂O₅). 4+ / Nb 3+ Reversible transformation.
[0030] Figure 6The rate performance of the lithium-ion half-cell prepared in this application example is shown at different currents. HE-Nb2O5 exhibits discharge capacities of 263.9, 261.5, 251, 240, 228, 205, 184, and 163 mAh g⁻¹ at different current densities of 0.5, 1, 2, 5, 10, 20, 50C, and 100C, respectively. -1 The average discharge capacities of the Nb2O5 anode under the same conditions were 195, 189, 179, 160, 146, 131, 89 and 42 mAh g, respectively. -1 When the current density recovered to 0.5C, the discharge capacity of HE-Nb2O5 rapidly recovered to 290 mAh g⁻¹. -1 This confirms that highly entropy-doped Nb₂O₅ exhibits excellent rate performance.
[0031] Figure 7 This application example demonstrates the long-term cycling stability of the lithium-ion half-cell at a current density of 10C. The first-cycle capacity of HE-Nb2O5 at 10C is 243 mAh g⁻¹. -1 It has a higher capacity than Nb2O5 (115 mAh g). -1 The capacity retention rate of HE-Nb2O5 after 1000 cycles was 88%.
[0032] Figure 8 The figure shows the lithium-ion diffusion coefficient of the lithium-ion half-cell fabricated in this application example, calculated based on GITT testing. Compared to Nb₂O₅, HE-Nb₂O₅ material exhibits a two-order-of-magnitude improvement in lithium-ion diffusion capability, with a DLi⁺ range of 7.4 × 10⁻⁶. - 8cm 2 s -1 and 3×10 - 10 cm 2 s -1 The faster ion migration rate in the HE-Nb2O5 electrode contributes to its excellent rate performance, which also explains its high capacity and high stability in high current testing.
[0033] Figure 9 This example shows the non-in-situ Nb 3pXPS spectra of the negative electrode of a lithium-ion half-cell under different charge and discharge states. The results demonstrate the Nb content during the discharge process. 5+ / Nb 4+ and Nb 4+ / Nb 3+ The process of redox pair transformation.
[0034] Example 2 A method for preparing HE-Nb2O5 nanoparticles includes the following steps: 1) Dissolve 0.950 mmol niobium pentachloride, 0.01 mmol aluminum nitrate nonahydrate, 0.01 mmol cobalt nitrate nonahydrate, 0.01 mmol chromium nitrate nonahydrate, 0.01 mmol ferric nitrate nonahydrate and 0.01 mmol nickel nitrate hexahydrate in 17 mL of ethanol and mix well to obtain mixed solution A; 2) Dissolve 2.5 mmol of terephthalic acid in 17 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 50 mL polytetrafluoroethylene-lined hydrothermal reactor and place it in a 200℃ oven for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0035] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain HE-Nb2O5 nanoparticles.
[0036] Example 3 A method for preparing HE-Nb2O5 nanoparticles includes the following steps: 1) Dissolve 0.950 mmol niobium pentachloride, 0.01 mmol aluminum nitrate nonahydrate, 0.01 mmol cobalt nitrate nonahydrate, 0.01 mmol chromium nitrate nonahydrate, 0.01 mmol ferric nitrate nonahydrate and 0.01 mmol nickel nitrate hexahydrate in 17 mL of ethanol and mix well to obtain mixed solution A; 2) Dissolve 2.5 mmol of terephthalic acid in 17 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 50 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 180℃ and react for 24 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0037] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain HE-Nb2O5 nanoparticles.
[0038] Example 4 A method for preparing HE-Nb2O5 nanoparticles includes the following steps: 1) Dissolve 0.950 mmol niobium pentachloride, 0.01 mmol aluminum nitrate nonahydrate, 0.01 mmol cobalt nitrate nonahydrate, 0.01 mmol chromium nitrate nonahydrate, 0.01 mmol ferric nitrate nonahydrate and 0.01 mmol nickel nitrate hexahydrate in 17 mL of ethanol and mix well to obtain mixed solution A; 2) Dissolve 2.5 mmol of terephthalic acid in 17 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 50 mL polytetrafluoroethylene-lined hydrothermal reactor and place it in a 200℃ oven for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0039] 5) The precursor was placed in a muffle furnace and heated to 700°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain HE-Nb2O5 nanoparticles.
