Method for adding trace elements to water, strontium zinc dissolving material, selenium dissolving material and method of manufacture
By using electrolysis with strontium-zinc and selenium dissolving materials in water, the trace elements selenium, strontium, and zinc enter the water in ionic form, solving the problems of inorganicization and absorption difficulties of trace elements in water, and realizing a healthy drinking water solution with controllable content.
Patent Information
- Application Number
- CN202511529692.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-10-24
AI Technical Summary
When adding trace elements to water using existing technologies, the trace elements are easily rendered inorganic, making them difficult for the human body to absorb and their concentration uncontrollable.
Using strontium-zinc and selenium dissolving materials as the intermediate conductive layer, the trace elements selenium, strontium, and zinc are ionized and incorporated into the drinking water through electrolysis. The element content is adjusted by controlling the electrolysis parameters using conductive electrodes.
It achieves effective absorption and content control of trace elements, provides an effective way to drink healthy water, and has broad application prospects and economic benefits.
Smart Images

Figure CN121361882B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of trace element technology, specifically relating to a method for adding trace elements to water, strontium-zinc dissolving materials, selenium dissolving materials, and preparation methods. Background Technology
[0002] Trace elements refer to elements present in the human body at concentrations below 0.01%. Numerous academic studies have confirmed that selenium, strontium, and zinc are essential elements for human health. Medical research has demonstrated that these trace elements have significant auxiliary therapeutic effects in improving immunity and cardiovascular diseases, and also exhibit some inhibitory effects on tumors. For example, Zhao Jin, in "The Role of Strontium in Traditional Chinese Medicine," points out that strontium's biological functions are closely related to bone formation, cardiovascular function and structure, and neuromuscular excitability. Furthermore, strontium has anti-aging, anti-cancer, and immune-enhancing effects. Zhang Yong, in "A Brief Discussion on the Role of Selenium in the Human Body," points out that selenium plays a role in preventing various cancers and also has regulatory effects on hypertension and diabetes. Zinc is one of the most widely metabolized elements in the human body and is an important component of more than 200 enzymes, DNA, and RNA. Zinc deficiency can reduce enzyme activity, thereby affecting the normal function of many systems in the body. Therefore, adequate intake of selenium, strontium, and zinc is crucial for maintaining health.
[0003] Besides ingesting foods containing trace elements, trace elements can also enter the human body through drinking water. Currently, the method of adding trace elements to water involves crushing minerals containing trace elements, placing them in a filter bag, and then adding the filter bag to the water. However, during the process of entering the water, the trace elements are prone to inorganic transformation, making them difficult for the human body to absorb. Furthermore, this method of addition makes the trace element content in the water uncontrollable. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a method for adding trace elements to water, a strontium-zinc dissolving material, a selenium dissolving material, and a preparation method. This invention prepares a selenium / strontium / zinc trace element dissolving functional material, primarily composed of selenium, strontium, and zinc. Using a conductive electrocatalytic electrode, electrolysis allows the selenium, strontium, and zinc trace elements in the material to be ionized and incorporated into drinking water. This invention overcomes the drawbacks of the inorganic formation of selenium, strontium, and zinc during their introduction into water, resulting in poor absorption by the human body and uncontrollable concentrations.
[0005] The present invention is specifically implemented through the following technical solutions.
[0006] The first objective of this invention is to provide a method for adding trace elements to water, comprising the following steps: In preparing strontium-zinc or selenium-soluble materials, the strontium-zinc and / or selenium-soluble materials are placed between conductive electrodes as an intermediate conductive layer. Electrolysis is performed at the anodic electrode using the conductive electrodes in water, allowing the selenium, strontium, and zinc elements in the dissolved materials to enter the water in ionic form through electrolysis.
