A fully-dull antistatic polyester fiber and a method for preparing the same

By combining modified silicone resin fillers and antistatic agents, the problem of insufficient matte and antistatic properties of polyester fibers was solved, and polyester fibers with high mechanical strength, stable antistatic properties and soft matte finish were prepared.

CN121363054BActive Publication Date: 2026-11-24TAICANG YIFENG CHEMICAL FIBER CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511558650.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-10-29
Publication Date
2026-11-24
Estimated Expiration
2045-10-29

AI Technical Summary

Technical Problem

Existing polyester fibers are insufficient in terms of matting and antistatic properties, making it difficult to simultaneously meet the requirements of high-end textiles for softness, matte finish, and antistatic properties. They also suffer from decreased mechanical properties and poor dispersibility of functional components.

Method used

A combination of modified silicone resin filler and modified antistatic agent is used. Through modification with core-shell silica and organosilane coupling agent, an organic-inorganic hybrid silicone resin filler is formed, which forms a chemical bridging structure with polyester fiber, improving interfacial compatibility and stability. Furthermore, the antistatic performance is enhanced by the chemical bonding between the modified antistatic agent and the polyester fiber.

Benefits of technology

It achieves long-lasting and stable antistatic properties of polyester fibers, improves mechanical strength and matting properties, enhances the soft matte effect and hydrophilicity of fibers, and improves the overall stability and functional durability of fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses a fully matte and antistatic polyester fiber and its preparation method, belonging to the field of fiber preparation technology. It addresses the technical problem that the matte and antistatic properties of polyester fibers in existing technologies need further improvement. Specifically, it comprises the following components by weight: 60-80 parts polyethylene terephthalate, 4-6 parts silicone resin filler, 10-15 parts modified antistatic agent, and 1-3 parts auxiliary additives. This invention prepares polyester fibers by preparing a highly hydrophilic modified antistatic agent, which is then melt-spun together with an organic-inorganic hybrid silicone resin filler and a polyester matrix. This process not only improves the antistatic and matte properties of the polyester fiber but also enhances its hydrophilicity and mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fiber preparation technology, specifically to a fully matte antistatic polyester fiber and its preparation method. Background Technology

[0002] As textiles develop towards high-end and functional directions, polyester fiber (PET) is widely used due to its high mechanical strength, abrasion resistance, good washability, and low cost. However, ordinary polyester fiber has a high gloss and obvious surface mirror reflection, which does not meet the requirements of some consumer products or industrial applications that have high appearance requirements for soft, matte and full matte finishes. At the same time, polyester fiber itself has strong electrical insulation properties, which makes it easy to accumulate static electricity, affecting wearing comfort, attracting dust, and causing static discharge or even sparks, which is detrimental to clothing, safety, protection, underwear, bedding, etc.

[0003] To integrate aesthetic and functional requirements, researchers have been using various modification methods in recent years to improve matting and antistatic properties. Commonly used matting materials include adding matting agents and modifying the fiber structure, such as using rough or irregular cross-sections or applying a matting coating to the fiber surface to scatter light and reduce specular reflection. In terms of antistatic properties, commonly used materials or methods include incorporating conductive fibers, mixing in polar / charge carrier additives, and coating the surface with antistatic agents.

[0004] Although the aforementioned technical methods have achieved certain results in laboratory or some industrial applications, there are still many limitations and shortcomings in actual products: First, while matting agents such as silica nanoparticle fillers can reduce gloss and increase haze, excessive use can weaken the mechanical properties of fibers, such as reducing breaking strength and elongation, and may also affect spinning stability, increase melt viscosity, or damage processing equipment; Second, antistatic auxiliaries or conductive materials may be incompatible with the heat resistance, washability, and abrasion resistance of the polyester matrix, and are easily rinsed or thermally decomposed in high-temperature melting or washing environments. On the other hand, the poor dispersibility of polar auxiliaries or conductive fillers often leads to uneven distribution inside or on the surface of the fiber, resulting in serious local static electricity accumulation; Furthermore, in pursuing a fully matte appearance and antistatic properties, the fiber's hand feel, softness, gloss control precision, hydrophilicity / hygroscopicity, and other properties are often sacrificed.

[0005] The main reasons for these shortcomings are: compatibility issues between matting agents and antistatic agents in compounding, and poor thermal stability between polar / conductive additives and polyester melt or polyester segments. To address these issues, a solution is proposed. Summary of the Invention

[0006] The purpose of this invention is to provide a fully matte and antistatic polyester fiber and its preparation method, in order to solve the technical problem that the matte and antistatic properties of polyester fibers need to be further improved in the prior art.

[0007] The objective of this invention can be achieved through the following technical solution: a fully matte antistatic polyester fiber, comprising the following components by weight: 60-80 parts polyethylene terephthalate, 4-6 parts silicone resin filler, 10-15 parts modified antistatic agent and 1-3 parts auxiliary additives.

