Antireflection film, method of manufacturing, use and electronic device
By applying an electrostatic field and corona treatment during the preparation of the antireflective film, the surface energy and roughness of the film are improved, which solves the problem of poor wear resistance of existing antireflective films and achieves a significant improvement in the wear resistance and service life of the film.
Patent Information
- Application Number
- CN202511683271.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-11-17
AI Technical Summary
Existing antireflective films have poor wear resistance, short service life, and poor practicality.
In the preparation of the antireflective film, an electrostatic field, especially a DC electric field, is applied during corona treatment to increase the surface energy and roughness of the film, and the AF layer is stably attached after baking, thereby improving the wear resistance of the AF layer.
It significantly improves the wear resistance and service life of the anti-reflective film, ensuring that the AF layer can still maintain good hydrophobicity and anti-fouling ability after high-frequency wiping.
Smart Images

Figure CN121364517B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of optical film technology, specifically relating to an anti-reflective film, its preparation method, its application, and electronic equipment. Background Technology
[0002] The top layer of existing anti-reflective products is the AF layer (Anti-Fingerprint), which literally means anti-fingerprint film. It has anti-fingerprint properties, strong stain resistance, and is easy to clean. The film surface must not only resist the touch of different hands, scratches from fingernails, friction from various fabric pockets, and damage from hard objects like keys, but also resist corrosion from oil, salt, soy sauce, and vinegar used in daily life, as well as sun, wind, and rain. The film must meet certain requirements, such as being waterproof, moisture-proof, abrasion-resistant, stain-resistant, and easy to clean. AF film can maximize these capabilities of conventional films. Existing anti-reflective products have poor abrasion resistance, short service life, and limited practicality.
[0003] Therefore, in view of the above-mentioned technical problems, it is necessary to provide an anti-reflective film, a preparation method, an application, and an electronic device. Summary of the Invention
[0004] The purpose of this invention is to provide an anti-reflective film, its preparation method, its application, and an electronic device.
[0005] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:
[0006] The anti-reflective film includes a substrate layer, a hardening layer, an AR layer, and an AF layer arranged in sequence. After the AR layer is formed, it undergoes corona treatment under an additional applied electrostatic field before the AF layer is formed.
[0007] In one or more embodiments of the present invention, the corona treatment is an automatic program of the spraying machine, and the electric arc of each tip discharge is kept consistent by the automatic program, with its voltage controlled at 500V.
[0008] In one or more embodiments of the present invention, the electrostatic field satisfies the following conditions: the DC voltage is 50-1000V, and the electric field direction is towards the AR layer. Preferably, the voltage is 100-200V. The corona distance remains consistent, and the electric field strength is only related to the voltage. The DC power supply can be an MDX1.5K power supply from Advanced Technology & Materials Co., Ltd. (AE), USA, etc.
[0009] In one or more embodiments of the present invention, the electrostatic field is a DC pulsed electric field with a pulse frequency of 80-250Hz.
[0010] In one or more embodiments of the present invention, during the preparation process, the AF layer is dried immediately after coating.
[0011] In one or more embodiments of the present invention, the substrate is selected from: PET, SRF, TAC, PMMA, PC, COP, and glass.
[0012] In one or more embodiments of the present invention, the method for preparing the antireflective film is characterized by comprising the following steps:
[0013] a. Corona treatment: Select a substrate coated with an anti-reflective functional layer (AR layer), and perform corona discharge treatment on the surface of the substrate in the electric field applied by a DC power supply.
[0014] b. Preparation of AF layer: Apply AF solution (anti-fingerprint liquid, composed of perfluorocyclic ether, particle size 2-80nm) to the surface of the corona-treated substrate.
[0015] c. Curing treatment: Place the substrate coated with AF solution into an oven for baking, and let it stand after baking.
[0016] In one or more embodiments of the present invention, the baking process satisfies the following conditions: the baking temperature is 100-150°C, the baking time is 3-10 minutes, and / or the resting time is 24-72 hours.
[0017] In one or more embodiments of the present invention, an anti-reflective film is applied to a terminal having a viewing window. The terminal may be, for example, eyeglasses (including smart glasses), a window, a HUD device, etc.