[0007] The preparation method of the strontium-zinc dissolving material includes the following steps: Dolomite and strontium ore are pretreated, and then a mixture is prepared using the pretreated dolomite powder, strontium ore powder, foaming agent, rosin alcohol and volatile paraffin as raw materials. The mixture is pressed into the required shape to obtain a strontium-zinc mixture. After drying the strontium-zinc mixture, it is subjected to strengthening treatment and then cooled to obtain a strontium-zinc dissolving material. The preparation method of the selenium dissolving material includes the following steps: Selenium stone is pretreated, and a mixture is prepared using selenium stone powder, activated carbon powder, foaming agent, rosin alcohol and volatile paraffin as raw materials. The mixture is then pressed into the required shape to obtain a selenium mixture. The selenium mixture is then subjected to strengthening treatment to obtain a selenium dissolving material.
[0008] This invention prepares a selenium / strontium / zinc trace element dissolving functional material, mainly composed of selenium, strontium, and zinc as basic components. With the help of a conductive electrocatalytic electrode, the selenium, strontium, and zinc trace elements in the functional material are ionized and incorporated into drinking water through electrolysis. This invention solves the drawbacks of the trace elements selenium, strontium, and zinc becoming inorganic during the process of entering water, making them difficult for the human body to absorb, and the content being uncontrollable.
[0009] In a preferred embodiment of the present invention, the mass percentage of dolomite powder is 20% to 50% and the remainder is strontium ore powder, totaling 100% in the total amount of dolomite powder and strontium ore powder. In the strontium-zinc mixture, the amount of foaming agent added is 0.5 times the total volume of dolomite powder and strontium ore powder, the amount of rosin alcohol added is 0.1 to 0.3 times the total volume of dolomite powder and strontium ore powder, and the amount of paraffin wax added is 0.2 to 0.5 times the total volume of dolomite powder and strontium ore powder.
[0010] In a preferred embodiment of the present invention, the pretreatment steps for dolomite and strontium ore are as follows: the dolomite and strontium ore are placed in an oxalic acid solution with a mass concentration of 2% to 6% and boiled at a water temperature of 80 to 100 for 2 hours, washed clean with water, soaked in pure water for more than 10 hours, dehydrated and dried; and then pulverized to 150 mesh.
[0011] In a preferred embodiment of the present invention, the strengthening treatment in preparing the strontium-zinc dissolving material refers to drying the strontium-zinc mixture and then subjecting it to thermal oxidation treatment. After cooling, the strontium-zinc dissolving material is obtained. The thermal oxidation treatment temperature is 650℃~970℃, and the holding time is 6 hours. High-temperature calcination causes partial melting and sintering of the raw materials at high temperatures, resulting in particle reorganization and ultimately achieving a transformation of the powder from soft to hard, thus improving mechanical strength. Alternatively, the strengthening treatment involves coating the surface of the strontium-zinc mixture with food-grade high-temperature resistant ceramic adhesive, allowing it to stand, and then drying and curing it. Preferably, it is allowed to stand for more than 24 hours, followed by treatment in an oven at 70℃~100℃ for 8 hours. The high-temperature resistant ceramic adhesive is used to improve the mechanical strength of the molded trace element dissolving material.
[0012] In a preferred embodiment of the present invention, when preparing the selenium dissolving material, the mass ratio of selenite powder to activated carbon powder is 1:1, the amount of foaming agent added is 0.5 times the total volume of selenite powder and activated carbon powder, the amount of rosin alcohol added is 0.1 to 0.3 times the total volume of selenite powder and activated carbon powder, and the amount of paraffin wax added is 0.2 to 0.5 times the total volume of selenite powder and activated carbon powder.
[0013] In a preferred embodiment of the present invention, the strengthening treatment in preparing the selenium dissolving material refers to drying the selenium mixture and then subjecting it to thermal oxidation treatment. After cooling, the selenium dissolving material is obtained. The thermal oxidation treatment temperature is 230℃~270℃, and the holding time is 2 hours. High-temperature calcination causes partial melting and sintering of the raw materials at high temperatures, resulting in particle reorganization and ultimately achieving a transformation of the powder from soft to hard, thus improving mechanical strength. Alternatively, the strengthening treatment involves coating the surface of the selenium mixture with food-grade high-temperature resistant ceramic adhesive, allowing it to stand, and then drying and curing it. Preferably, it is allowed to stand for more than 24 hours, followed by treatment in an oven at 70℃~100℃ for 8 hours. The high-temperature resistant ceramic adhesive is used to improve the mechanical strength of the molded trace element dissolving material.