[0008] Furthermore, the modified silicone resin is prepared by the following steps: A1. Place the core-shell silica and n-butanol in a reaction vessel and stir at room temperature for 20-40 minutes to obtain a dispersion. A2. Place 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, phenyltrimethoxysilane, 2,4-dihydroxyacetophenone, deionized water and n-butanol in a reaction vessel and stir. Slowly add the dispersion. Heat the reaction vessel to 40-50℃ and keep it at this temperature for 15-30 minutes. Add concentrated sulfuric acid and heat the reaction vessel to 80-90℃. Keep it at this temperature for 4-6 hours. Post-treatment yields the silicone resin filler.

[0009] The reaction principle for preparing silicone resin fillers is as follows: During the reaction, core-shell silica is dispersed in n-butanol and a stable dispersion is formed by stirring. Further, when 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, phenyltrimethoxysilane, 2,4-dihydroxyacetophenone, deionized water, and n-butanol are mixed together and the silica-containing dispersion is slowly added, the system undergoes the first stage of pre-hydrolysis and condensation reaction at 40-50℃, mainly including the hydrolysis reaction of silanes and the condensation reaction between hydroxyl groups. After the addition of concentrated sulfuric acid, the pH of the system drops sharply, entering a strong acid catalytic condition, which accelerates the hydrolysis and condensation reaction rate, and finally, a silicone resin filler coated with core-shell silica is obtained.

[0010] Further, in step A1, the ratio of the core-shell silica to n-butanol is 2-4g:50-100mL; in step A2, the ratio of the 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, phenyltrimethoxysilane, 2,4-dihydroxyacetophenone, deionized water, n-butanol, dispersion, and concentrated sulfuric acid is 8-10g:7-9g:0.2-0.4g:60-80mL:1-2mL:20-40mL:1-2mL, and the concentration of the concentrated sulfuric acid is 50-70wt%. The post-treatment steps include: after the reaction is completed, the reaction solution is allowed to cool to room temperature, stand for 4-6 hours, filtered, the filter cake is washed 2-4 times with deionized water and ethanol, transferred to an oven at 50-60℃, dried to constant weight, ground, and passed through a 500-mesh sieve to obtain the silicone resin filler.

[0011] Furthermore, the core-shell silica is prepared by the following steps: B1. Cyclohexane, polyoxyethylene tert-octylphenyl ether, n-hexanol and deionized water were placed in a reaction vessel and stirred. Tetraethyl orthosilicate was added and reacted at room temperature for 1-2 hours. Ammonia solution was added and stirred at room temperature for 4-6 hours. Post-treatment was then performed to obtain the core-shell silica precursor. The reaction principle for preparing core-shell silica precursors is as follows: During the reaction, in a reverse microemulsion system constructed with cyclohexane as the oil phase, polyoxyethylene tert-octylphenyl ether as the nonionic surfactant, and n-hexanol as the co-surfactant, tiny water droplets are stably encapsulated in the organic phase, forming an oil-in-water microreactor. When tetraethyl orthosilicate is added, it gradually hydrolyzes within the water droplets and undergoes a condensation reaction catalyzed by ammonia, generating spherical silica nanoparticles, thus obtaining a core-shell silica precursor.

[0012] B2. Place the core-shell silica precursor and deionized water in a reaction vessel, heat the reaction vessel to 55-65℃, stir for 15-30 min, slowly add tin tetrachloride pentahydrate solution, add sodium hydroxide solution until the pH of the system is 9-10, keep the reaction at the temperature for 0.5-1 h, and then perform post-treatment to obtain core-shell silica.

[0013] The reaction principle for the preparation of core-shell silica is as follows: During the reaction, pretreated silica particles are redispersed in deionized water and heated to 55-65℃ for a certain period of time to ensure uniform particle dispersion and sufficient surface hydroxyl activity. Then, a tin tetrachloride pentahydrate aqueous solution is slowly added dropwise. Tin ions in the system partially hydrolyze in the aqueous solution and are electrostatically attracted to the surface hydroxyl groups of silica upon approaching the silica surface. A certain amount of sodium hydroxide aqueous solution is then added dropwise to control the pH of the system at a weakly alkaline condition of 9-10. The tin ions undergo further alkaline hydrolysis to generate tin hydroxide precipitate, which is directionally deposited on the surface of the silica particles. After a isothermal reaction and aging process of 0.5-1 hour, the tin hydroxide precipitate dehydrates and transforms into tin oxide, forming a continuous and uniform shell coating the silica surface, thus obtaining core-shell silica.