[0018] In one or more embodiments of the present invention, an electronic device includes a display and an anti-reflective film disposed on the display window. This device can be a mobile phone, computer, portable computer, etc.
[0019] Compared with existing technologies, the antireflective film, preparation method, application, and electronic device of this invention, by introducing an electric field during the corona treatment, allows the tip discharge energy to penetrate the entire film, thereby increasing both the surface energy and corona depth, and improving its roughness. This enables the subsequent spraying of the AF solution to be efficiently and stably coated onto the AR layer. Finally, the AF-coated film is placed in an oven to bake and heat the AF layer, allowing it to stand for a period of time to further stabilize its adhesion to the film. This effectively improves the wear resistance and practicality of the AF film. Furthermore, the method of this invention is convenient, effective, environmentally friendly, and low-cost. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 This is a schematic diagram of the structure of the antireflective film in one embodiment of the present invention;
[0022] Figure 2 This is a schematic diagram illustrating the process comparison of the antireflective film in one embodiment of the present invention;
[0023] Figure 3 The following are comparative images of the abrasion resistance test results of the anti-reflective film in one embodiment of the present invention: a is a microscopic image of abrasion resistance after 10,000 cycles without corona treatment; b is a microscopic image of abrasion resistance after 10,000 cycles with corona treatment; c is a microscopic image of abrasion resistance after 10,000 cycles with corona treatment and an electric field of 100V; and d is a microscopic image of abrasion resistance after 10,000 cycles with corona treatment and an electric field of 200V.
[0024] Explanation of key figure labels:
[0025] 1. Protective film; 2. Substrate; 3. Hardened layer; 4. AR layer; 5. AF layer. Detailed Implementation
[0026] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments disclosed herein. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.
[0027] like Figure 1 As shown, one structure of the antireflective film of the present invention can be formed sequentially as a substrate 2, a hardened layer 3, an AR layer 4, and an AF layer 5. In this case, the AR layer 4 can undergo corona treatment, applying an additional electric field during the corona treatment. Of course, a protective film 1 can also be additionally provided to protect the substrate 2.
[0028] The substrate with the functional layer (AR layer, mainly for anti-reflection) is subjected to corona treatment. A high-frequency AC voltage induces corona discharge on the plastic surface, generating low-temperature plasma. Electrons, ions, and photons in the plasma act on the film surface, causing polymer molecular chains to break and oxidize, generating polar groups such as carbonyl and peroxides. A new electric field is added during corona treatment, improving corona efficiency and significantly increasing the film's surface energy, thereby increasing surface tension, reducing surface contamination, and increasing the contact area, indirectly improving adhesion. This allows the AF solution (anti-fingerprint liquid, perfluorocyclic ether, 2-80nm) to be more stably coated on the functional layer. Finally, after baking the film in an oven for several minutes, it is left to stand for 48 hours to stabilize the AF coating before subsequent sample testing. Results show that after 10,000 cycles of standard abrasion testing, the water droplet angle is significantly improved. After 10,000 cycles of wiping with the improved AF-coated sample treated with an electric field and corona, the water droplet angle remains above 90°, and the AF layer on the product surface does not peel off. The sample surface also shows no pitting or scratches. This treatment method quickly and easily improves the abrasion resistance and performance of PET antireflective film, and is expected to occupy a new market share in the PET antireflective film industry.
[0029] To verify the improvement in wear resistance of the samples before and after the modification, the following four groups of different process treatments will be carried out: Group 1 is the sample without corona treatment, Group 2 is the ordinary corona treatment before the modification, Group 3 is the sample with DC power supply and 100V electric field applied during corona treatment, and Group 4 is the sample with 200V electric field applied. The four groups of different treatments will be tested and analyzed in the future.
[0030] AF optimization: To further improve the stability of the AF layer, the sprayed film is placed in an oven at 120°C for 5 minutes. Under high temperature, the AF solution sprayed on the AR layer of the film is cured faster, the drying time is shortened, and the risk of performance degradation due to incomplete curing is reduced.