[0014] In a preferred embodiment of the present invention, the pretreatment steps for selenium stone are as follows: the selenium stone is soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried; and pulverized to 50 mesh. The selenium stone powder is soaked in a 0.2~0.8% NaOH aqueous solution for 4 hours, then soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried.
[0015] In a preferred embodiment of the present invention, the strontium-zinc dissolving material, the selenium dissolving material, and the conductive electrocatalyst electrode are respectively circular, plate-shaped, or tubular. The surface of the conductive electrode is coated with an oxide coating containing Se, Sr, and Zn elements. Direct current is used, and the voltage and current are adjusted as needed; preferably, the voltage is 9V~14V and the current is 0.5A~2A.
[0016] The second objective of this invention is to provide a method for preparing a strontium-zinc dissolving material, comprising the following steps: pretreating dolomite and strontium ore, then using the pretreated dolomite powder, strontium ore powder, foaming agent, rosin alcohol, and paraffin wax as raw materials to prepare a mixture, pressing the mixture into the desired shape to obtain a strontium-zinc mixture, drying the strontium-zinc mixture and then subjecting it to thermal oxidation treatment, and after cooling, obtaining the strontium-zinc dissolving material.
[0017] The third objective of this invention is to provide a method for preparing a selenium-dissolving material, comprising the following steps: Selenium stone is pretreated, and a mixture is prepared using selenium stone powder, activated carbon powder, foaming agent, rosin alcohol and paraffin as raw materials. The mixture is pressed into the required shape to obtain a selenium mixture. After drying the selenium mixture, it is subjected to thermal oxidation treatment. After cooling, a selenium soluble material is obtained.
[0018] The fourth objective of this invention is to provide a strontium-zinc dissolving material prepared by the above-described method.
[0019] The fifth objective of this invention is to provide a selenium dissolving material prepared by the above-described method.
[0020] The trace element dissolving material contains 0.1-0.13% Se, 30%-60% Sr (calculated as SrSO4), 0.9-1.4% Zn, and an iodine value of 1000-1300 mg / L for C. The dissolving material also contains calcium, magnesium, iron, silicon, etc.
[0021] Compared with the prior art, the present invention has the following beneficial effects: Compared to traditional methods that directly add minerals containing trace elements to water, this invention uses mineral raw materials containing selenium, strontium, and zinc, combined with foaming agents, rosin alcohol, and volatile paraffin wax, and after strengthening treatment, prepares a selenium / strontium / zinc trace element dissolving functional material. This material serves as an intermediate conductive layer, placed between conductive electrodes. In conjunction with the conductive electrodes, electrolysis in water allows the selenium, strontium, and zinc trace elements in the dissolving functional material to be ionized and incorporated into the drinking water. This solves the drawbacks of the trace elements selenium, strontium, and zinc becoming inorganic during their entry into water, making them difficult for the human body to absorb, and resulting in uncontrollable concentrations.
[0022] The trace element dissolving material is placed between conductive electrocatalytic electrodes. Strontium, zinc trace element dissolving materials and selenium stone dissolving materials are formulated according to water quality requirements. Electrolysis is performed using conductive electrocatalytic electrodes. By controlling the electrolysis parameters, the trace elements selenium, strontium, and zinc in the water can be adjusted as needed.
[0023] This invention dissolves trace elements in water in an ionic state, which is beneficial for human absorption. Furthermore, the content of trace elements entering the water can be controlled as needed, providing an effective way for the human body to ingest trace elements. This invention will be widely used in the field of health and will bring huge economic benefits. In addition, the method is simple and easy to implement. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the device for adding selenium / strontium / zinc trace elements to water provided by the present invention. Detailed Implementation
[0025] To enable those skilled in the art to better understand and implement the technical solutions of the present invention, the present invention will be further described below with reference to specific embodiments and accompanying drawings. However, the embodiments described are not intended to limit the present invention. Unless otherwise specified, the experimental methods and detection methods described in the following embodiments are conventional methods; unless otherwise specified, the reagents and materials described are commercially available.