[0014] Further, in step B1, the ratio of cyclohexane, polyoxyethylene tert-octylphenyl ether, n-hexanol, deionized water, tetraethyl orthosilicate, and ammonia solution is 300-400 mL: 100-120 g: 80-100 mL: 15-20 mL: 1-2 g: 5-7 mL, and the concentration of the ammonia solution is 50-70 wt%. The post-treatment step includes: after the reaction is complete, wait for the reaction solution to cool to room temperature, add 150-200 mL of ethanol to precipitate the precipitate, filter, wash the filter cake 2-4 times with deionized water and ethanol, transfer it to an oven at 50-60°C, and dry it until... The core-shell silica precursor was obtained by constant weight. In step B2, the ratio of the core-shell silica precursor, deionized water, and tin tetrachloride pentahydrate solution was 2-4g:40-80mL:100-150mL. The concentration of the tin tetrachloride pentahydrate solution was 0.3-0.5mol / L, and the concentration of the sodium hydroxide solution was 1.5-2mol / L. The post-treatment steps included: after the reaction was completed, the reaction solution was cooled to room temperature, filtered, the filter cake was washed 2-4 times with deionized water and ethanol, transferred to an oven at 50-60℃, and dried to constant weight to obtain core-shell silica.

[0015] Furthermore, the modified antistatic agent is prepared by: placing Eucommia ulmoides gum and toluene in a reaction vessel and stirring; heating the reaction vessel to 75-85℃ and stirring for 15-30 minutes; adding glycidyl methacrylate, polyethylene glycol diacrylate and benzoyl peroxide; and reacting for 4-6 hours; and then performing post-treatment to obtain the modified antistatic agent.

[0016] The preparation reaction formula for the modified antistatic agent is as follows:

[0017] The preparation reaction principle of modified antistatic agents is as follows: During the reaction, under high temperature conditions, benzoyl peroxide decomposes to generate free radicals, which initiate free radical polymerization of eucommia gum, glycidyl methacrylate, and polyethylene glycol diacrylate to obtain a modified antistatic agent.

[0018] Furthermore, the ratio of Eucommia ulmoides gum, toluene, glycidyl methacrylate, polyethylene glycol diacrylate, and benzoyl peroxide is 4-6g:80-100mL:4-6g:2-4g:0.3-0.5g. The post-treatment steps include: after the reaction is completed, the reaction system is cooled to room temperature, the reaction solution is added to anhydrous ethanol for precipitation, filtered, the filter cake is washed 2-4 times with deionized water and acetone, transferred to an oven at 50-60℃, and dried to constant weight to obtain the modified antistatic agent.

[0019] This invention also proposes a method for preparing fully matte and antistatic polyester fibers, comprising the following steps: S1. Place polyethylene terephthalate, silicone resin filler, modified antistatic agent and auxiliary additives in a high-speed homogenizer and mix evenly to obtain a mixture; S2. Add the mixture to a twin-screw extruder, melt extrude, and spin to obtain polyester fibers.

[0020] The reaction principle for the preparation of polyester fibers is as follows: During the reaction, under heating conditions, the epoxy groups in the modified antistatic agent undergo a ring-opening reaction with the hydroxyl and amino groups in polyethylene terephthalate and silicone resin filler to form chemical bonds, thus obtaining polyester fibers.

[0021] Further, in step S2, the auxiliary additive is composed of plasticizer, flame retardant, antioxidant and lubricant in a mass ratio of 4:2:2:4. The plasticizer is one or more of diisononyl phthalate, dioctyl adipate and dibutyl sebacate. The flame retardant is one or more of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, triphenyl phosphate and magnesium hydroxide. The antioxidant is one or more of tris(2,4-di-tert-butylphenyl) phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and dioctadecyl thiodipropionate. The lubricant is one or more of oleamide, paraffin and oleic acid. Furthermore, the temperatures of the eight temperature zones of the twin-screw extruder from the feed inlet to the discharge outlet are 190℃, 190℃, 200℃, 200℃, 220℃, 220℃, 250℃, and 250℃ respectively. The main engine speed of the twin-screw extruder is 120-160 rpm, and the pressure is 80-120 bar.

[0022] The present invention has the following beneficial effects: 1. This invention relates to a modified antistatic agent obtained by graft polymerization of Eucommia ulmoides gum with glycidyl methacrylate and polyethylene glycol diacrylate under the initiation of benzoyl peroxide. The antistatic agent's molecular structure incorporates hydrophilic polyethylene glycol segments, an Eucommia ulmoides gum backbone, and active epoxy functional groups. This gives it not only good polarity and flexibility but also the ability to undergo ring-opening reactions with the carboxyl or hydroxyl groups at the ends of the polyester molecular chains, forming covalent bonds. This improves its dispersibility and durability in the polyester matrix and facilitates migration to the fiber surface during fiber forming. This antistatic agent enhances the adsorption capacity of water molecules on the fiber surface, effectively reduces the surface resistance of the fiber, and significantly improves the problem of static electricity accumulation in polyester fibers. At the same time, the epoxy groups in this antistatic agent can also react with the hydroxyl or amino functional groups on the surface of silicone resin fillers to construct a chemical bridging structure between the antistatic agent, filler, and polyester, which enhances the interfacial compatibility and stability of the entire fiber material system. This makes the modified antistatic agent less likely to precipitate or migrate, and it can maintain its functional integrity during high-temperature melt extrusion and spinning, thus achieving long-term and stable antistatic modification of polyester fibers.