[0040] Comparative Example 1 1) Dissolve 1.9 mmol niobium pentachloride, 0.02 mmol aluminum nitrate nonahydrate, 0.02 mmol cobalt nitrate nonahydrate, 0.02 mmol chromium nitrate nonahydrate and 0.02 mmol nickel nitrate hexahydrate in 35 mL of ethanol and mix well to obtain mixed solution A; 2) Dissolve 5 mmol of terephthalic acid in 35 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 70 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 200℃ and react for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0041] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain Co / Ni / Cr / Al-Nb2O5 nanoparticles.
[0042] Comparative Example 2 1) Dissolve 1.9 mmol niobium pentachloride, 0.02 mmol aluminum nitrate nonahydrate, 0.02 mmol chromium nitrate nonahydrate, 0.02 mmol ferric nitrate nonahydrate, and 0.02 mmol nickel nitrate hexahydrate in 35 mL of ethanol and mix thoroughly to obtain mixed solution A; 2) Dissolve 5 mmol of terephthalic acid in 35 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 70 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 200℃ and react for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0043] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain Al / Ni / Cr / Fe-Nb2O5 nanoparticles.
[0044] Comparative Example 3 1) Dissolve 1.9 mmol niobium pentachloride, 0.02 mmol cobalt nitrate nonahydrate, 0.02 mmol ferric nitrate nonahydrate, 0.02 mmol chromium nitrate nonahydrate, and 0.02 mmol nickel nitrate hexahydrate in 35 mL of ethanol and mix thoroughly to obtain mixed solution A; 2) Dissolve 5 mmol of terephthalic acid in 35 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 70 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 200℃ and react for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0045] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain Co / Ni / Cr / Fe-Nb2O5 nanoparticles.
[0046] Comparative Example 4 1) Dissolve 1.9 mmol niobium pentachloride, 0.02 mmol ferric nitrate nonahydrate, 0.02 mmol aluminum nitrate nonahydrate, 0.02 mmol cobalt nitrate nonahydrate and 0.02 mmol chromium nitrate nonahydrate in 35 mL of ethanol and mix well to obtain mixed solution A; 2) Dissolve 5 mmol of terephthalic acid in 35 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 70 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 200℃ and react for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0047] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain Co / Al / Cr / Fe-Nb2O5 nanoparticles.
[0048] Comparative Example 5 1) Dissolve 1.9 mmol niobium pentachloride, 0.02 mmol ferric nitrate nonahydrate, 0.02 mmol aluminum nitrate nonahydrate, 0.02 mmol cobalt nitrate nonahydrate, and 0.02 mmol nickel nitrate hexahydrate in 35 mL of ethanol and mix thoroughly to obtain mixed solution A; 2) Dissolve 5 mmol of terephthalic acid in 35 mL of ethanol to obtain mixed solution B; 3) Mix solution A and solution B thoroughly to obtain a colorless and transparent precursor solution; 4) Transfer the precursor solution to a 70 mL hydrothermal reactor lined with polytetrafluoroethylene, place it in an oven at 200℃ and react for 12 h. After the reaction is complete, allow it to cool naturally to room temperature, centrifuge to collect the precipitate, wash it three times with anhydrous ethanol, and vacuum dry it at 70℃ for 12 h to obtain the precursor powder.
[0049] 5) The precursor was placed in a muffle furnace and heated to 750°C at a heating rate of 5°C / min, held for 3 hours, and then cooled to room temperature to obtain Ni / Al / Co / Fe-Nb2O5 nanoparticles.