[0026] This invention prepares strontium-zinc dissolving materials and / or selenium dissolving materials as functional materials. The main components are selenium, strontium, and zinc. Using conductive electrocatalytic electrodes, the trace elements selenium, strontium, and zinc in the functional materials are dissolved through electrolysis and ionized into drinking water. This invention solves the problems of trace elements selenium, strontium, and zinc becoming inorganic during water infusion, making them difficult for the human body to absorb, and resulting in uncontrollable concentrations. The specific technical solution is as follows:
[0027] This invention provides a method for adding trace elements to water, comprising the following steps: Strontium-zinc or selenium-soluble materials are prepared by placing the strontium-zinc and / or selenium-soluble materials as an intermediate conductive layer between conductive electrocatalytic electrodes. In water, electrolysis allows the selenium, strontium, and zinc elements in the dissolved materials to enter the water in ionic form. It should be noted that the ratio of strontium, zinc, and selenium-soluble materials is adjusted according to water quality requirements, and electrolysis is performed using conductive electrocatalytic electrodes. By controlling the electrolysis parameters, the levels of selenium, strontium, and zinc in the water can be adjusted as needed.
[0028] When strontium and zinc need to be added, strontium-zinc dissolving materials are used; when selenium needs to be added, selenium dissolving materials are used; when both strontium, zinc, and selenium need to be added simultaneously, both strontium-zinc dissolving materials and selenium dissolving materials are used. To further improve the conductivity of the selenium dissolving material, it can be coated with carbon fiber cloth.
[0029] The preparation method of the strontium-zinc dissolving material includes the following steps: Dolomite and strontium ore are pretreated, and then a mixture is prepared using the pretreated dolomite powder, strontium ore powder, foaming agent, rosin alcohol and paraffin as raw materials. The mixture is pressed into the required shape to obtain a strontium-zinc mixture. The strontium-zinc mixture is then subjected to strengthening treatment to obtain a strontium-zinc dissolving material.
[0030] In a preferred embodiment of the present invention, the mass percentage of dolomite powder is 20% to 50% and the remainder is strontium ore powder, totaling 100% in the total amount of dolomite powder and strontium ore powder. In the strontium-zinc mixture, the amount of foaming agent added is 0.5 times the total volume of dolomite powder and strontium ore powder, the amount of rosin alcohol added is 0.1 to 0.3 times the total volume of dolomite powder and strontium ore powder, and the amount of paraffin wax added is 0.2 to 0.5 times the total volume of dolomite powder and strontium ore powder.
[0031] In a preferred embodiment of the present invention, the pretreatment steps for dolomite and strontium ore are as follows: the dolomite and strontium ore are placed in a 2%~6% oxalic acid solution and boiled at a water temperature of 80~100 for 2 hours, washed clean with water, soaked in pure water for more than 10 hours, dehydrated and dried; and then pulverized to 150 mesh.
[0032] In a preferred embodiment of the present invention, when preparing the strontium-zinc dissolving material, the strengthening treatment refers to drying the strontium-zinc mixture and then subjecting it to thermal oxidation treatment. After cooling, the strontium-zinc dissolving material is obtained. The temperature of the thermal oxidation treatment is 650℃~970℃, and the holding time is 6 hours. Alternatively, the strengthening treatment refers to coating the surface of the strontium-zinc mixture with food-grade high-temperature resistant ceramic adhesive, allowing it to stand, and then drying and curing it.
[0033] The preparation method of the selenium dissolving material includes the following steps: Selenium stone is pretreated, and a mixture is prepared using selenium stone powder, activated carbon powder, foaming agent, rosin alcohol and paraffin as raw materials. The mixture is pressed into the required shape to obtain a selenium mixture. After strengthening treatment of the selenium mixture, a selenium dissolving material is obtained.