[0023] 2. This invention involves the hydrolysis and condensation of tetraethyl orthosilicate under alkaline catalysis to obtain a core-shell silica precursor. Further, a tin oxide shell structure is modified onto its exterior using a chemical precipitation method to obtain core-shell silica. Firstly, the nanoparticle size and shell structure of the core-shell silica provide excellent dispersibility, enabling it to be uniformly distributed within the polyester matrix during melt spinning, forming a micro-reinforcing network and effectively improving the mechanical strength of the fiber. Secondly, the tin element contained in the shell of the core-shell silica imparts certain conductivity and ion migration capabilities, synergistically promoting the improvement of electrostatic accumulation in polyester fibers. Furthermore, the inorganic core structure of the core-shell silica possesses excellent light scattering capabilities, significantly reducing the gloss of the fiber surface, increasing haze, and improving the extinction performance of the fiber, giving it a soft, matte visual effect. As a precursor to silicone resin fillers, the surface functional groups of the core-shell silica provide reaction sites for subsequent organic modification, enhancing the interfacial compatibility between the filler and the polyester matrix, and contributing to the improvement of fiber structure stability.

[0024] 3. This invention involves modifying the surface of core-shell silica with various organosilane coupling agents and functional small molecules to obtain an organic-inorganic hybrid silicone resin filler. This silicone resin filler not only possesses the dimensional stability and optical properties of inorganic silica, but also improves its compatibility and reactivity with the polyester matrix through the introduction of organic functional groups. Furthermore, the silicone resin filler exhibits nanoscale particle size and uniform dispersion characteristics, enabling it to be fully dispersed in the molten polyester system, forming a stable three-dimensional filler network structure, thus enhancing the mechanical strength of the polyester fibers. The inorganic phase in the filler provides skeletal support, enhancing the structural integrity of the polyester fibers, while the organic segments provided by the silane coupling agent improve its compatibility with... The interfacial compatibility of polyester molecules reduces interfacial delamination and improves the overall stability of the composite material. Secondly, the silicone resin filler contains a large number of hydroxyl groups in its structure, which can chemically react with the epoxy groups in the polyester molecular chain and the modified antistatic agent to form a certain cross-linking structure during high-temperature melting, thereby inhibiting the migration of functional components and improving the antistatic durability and dispersion stability of polyester fibers. In addition, the inorganic components in the silicone resin filler have good light scattering ability, which can significantly reduce the gloss of polyester fibers, improve their haze and matteness, and make the fiber surface present a soft, matte texture, thus improving the visual quality of polyester fibers in high-end applications such as clothing fabrics. Detailed Implementation

[0025] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] The polyethylene terephthalate used in this invention was purchased from Dongguan Lerui Plastics Co., Ltd., model NRSC2697, brand name nairui, with a molecular weight of 30-50K. The Eucommia ulmoides gum used in this invention was purchased from Guangdong Fangxin Biotechnology Co., Ltd., under the brand name Penglei, and is classified as a superior grade.

[0027] Example 1 This embodiment provides a method for preparing core-shell silica for use in modified silicone resin for fully matte and antistatic polyester fibers, comprising the following steps: Step I: Preparation of core-shell silica precursor Weigh out 3000 mL of cyclohexane, 1000 g of polyoxyethylene tert-octylphenyl ether, 800 mL of n-hexanol and 150 mL of deionized water and place them in a reaction vessel and stir. Add 10 g of tetraethyl orthosilicate and react at room temperature for 1 h. Add 50 mL of ammonia solution and stir at room temperature for 4 h. After the reaction is complete, wait for the reaction solution to cool to room temperature and add 1500 mL of ethanol to precipitate the precipitate. Filter the precipitate and wash it twice with deionized water and ethanol. Transfer the precipitate to an oven at 50 °C and dry it to constant weight to obtain the core-shell silica precursor.

[0028] Step II: Preparation of core-shell silica Weigh 20g of core-shell silica precursor and 400mL of deionized water and place them in a reaction vessel. Heat the reaction vessel to 55℃ and stir for 15min. Slowly add 1000mL of 0.3mol / L tin tetrachloride pentahydrate aqueous solution and add 1.5mol / L sodium hydroxide aqueous solution until the pH of the system is 9. Keep the reaction vessel at this temperature for 0.5h. After the reaction is complete, wait for the reaction solution to cool to room temperature, filter it, wash the filter cake twice with deionized water and ethanol, transfer it to an oven at 50℃, and dry it to constant weight to obtain core-shell silica.