[0050] The lithium-ion half-cells prepared in Comparative Examples 1 / 2 / 3 / 4 / 5 were subjected to cycle performance tests. At a current density of 0.5C, the discharge capacities were 241, 222, 212, 216, and 229 mAh g, respectively. -1 All of them have higher specific capacities than undoped Nb2O5, but lower than HE-Nb2O5, confirming that the five elements have a synergistic effect, with high-entropy doped Nb2O5 exhibiting the highest specific capacity.
[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A high-entropy-doped niobium pentoxide nanoparticle, characterized in that, The chemical formula of the high-entropy doped niobium pentoxide nanoparticles is Nb 1-x Fe a Co e Ni i Cr j Al k O 2.5 , wherein x=a+e+i+j+k, 0.04≤x≤0.06, 0<a<1, 0<e<1, 0<i<1, 0<j<1, 0<k<1; the nanoparticles have an orthorhombic crystal system with a space group of P2 / m, the doping metals occupy Nb sites in an atomically dispersed state, the unit cell parameter along the c-axis is expanded to 0.41 nm; and the size of the nanoparticles ranges from 50 nm to 200 nm.
2. The high-entropy doped niobium pentoxide nanoparticles according to claim 1, characterized in that, The nanoparticles have a discharge capacity of no less than 156 mAh g at a 100 C rate. -1 And the lithium-ion diffusion coefficient is 10. -8 -10 -10 cm 2 / s.
3. The high-entropy doped niobium pentoxide nanoparticles according to claim 1, characterized in that, The value of x is 0.
05.
4. A method for preparing high-entropy doped niobium pentoxide nanoparticles according to any one of claims 1-3, characterized in that, Includes the following steps: (1) Dissolve niobium source, iron source, cobalt source, nickel source, chromium source and aluminum source in N,N-dimethylformamide or ethanol to form metal mixed solution A; (2) Dissolve the organic ligand in N,N-dimethylformamide or ethanol to form ligand solution B; (3) Mix solution A and solution B evenly to obtain the precursor solution; (4) Place the precursor liquid in a hydrothermal reactor and react at 160-220℃ for 6-24 hours. After the reaction is completed, centrifuge, wash and dry to obtain the precursor. (5) The precursor is sintered under a protective atmosphere to obtain the high-entropy doped niobium pentoxide nanoparticles.
5. The preparation method according to claim 4, characterized in that, The niobium source is niobium pentachloride; the iron source is ferric chloride or ferric nitrate; the cobalt source is cobalt chloride or cobalt nitrate; the nickel source is nickel chloride or nickel nitrate; the chromium source is chromium chloride or chromium nitrate; and the aluminum source is aluminum chloride or aluminum nitrate.
6. The preparation method according to claim 4, characterized in that, The organic ligand is terephthalic acid; and the molar ratio of the organic ligand to the niobium source is (2-5):
1.
7. The preparation method according to claim 4, characterized in that, In step (1), the molar volume ratio of the niobium source to N,N-dimethylformamide or ethanol is 1 mmol : (15-23) mL; in step (2), the molar volume ratio of the organic ligand to N,N-dimethylformamide or ethanol is 1 mmol : (1-1.6) mL.
8. The preparation method according to claim 4, characterized in that, In step (5), the sintering is carried out by heating to 700-800°C at a heating rate of 2-5°C / min, holding at that temperature for 3-6 hours, and then cooling to room temperature.
9. A lithium-ion battery anode material, characterized in that, It includes the high-entropy doped niobium pentoxide nanoparticles as described in any one of claims 1-3.
10. A lithium-ion battery, characterized in that, Its negative electrode adopts the lithium-ion battery negative electrode material as described in claim 9; the battery retains a capacity of not less than 88% after 1000 cycles at a 10 C rate, and the volume change rate is less than 1.5%.
Citation Information
Patent Citations
Niobate and niobate composite material and application of niobate composite material to secondary lithium battery
CN102760876A
Anion-cation high-entropy doped lithium-rich manganese-based positive electrode material and preparation thereof, and battery based on material
CN119170798A