[0034] In a preferred embodiment of the present invention, when preparing the selenium dissolving material, the mass ratio of selenite powder to activated carbon powder is 1:1, the amount of foaming agent added is 0.5 times the total volume of selenite powder and activated carbon powder, the amount of rosin alcohol added is 0.1 to 0.3 times the total volume of selenite powder and activated carbon powder, and the amount of paraffin wax added is 0.2 to 0.5 times the total volume of selenite powder and activated carbon powder.
[0035] In a preferred embodiment of the present invention, when preparing the selenium dissolving material, the strengthening treatment refers to drying the selenium mixture and then subjecting it to thermal oxidation treatment, followed by cooling to obtain the selenium dissolving material. The temperature of the thermal oxidation treatment is 230℃~270℃, and the holding time is 2 hours. Alternatively, the strengthening treatment refers to coating the surface of the selenium mixture with food-grade high-temperature resistant ceramic adhesive, allowing it to stand, and then drying and curing it.
[0036] In a preferred embodiment of the present invention, the pretreatment steps for selenium stone are as follows: the selenium stone is soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried; and pulverized to 50 mesh. The selenium stone powder is soaked in a 0.2%~0.8% NaOH aqueous solution for 4 hours, then soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried.
[0037] In a preferred embodiment of the present invention, the strontium-zinc dissolving material, the selenium dissolving material, and the conductive electrocatalytic electrode are respectively circular, plate-shaped, or tubular.
[0038] The invention will be specifically described below through the following embodiments.
[0039] Preparation Example 1 The preparation method of strontium-zinc dissolving material includes the following steps: (1) Place the matrix dolomite and strontium ore in a 2% oxalic acid solution and boil for 2 hours at 80°C. After washing with water, soak in pure water for more than 10 hours, dehydrate and dry; then crush to 150 mesh.
[0040] (2) Mix the matrix dolomite (20%) and strontium ore (80%) powders in a vibratory mixer for 8 hours. Take them out and put them into a mixer. Add 0.5 times the powder volume of polyurethane foaming agent (purchased from Yangzi Insulation Building Materials Co., Ltd., Hejian City, Hebei Province), 0.1 times the volume of rosin alcohol, and 0.2 times the volume of paraffin wax and stir for 4 hours. Prepare a strontium-zinc mixture. Press it into the required shape on a press according to the needs. Dry it in a drying oven at 80°C for 90 minutes. Then put it into a sintering furnace and heat-oxidize it at 650°C for 6 hours. Through high-temperature calcination, the raw materials (such as shale, clay, silica, alumina) partially melt and sinter at high temperature, and the particles are reorganized. Finally, the powder particles are transformed from soft to hard, which improves the mechanical strength. Then cool it to room temperature to form a semi-ceramic product.
[0041] Preparation Example 2 The preparation method of strontium-zinc dissolving material includes the following steps: (1) Place the matrix dolomite and strontium ore in a 6% oxalic acid solution and boil for 2 hours at 100°C. After washing with water, soak in pure water for more than 10 hours, dehydrate and dry; then pulverize to 150 mesh.
[0042] (2) Mix the powders of dolomite (50%) and strontium ore (50%) in a vibratory mixer for 8 hours. Remove the mixture and place it in a mixer. Add 0.5 times the volume of polyurethane foaming agent, 0.3 times the volume of rosin alcohol, and 0.5 times the volume of paraffin wax. Stir for 4 hours to prepare a strontium-zinc mixture. Press the mixture into the required shape on a press according to the requirements. Dry it in a drying oven at 80°C for 90 minutes. Then place it in a sintering furnace and heat-oxidize it at 970°C for 6 hours. Then cool it to room temperature to form a semi-ceramic product.