[0029] Example 2 This embodiment provides a method for preparing core-shell silica for use in modified silicone resin for fully matte and antistatic polyester fibers, comprising the following steps: Step I: Preparation of core-shell silica precursor Weigh out 3500 mL of cyclohexane, 1100 g of polyoxyethylene tert-octylphenyl ether, 900 mL of n-hexanol and 175 mL of deionized water and place them in a reaction vessel and stir. Add 15 g of tetraethyl orthosilicate and react at room temperature for 1.5 h. Add 60 mL of ammonia solution and stir at room temperature for 5 h. After the reaction is complete, wait for the reaction solution to cool to room temperature, add 1750 mL of ethanol to precipitate the precipitate, filter, wash the filter cake three times with deionized water and ethanol, transfer it to an oven at 55 °C and dry it to constant weight to obtain the core-shell silica precursor.

[0030] Step II: Preparation of core-shell silica Weigh 30g of core-shell silica precursor and 600mL of deionized water and place them in a reaction vessel. Heat the reaction vessel to 60℃ and stir for 20min. Slowly add 1250mL of 0.4mol / L tin tetrachloride pentahydrate aqueous solution and add 1.7mol / L sodium hydroxide aqueous solution until the pH of the system is 9.5. Keep the reaction vessel at this temperature for 0.5h. After the reaction is complete, wait for the reaction solution to cool to room temperature, filter it, wash the filter cake three times with deionized water and ethanol, transfer it to an oven at 55℃ and dry it to constant weight to obtain core-shell silica.

[0031] Example 3 This embodiment provides a method for preparing core-shell silica for use in modified silicone resin for fully matte and antistatic polyester fibers, comprising the following steps: Step I: Preparation of core-shell silica precursor Weigh out 4000 mL of cyclohexane, 1200 g of polyoxyethylene tert-octylphenyl ether, 1000 mL of n-hexanol and 200 mL of deionized water and place them in a reaction vessel and stir. Add 20 g of tetraethyl orthosilicate and react at room temperature for 2 h. Add 70 mL of ammonia solution and stir at room temperature for 6 h. After the reaction is complete, wait for the reaction solution to cool to room temperature, add 2000 mL of ethanol to precipitate the precipitate, filter, wash the filter cake 4 times with deionized water and ethanol, transfer it to an oven at 60 °C and dry it to constant weight to obtain the core-shell silica precursor.

[0032] Step II: Preparation of core-shell silica Weigh 40g of core-shell silica precursor and 800mL of deionized water and place them in a reaction vessel. Heat the reaction vessel to 65℃ and stir for 30min. Slowly add 1500mL of 0.5mol / L tin tetrachloride pentahydrate aqueous solution and add 2mol / L sodium hydroxide aqueous solution until the pH of the system is 10. Keep the reaction vessel at this temperature for 1h. After the reaction is complete, wait for the reaction solution to cool to room temperature, filter it, wash the filter cake 4 times with deionized water and ethanol, transfer it to an oven at 60℃ and dry it to constant weight to obtain core-shell silica.

[0033] Example 4 This embodiment provides a method for preparing fully matte and antistatic polyester fibers, including the following steps: Step ①: Preparation of dispersion Weigh 20g of the core-shell silica prepared in Example 1 and 500mL of n-butanol and place them in a reaction vessel. Stir at room temperature for 20min to obtain a dispersion.

[0034] Step 2: Preparation of silicone resin filler Weigh out 80g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 70g of phenyltrimethoxysilane, 2g of 2,4-dihydroxyacetophenone, 600mL of deionized water, and 10mL of n-butanol and place them in a reaction vessel. Stir, slowly add 200mL of dispersion, heat the reaction vessel to 40℃, and keep the reaction at this temperature for 15min. Add 10mL of 50wt% concentrated sulfuric acid, heat the reaction vessel to 80℃, and keep the reaction at this temperature for 4h. After the reaction is complete, let the reaction solution cool to room temperature and stand for 4h. Filter the solution, wash the filter cake twice with deionized water and ethanol, transfer it to an oven at 50℃, dry it to constant weight, grind it, and pass it through a 500-mesh sieve to obtain silicone resin filler.

[0035] Example 5 This embodiment provides a method for preparing fully matte and antistatic polyester fibers, including the following steps: Step ①: Preparation of dispersion Weigh 30g of the core-shell silica prepared in Example 2 and 750mL of n-butanol and place them in a reaction vessel. Stir at room temperature for 30min to obtain a dispersion.