[0031] Many materials, such as plastic films, have low surface tension, which can affect subsequent processing steps such as coating. For example, common polyethylene films have low surface tension when untreated, making it difficult for inks to adhere firmly and causing the coating to easily peel off. Corona treatment is an important step before coating. Under the action of a high-voltage electric field, when the local surface electric field strength exceeds the breakdown field strength, gas molecules ionize and react chemically with surface atoms or molecules. By adding an electric field, the molecular chains of non-polar plastics (such as polyethylene and polypropylene) can be broken down, forming active sites. Simultaneously, the strong oxidizing effect of ozone causes the formation of polar groups such as carbonyl and hydroxyl groups on the surface, resulting in tiny particles and pores. The resulting micro-uneven structure increases surface roughness and significantly enhances surface energy. This reduces surface contaminants, indirectly improving adhesion and allowing the AF solution to better adhere to the film surface, thereby indirectly improving the quality and wear resistance of the AF layer.
[0032] The original small-scale AF spraying machine used an insulating plate under the corona-coated sample film, which was grounded, preventing the surface corona treatment from penetrating the entire film. This limited its efficiency in improving roughness. To improve corona efficiency, an electric field was introduced simultaneously during corona treatment, and a steel plate was placed under the film sample to allow the electric field to penetrate the entire film. To reduce AC voltage fluctuations that caused inconsistent film treatment results, a stable power supply was essential. The new method adds a steel plate under the film and applies a 100V-200V electric field during corona treatment, further improving corona efficiency, increasing the film surface energy, and allowing the AF solution to adhere more efficiently and stably to the AR layer, thus improving the film's wear resistance.
[0033] Substrate pretreatment: Select the substrate with AR coating and cut it into A4 standard samples of 210mm×297mm using a utility knife and cutter to reduce errors in subsequent experiments and production.
[0034] Corona treatment: Place the standard sample into the corona device, and place a steel plate (instead of the traditional insulating plate) under the sample. Introduce a stable DC power supply (preferably AEMDX1.5K type) to apply an electric field of 50-1000V (preferably 100-200V). During the corona discharge process, the electric field penetrates the entire film, destroys the non-polar molecular chains on the PET surface, and generates polar groups such as carbonyl and hydroxyl groups. At the same time, it forms a micro-uneven structure on the surface, increases the surface roughness and surface energy, reduces surface contamination, and lays the foundation for the adhesion of AF solution.
[0035] AF layer preparation: A perfluorocyclic ether AF solution (particle size 2-80nm) is sprayed onto the surface of the corona-treated sample to enhance the bonding force between the AF solution and the AR layer by utilizing the increased surface energy and roughness.
[0036] Curing treatment: Place the sprayed sample in an oven and bake at 120℃ for 5 minutes to accelerate the curing of the AF solution; after baking, let it stand for 48 hours to allow the AF layer to adhere completely and stably, avoiding performance degradation due to incomplete curing.
[0037] Example 1
[0038] Substrate: AR-coated PET rolls;
[0039] Equipment: Small AF sprayer (including improved corona device), AEMDX1.5K DC power supply, oven (temperature control accuracy ±2℃), roughness tester (SJ-210), wear tester (ZJ-339-GSR), water droplet angle tester (RM-J08A), 3D laser microscope (LEXT-OLS5000);
[0040] Materials: AF solution (perfluorocyclic ether, 2-80nm), 0000# steel wool (BONSTAR, Japan).
[0041] Step 1: Sample Preparation
[0042] The AR-coated PET rolls were cut into A4 samples of 210mm×297mm. A total of 4 groups were prepared, with 3 parallel samples in each group, and were labeled as Group 1 (no corona), Group 2 (normal corona), Group 3 (corona + 100V electric field), and Group 4 (corona + 200V electric field).
[0043] Step 2: Corona treatment, in which...
[0044] Group 1: No corona treatment performed;
[0045] Group 2: Place the sample into the corona device (with an insulating plate underneath) for routine corona treatment. The corona treatment is an automatic program of the spraying machine. The electric arc of each tip discharge is kept consistent by the automatic program, and the voltage is controlled at 500V.