[0043] Preparation Example 3 The preparation method of strontium-zinc dissolving material includes the following steps: (1) Place the matrix dolomite and strontium ore in a 4% oxalic acid solution and boil at 90°C for 2 hours. After washing with water, soak in pure water for more than 10 hours, dehydrate and dry; then crush to 150 mesh.
[0044] (2) Mix the matrix dolomite (40%) and strontium ore (60%) powders in a vibratory mixer for 8 hours. Remove the mixture and place it in a mixer. Add 0.5 times the volume of polyurethane foaming agent, 0.2 times the volume of rosin alcohol, and 0.4 times the volume of paraffin wax and stir for 4 hours. Prepare a strontium-zinc mixture and press it into the required shape on a press according to the requirements. Dry it in a drying oven at 45°C for 90 minutes, cool it to room temperature, and then quickly brush it onto the surface of the molded product blank with a brush dipped in food-grade high-temperature resistant ceramic adhesive. The high-temperature resistant ceramic adhesive is used to improve the mechanical strength of the molded trace element dissolved material. The high-temperature resistant ceramic adhesive used in this embodiment is Feitegu brand. This ceramic adhesive has a service temperature of 60°C to 200°C and is placed for more than 24 hours. Then put it in an oven and treat it at 90°C for 8 hours, and then cool it to room temperature.
[0045] Preparation Example 4 The preparation method of strontium-zinc dissolving material includes the following steps: (1) Place the matrix dolomite and strontium ore in a 3% oxalic acid solution and boil at 85°C for 2 hours. After washing with water, soak in pure water for more than 10 hours, dehydrate and dry; then pulverize to 150 mesh.
[0046] (2) Mix the matrix dolomite (30%) and strontium ore (70%) powders in a vibratory mixer for 8 hours. Remove the mixture and place it in a mixer. Add 0.5 times the powder volume of polyurethane foaming agent, 0.1 times the volume of rosin alcohol, and 0.5 times the volume of paraffin wax. Stir for 4 hours to prepare a strontium-zinc mixture. Press the mixture into the required shape on a press according to the requirements. Dry the mixture in a drying oven at 45°C for 90 minutes. Cool it to room temperature. Then, use a brush to quickly apply food-grade high-temperature resistant ceramic adhesive to the surface of the molded product blank. The high-temperature resistant ceramic adhesive used in this embodiment is Feitegu brand. This ceramic adhesive has a service temperature of 60°C to 200°C and can be left for more than 24 hours. Then, place it in an oven at 70°C for 8 hours and then cool it to room temperature.
[0047] Preparation Example 5 A method for preparing selenium-dissolving materials includes the following steps: (1) The selenium stone was soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried; and pulverized to 50 mesh. The selenium stone powder was soaked in a 0.2% NaOH aqueous solution for 4 hours, then soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried.
[0048] (2) Place selenium stone powder and activated charcoal powder into a mixer at a mass ratio of 1:1, add foaming agent (0.5 times the powder volume), rosin alcohol (0.1 times the volume), and paraffin wax (0.2 times the volume), and stir for 1 hour. Press into the desired shape on a press. Dry in a drying oven at 230°C for 2 hours. Allow to cool naturally to room temperature.
[0049] Preparation Example 6 A method for preparing selenium-dissolving materials includes the following steps: (1) The selenium stone was soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried; and pulverized to 50 mesh. The selenium stone powder was soaked in 0.8% NaOH aqueous solution for 4 hours, then soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried.
[0050] (2) Place selenium stone powder and activated charcoal powder into a mixer at a mass ratio of 1:1, add 0.5 times the volume of polyurethane foaming agent, 0.3 times the volume of rosin alcohol, and 0.5 times the volume of paraffin wax, and stir for 1 hour. Press into the desired shape on a press. Dry in a drying oven at 270°C for 2 hours. Allow to cool naturally to room temperature.
[0051] Preparation Example 7 A method for preparing selenium-dissolving materials includes the following steps: (1) The selenium stone was soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried; and pulverized to 50 mesh. The selenium stone powder was soaked in 0.5% NaOH aqueous solution for 4 hours, then soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried.