[0036] Step 2: Preparation of silicone resin filler Weigh out 90g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 80g of phenyltrimethoxysilane, 3g of 2,4-dihydroxyacetophenone, 700mL of deionized water, and 15mL of n-butanol and place them in a reaction vessel. Stir, slowly add 300mL of dispersion, heat the reaction vessel to 45℃, and keep the reaction at this temperature for 20min. Add 15mL of 60wt% concentrated sulfuric acid, heat the reaction vessel to 85℃, and keep the reaction at this temperature for 5h. After the reaction is complete, let the reaction solution cool to room temperature and stand for 5h. Filter the solution, wash the filter cake three times with deionized water and ethanol, transfer it to an oven at 55℃, dry it to constant weight, grind it, and pass it through a 500-mesh sieve to obtain the silicone resin filler.

[0037] Example 6 This embodiment provides a method for preparing fully matte and antistatic polyester fibers, including the following steps: Step ①: Preparation of dispersion Weigh 40g of the core-shell silica prepared in Example 3 and 1000mL of n-butanol and place them in a reaction vessel. Stir at room temperature for 40min to obtain a dispersion.

[0038] Step 2: Preparation of silicone resin filler Weigh out 100g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 90g of phenyltrimethoxysilane, 4g of 2,4-dihydroxyacetophenone, 800mL of deionized water, and 20mL of n-butanol and place them in a reaction vessel. Stir, slowly add 400mL of dispersion, heat the reaction vessel to 50℃, and keep the reaction at this temperature for 30min. Add 20mL of 70wt% concentrated sulfuric acid, heat the reaction vessel to 90℃, and keep the reaction at this temperature for 6h. After the reaction is complete, let the reaction solution cool to room temperature and stand for 6h. Filter the solution, wash the filter cake four times with deionized water and ethanol, transfer it to an oven at 60℃, dry it to constant weight, grind it, and pass it through a 500-mesh sieve to obtain the silicone resin filler.

[0039] Example 7 This embodiment provides a method for preparing fully matte and antistatic polyester fibers, including the following steps: Step 1: Preparation of modified antistatic agent Weigh out 40g of Eucommia ulmoides gum and 800mL of toluene and place them in a reaction vessel. Stir the reaction vessel to 75℃ and keep it at that temperature for 15min. Add 40g of glycidyl methacrylate, 20g of polyethylene glycol diacrylate and 3g of benzoyl peroxide. Keep the reaction vessel at that temperature for 4h. After the reaction is complete, wait for the reaction system to cool to room temperature. Add the reaction solution to anhydrous ethanol for precipitation. Filter the solution and wash the filter cake twice with deionized water and acetone. Transfer the filter cake to an oven at 50℃ and dry it to constant weight to obtain the modified antistatic agent.

[0040] Step 2: Preparation of the mixture Diisononyl phthalate, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] and oleic acid were mixed evenly in a mass ratio of 4:2:2:4 to obtain an auxiliary additive for later use. Weigh out the following by weight: 60 parts polyethylene terephthalate, 4 parts silicone resin filler prepared in Example 4, 10 parts modified antistatic agent and 1 part auxiliary additive, place them in a high-speed homogenizer and mix them evenly to obtain a mixture.

[0041] Step 3: Preparation of polyester fibers The mixture is added to a twin-screw extruder, melt-extruded, and then extruded through a 0.3mm orifice filament spinneret. After being stretched three times and air-cooled in an annular manner, polyester fibers are obtained. The twin-screw extruder has eight temperature zones from the feed inlet to the discharge outlet, with temperatures of 190℃, 190℃, 200℃, 200℃, 220℃, 220℃, 250℃, and 250℃ respectively. The main motor speed of the twin-screw extruder is 120 rpm, and the pressure is 80 bar.

[0042] Example 8 This embodiment provides a method for preparing fully matte and antistatic polyester fibers, including the following steps: Step 1: Preparation of modified antistatic agent Weigh out 50g of Eucommia ulmoides gum and 900mL of toluene and place them in a reaction vessel. Stir the reaction vessel to 80℃ and keep it at that temperature for 20min. Add 50g of glycidyl methacrylate, 30g of polyethylene glycol diacrylate and 4g of benzoyl peroxide. Keep the reaction vessel at that temperature for 5h. After the reaction is complete, wait for the reaction system to cool to room temperature. Add the reaction solution to anhydrous ethanol for precipitation. Filter the solution and wash the filter cake three times with deionized water and acetone. Transfer the filter cake to an oven at 55℃ and dry it to constant weight to obtain the modified antistatic agent.

[0043] Step 2: Preparation of the mixture Diisononyl phthalate, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] and oleic acid were mixed evenly in a mass ratio of 4:2:2:4 to obtain an auxiliary additive for later use. Weigh out the following by weight: 70 parts polyethylene terephthalate, 5 parts silicone resin filler prepared in Example 5, 12.5 parts modified antistatic agent and 2 parts auxiliary additives, place them in a high-speed homogenizer and mix them evenly to obtain a mixture.

[0044] Step 3: Preparation of polyester fibers The mixture is added to a twin-screw extruder, melt-extruded, and then extruded through a 0.4mm orifice filament spinneret. After being drawn 3.5 times and air-cooled in an annular manner, polyester fibers are obtained. The twin-screw extruder has eight temperature zones from the feed inlet to the discharge outlet, with temperatures of 190℃, 190℃, 200℃, 200℃, 220℃, 220℃, 250℃, and 250℃ respectively. The main motor speed of the twin-screw extruder is 140 rpm, and the pressure is 100 bar.

[0045] Example 9 This embodiment provides a method for preparing fully matte and antistatic polyester fibers, including the following steps: Step 1: Preparation of modified antistatic agent Weigh out 60g of Eucommia ulmoides gum and 1000mL of toluene and place them in a reaction vessel. Stir the reaction vessel to 85℃ and keep it at that temperature for 30min. Add 60g of glycidyl methacrylate, 40g of polyethylene glycol diacrylate and 5g of benzoyl peroxide. Keep the reaction vessel at that temperature for 6h. After the reaction is complete, wait for the reaction system to cool to room temperature. Add the reaction solution to anhydrous ethanol for precipitation. Filter the solution and wash the filter cake four times with deionized water and acetone. Transfer the filter cake to an oven at 60℃ and dry it to constant weight to obtain the modified antistatic agent.

[0046] Step 2: Preparation of the mixture Diisononyl phthalate, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] and oleic acid were mixed evenly in a mass ratio of 4:2:2:4 to obtain an auxiliary additive for later use. Weigh out the following by weight: 80 parts polyethylene terephthalate, 6 parts silicone resin filler prepared in Example 6, 15 parts modified antistatic agent and 3 parts auxiliary additives, place them in a high-speed homogenizer and mix them evenly to obtain a mixture.

[0047] Step 3: Preparation of polyester fibers The mixture is added to a twin-screw extruder, melt-extruded, and then extruded through a 0.5mm orifice filament spinneret. After being drawn 4 times and air-cooled in an annular manner, polyester fibers are obtained. The twin-screw extruder has eight temperature zones from the feed inlet to the discharge outlet, with temperatures of 190℃, 190℃, 200℃, 200℃, 220℃, 220℃, 250℃, and 250℃ respectively. The main motor speed of the twin-screw extruder is 160 rpm, and the pressure is 120 bar.

[0048] Comparative Example 1 The difference between this comparative example and Example 9 is that, in step ①, an equal amount of core-shell silica precursor is used to replace the core-shell silica in the preparation of the dispersion.

[0049] Comparative Example 2 The difference between this comparative example and Example 9 is that the addition of Eucommia ulmoides gum was omitted in step (1) when preparing the modified antistatic agent.

[0050] Comparative Example 3 The difference between this comparative example and Example 9 is that the modified antistatic agent was omitted when preparing the mixture in step (2).

[0051] Performance testing: The breaking strength and elongation at break of the polyester fibers prepared in Examples 7-9 and Comparative Examples 1-3 were tested in accordance with the standard GB / T 14337-2008 "Test Method for Tensile Properties of Chemical Fibers (Short Fibers)". The volume resistivity of the polyester fibers prepared in Examples 7-9 and Comparative Examples 1-3 was tested in accordance with the standard GB / T 12703.4-2010 "Evaluation of electrostatic properties of textiles - Part 4: Resistivity". The gloss of the polyester fibers prepared in Examples 7-9 and Comparative Examples 1-3 was tested in accordance with the standard FZ / T 01097-2006 "Test Method for Fabric Gloss". The haze of the polyester fibers prepared in Examples 7-9 and Comparative Examples 1-3 was tested in accordance with the standard GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics". The water absorption rate of the polyester fibers prepared in Examples 7-9 and Comparative Examples 1-3 was tested according to the standard GB / T 21655.1-2023 "Evaluation of moisture absorption and quick-drying properties of textiles - Part 1: Single combination test method". The specific data are shown in Table 1.

[0052] Table 1 - Performance Test Data for Each Sample

[0053] Data Analysis: A comparative analysis of the data in Table 1 reveals that the polyester fiber prepared in this invention has a breaking strength of 4.2 cN·dtex, a breaking elongation of 31.2%, and a volume resistivity of 3.5 × 10⁻⁶. 9 While exhibiting a gloss level of 34 GU and a haze of 17%, the water absorption rate was 11.2%, all of which were superior to the comparative example. This invention obtains a modified antistatic agent through graft polymerization of Eucommia ulmoides gum, glycidyl methacrylate, and polyethylene glycol diacrylate under benzoyl peroxide initiation. A core-shell silica precursor is obtained by hydrolyzing and condensing tetraethyl orthosilicate under alkaline catalysis. Further, a tin oxide shell structure is modified on its exterior using a chemical precipitation method to obtain core-shell silica. By modifying the surface of the core-shell silica with various organosilane coupling agents and functional small molecules, an organic-inorganic hybrid silicone resin filler is obtained. This filler not only improves the antistatic and matting properties of polyester fibers but also enhances their hydrophilicity and mechanical strength.