[0052] (2) Place selenium stone powder and activated charcoal powder into a mixer at a mass ratio of 1:1, add 0.5 times the volume of polyurethane foaming agent, 0.2 times the volume of rosin alcohol, and 0.4 times the volume of paraffin wax, and stir for 1 hour. Press into the desired shape on a press. Dry in a drying oven at 45°C for 90 minutes, cool to room temperature, and then quickly brush food-grade high-temperature resistant ceramic adhesive onto the surface of the formed product blank with a brush. The high-temperature resistant ceramic adhesive used in this embodiment is Feitegu brand, which has a service temperature of 60°C to 200°C and can be left for more than 24 hours. Then put it in an oven and treat it at 70°C for 8 hours, and then cool it to room temperature.
[0053] Preparation Example 8 A method for preparing selenium-dissolving materials includes the following steps: (1) The selenium stone was soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried; and pulverized to 50 mesh. The selenium stone powder was soaked in 0.6% NaOH aqueous solution for 4 hours, then soaked in pure water and ultrasonically cleaned twice, then dehydrated and dried.
[0054] (2) Place selenium stone powder and activated charcoal powder into a mixer at a mass ratio of 1:1, add 0.5 times the volume of polyurethane foaming agent, 0.1 times the volume of rosin alcohol, and 0.5 times the volume of paraffin wax, and stir for 1 hour. Press into the desired shape on a press. Dry in a drying oven at 45°C for 90 minutes, cool to room temperature, and then quickly brush food-grade high-temperature resistant ceramic adhesive onto the surface of the formed product blank with a brush. The high-temperature resistant ceramic adhesive used in this embodiment is Feitegu brand, which has a service temperature of 60°C to 200°C and can be left for more than 24 hours. Then put it in an oven and treat it at 100°C for 8 hours, and then cool it to room temperature.
[0055] Example 1 like Figure 1As shown, the first tubular platinum oxide coated electrode 2 (diameter 80mm, length 180mm, wall thickness 1mm) and the second tubular platinum oxide coated electrode 3 (diameter 25mm, length 180mm, wall thickness 1mm), purchased from Beijing Xiangcheng Yida Electromechanical Technology Co., Ltd., are respectively led out with conductive posts. The tubular selenium dissolving material 4 (diameter 75mm, length 180mm, wall thickness 10mm) prepared in Example 5 and the tubular strontium zinc dissolving material 5 (diameter 50mm, length 180mm, wall thickness 10mm) prepared in Example 1 are placed between the two platinum oxide coated electrodes. The entire structure is placed in a 10-inch water dispenser empty filter membrane shell 1, and a DC power supply 6 is connected to the leads of the two platinum oxide coated electrodes. On the power supply 6, 7 represents voltage and 8 represents current. The DC voltage is adjusted to 9V and the current to 793mA. The water was found to contain 35 ug / L of selenium ions, 420 ug / L of strontium ions, and 630 ug / L of zinc ions, which meets the requirements of the national standard GB8537-2018 "National Food Safety Standard for Drinking Natural Mineral Water".
[0056] Example 2 The electrodes in Application Example 1 were replaced with tubular electrodes (80mm diameter, 180mm length, 1mm wall thickness) of ruthenium-iridium metal oxide coated electrodes purchased from Beijing Xiangcheng Yida Electromechanical Technology Co., Ltd. Conductive posts were led out from each electrode. Selenium-soluble trace element dissolving material (75mm diameter, 180mm length, 10mm wall thickness), strontium-soluble trace element dissolving material (50mm diameter, 180mm length, 10mm wall thickness) were placed between the platinum metal oxide coated electrodes and placed in a 10-inch water dispenser empty filter membrane housing. DC power was connected to the leads of the two platinum metal oxide coated electrodes. The DC voltage was adjusted to 14V and the current to 1.7A. The measured selenium ion content in the water was 12ug / L, the strontium ion content was 300ug / L, and the zinc ion content was 840ug / L, which meets the requirements of the national standard GB8537-2018 "National Food Safety Standard for Drinking Natural Mineral Water".
[0057] As can be seen from the above embodiments, trace elements can enter water in an ionic state through the above electrolysis process, and the content of trace elements entering the water can be controlled by changing the electrolysis parameters to meet the requirements.
[0058] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, it is intended to include any modifications and variations that fall within the scope of the claims and their equivalents.
Claims
1. A method for adding trace elements to water, characterized in that, Includes the following steps: Prepare strontium-zinc dissolving materials and / or selenium dissolving materials, place the strontium-zinc dissolving materials and / or selenium dissolving materials as intermediate conductive layers between conductive electrodes, and in water, electrolyze the elements in the dissolving materials into the water in ionic form; The preparation method of the strontium-zinc dissolving material includes the following steps: Dolomite and strontium ore are pretreated. A mixture is prepared using the pretreated dolomite powder, strontium ore powder, foaming agent, rosin alcohol and volatile paraffin as raw materials. The mixture is pressed into the required shape to obtain a strontium-zinc mixture. The strontium-zinc mixture is then subjected to strengthening treatment to obtain a strontium-zinc dissolving material. The preparation method of the selenium dissolving material includes the following steps: Selenium stone is pretreated, and a mixture is prepared using pretreated selenium stone powder, activated carbon powder, foaming agent, rosin alcohol and volatile paraffin as raw materials. The mixture is pressed into the required shape to obtain a selenium mixture. The selenium mixture is then subjected to strengthening treatment to obtain a selenium dissolving material. The strontium-zinc dissolving material, selenium dissolving material, and conductive electrode are shaped as circles, plates, or tubes, respectively. The conductive electrode surface is coated with an oxide coating containing Se, Sr, and Zn elements. Direct current is used, with a voltage of 9V~14V and a current of 0.5A~2A. When preparing strontium-zinc dissolving materials, the strengthening treatment refers to drying the strontium-zinc mixture and then subjecting it to thermal oxidation treatment at a temperature of 650℃~970℃ for 6 hours; or, the strengthening treatment refers to coating the surface of the strontium-zinc mixture with food-grade ceramic adhesive, allowing it to stand, and then drying and curing it. When preparing selenium-soluble materials, the strengthening treatment refers to drying the selenium mixture and then subjecting it to thermal oxidation treatment at a temperature of 230℃~270℃ for 2 hours; or, the strengthening treatment refers to coating the surface of the selenium mixture with food-grade ceramic adhesive, allowing it to stand, and then drying and curing it.
2. The method according to claim 1, characterized in that, In the total amount of dolomite powder and strontium ore powder, the mass percentage of dolomite powder is 20%~50%, and the balance is strontium ore powder, totaling 100%. In the strontium-zinc mixture, the amount of foaming agent added is 0.5 times the total volume of dolomite powder and strontium ore powder, the amount of rosin alcohol added is 0.1~0.3 times the total volume of dolomite powder and strontium ore powder, and the amount of paraffin wax added is 0.2~0.5 times the total volume of dolomite powder and strontium ore powder.
3. The method according to claim 1, characterized in that, When preparing selenium dissolving materials, the mass ratio of selenite powder to activated carbon powder is 1:1, the amount of foaming agent added is 0.5 times the total volume of selenite powder and activated carbon powder, the amount of rosin alcohol added is 0.1 to 0.3 times the total volume of selenite powder and activated carbon powder, and the amount of paraffin wax added is 0.2 to 0.5 times the total volume of selenite powder and activated carbon powder.
Citation Information
Patent Citations
Preparation method of human body trace metal element filter element
CN109319892A
Conductive mineral material and preparation method thereof and mineralized filter element with conductive mineral material
CN113754019A
Porous ore filter element material and preparation method thereof
CN114715997A
Weakly-alkaline strontium-enriched mineralized filter element with antibacterial property and preparation method of weakly-alkaline strontium-enriched mineralized filter element
CN120518139A
Mineral water former
JP2003145154A