[0054] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A fully matte, antistatic polyester fiber, characterized in that, It includes the following components by weight: 60-80 parts polyethylene terephthalate, 4-6 parts silicone resin filler, 10-15 parts modified antistatic agent and 1-3 parts auxiliary additives. The auxiliary additives consist of plasticizers, flame retardants, antioxidants, and lubricants in a mass ratio of 4:2:2:4; The silicone resin filler is prepared by the following steps: A1. Place the core-shell silica and n-butanol in a reaction vessel and stir at room temperature for 20-40 minutes to obtain a dispersion. A2. Place 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, phenyltrimethoxysilane, 2,4-dihydroxyacetophenone, deionized water and n-butanol in a reaction vessel and stir. Slowly add the dispersion. Heat the reaction vessel to 40-50℃ and keep it at this temperature for 15-30 min. Add concentrated sulfuric acid and heat the reaction vessel to 80-90℃. Keep it at this temperature for 4-6 h. Post-treatment yields the silicone resin filler. The core-shell silica is prepared by the following steps: B1. Cyclohexane, polyoxyethylene tert-octylphenyl ether, n-hexanol and deionized water were placed in a reaction vessel and stirred. Tetraethyl orthosilicate was added and reacted at room temperature for 1-2 hours. Ammonia solution was added and stirred at room temperature for 4-6 hours. Post-treatment was then performed to obtain the core-shell silica precursor. B2. Place the core-shell silica precursor and deionized water in a reaction vessel, heat the reaction vessel to 55-65℃, keep it at this temperature and stir for 15-30 min, slowly add tin tetrachloride pentahydrate aqueous solution, add sodium hydroxide aqueous solution until the pH of the system is 9-10, keep it at this temperature for 0.5-1 h, and then process it to obtain core-shell silica. The modified antistatic agent is prepared by: placing Eucommia ulmoides gum and toluene in a reaction vessel and stirring; heating the reaction vessel to 75-85℃ and stirring for 15-30 minutes; adding glycidyl methacrylate, polyethylene glycol diacrylate and benzoyl peroxide; and reacting for 4-6 hours; and then performing post-treatment to obtain the modified antistatic agent.

2. The fully matte antistatic polyester fiber according to claim 1, characterized in that, In step A1, the ratio of core-shell silica to n-butanol is 2-4 g: 50-100 mL; in step A2, the ratio of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, phenyltrimethoxysilane, 2,4-dihydroxyacetophenone, deionized water, n-butanol, dispersion, and concentrated sulfuric acid is 8-10 g: 7-9 g: 0.2-0.4 g: 60-80 mL: 1-2 mL: 20-40 mL: 1-2 mL, and the concentration of concentrated sulfuric acid is 50-70 wt%.

3. The fully matte antistatic polyester fiber according to claim 1, characterized in that, In step B1, the ratio of cyclohexane, polyoxyethylene tert-octylphenyl ether, n-hexanol, deionized water, tetraethyl orthosilicate, and ammonia solution is 300-400 mL: 100-120 g: 80-100 mL: 15-20 mL: 1-2 g: 5-7 mL, and the concentration of the ammonia solution is 50-70 wt%. In step B2, the ratio of the core-shell silica precursor, deionized water, and tin tetrachloride pentahydrate solution is 2-4 g: 40-80 mL: 100-150 mL, the concentration of the tin tetrachloride pentahydrate solution is 0.3-0.5 mol / L, and the concentration of the sodium hydroxide solution is 1.5-2 mol / L.

4. The fully matte antistatic polyester fiber according to claim 1, characterized in that, The ratio of the amounts of Eucommia ulmoides gum, toluene, glycidyl methacrylate, polyethylene glycol diacrylate, and benzoyl peroxide is 4-6g:80-100mL:4-6g:2-4g:0.3-0.5g.

5. A method for preparing the fully matte antistatic polyester fiber according to any one of claims 1-4, characterized in that, Includes the following steps: S1. Place polyethylene terephthalate, silicone resin filler, modified antistatic agent and auxiliary additives in a high-speed homogenizer and mix evenly to obtain a mixture; S2. Add the mixture to a twin-screw extruder, melt extrude, and spin to obtain polyester fibers.

Citation Information

Patent Citations

  • Antistatic polyester fiber and preparation method thereof

    CN107699976A