[0046] Group 3: Based on the group, optimize the process by placing a steel plate under the corona device sample, connecting it to an AE DC power supply, applying a 100V electric field, and performing corona treatment.
[0047] Group 4: Same operation as Group 3, apply a 200V electric field.
[0048] Step 3: AF spraying and curing
[0049] AF solution was evenly sprayed onto the surface of the four groups of samples, then placed in an oven and baked at 120°C for 5 minutes. After being removed, the samples were left to stand for 48 hours.
[0050] Roughness test data
[0051] In order to enable the AF solution to adhere well to the AR functional layer, the surface roughness of the film is increased by corona treatment. The presence of surface roughness increases the surface area of the film, which indirectly improves the adhesion of AF and thus enhances its wear resistance.
[0052] Table 1. Test data of film surface roughness after AR coating on PET substrate and different treatment methods.
[0053]
[0054] The micro-uneven structure generated by corona discharge increases surface roughness, reduces surface contaminants, and enhances surface energy, indirectly improving adhesion and allowing AF to better adhere to the AR layer. Surface roughness was characterized using an SJ-210 (178-560-02DC) roughness tester, where Ra represents the arithmetic mean of the absolute values of the ordinate within a sampling length, Rq represents the root mean square value of the ordinate within a sampling length, and Rz represents the sum of the maximum profile peak height and the maximum profile valley depth within a sampling length. The results show that the surface roughness of the film treated with an electric field corona discharge is significantly improved. After applying a 200V electric field, the overall roughness improvement is approximately twice that of ordinary corona discharge, greatly increasing the surface area and adhesion area, thus providing a foundation for subsequent improvement in wear resistance. Table 1 shows that Ra (0.072μm), Rq (0.090μm), and Rz (0.369μm) are the largest among the four groups in group 4, indicating that corona treatment under a 200V electric field has the best effect on improving surface roughness.
[0055] Standard abrasion resistance test experiment
[0056] Standard abrasion testing is a commonly used method for evaluating the abrasion resistance of materials, coatings, or surfaces. Abrasion testing machines are used to test the abrasion resistance of various materials, coatings, or surfaces to assess their abrasion resistance under actual use conditions. The abrasion testing machine used is the ZJ-339-GSR abrasion wiping machine. Its abrasion wiping test steel wool model is 0000# (BON STAR, Japan). The specific experimental method involves using a 20×20mm steel wool abrasion head, a load of 1000g, a stroke of 40mm, and an abrasion speed of 50 cycles per minute. Samples with different processing methods were prepared into 40×100mm samples, fixed to the cover plate with adhesive tape, and then placed on the abrasion machine for testing. The specific water droplet angle test data after abrasion are shown in Table 2.
[0057] Table 2. Test data of abrasion resistance and water droplet contact angle of sprayed samples after different treatments on PET substrates coated with AR.
[0058]
[0059] Steel wool abrasion test (ZJ-339-GSR abrasion tester) primarily characterizes the fingerprint film's resistance to abrasion from hard objects. For characterizing the effect of AF coating after abrasion resistance testing, surface energy and surface tension are mainly used. Surface tension is the most suitable testing method, and the most convenient and effective characterization method is the water droplet angle test. The water droplet angle is easy to detect and observe, and it is an important data control indicator for AF fingerprint resistance. The higher the water droplet angle, the better the hydrophobicity; the better the hydrophobicity, the better the fingerprint resistance. The industry standard is to measure the contact angle to characterize surface energy. The larger the value, the smaller the surface energy, indicating that liquids are less likely to adhere, fingerprints are less likely to adhere, and are easier to wipe off. Using the RM-J08A water droplet angle tester to test the abrasion resistance samples, when the water droplet angle on the sample surface is <70°, the AF layer on the surface has been completely worn away and peeled off, and its hydrophobicity has greatly decreased. The initial water droplet angle of the AF samples after corona treatment showed a slight increase, but the effect was not significant. However, with the increase of wear cycles, the water droplet angle changed significantly. Even after 10,000 wear cycles, it remained above 75°, and after corona treatment with an electric field, it remained above 90°. The samples still maintained good hydrophobicity. The water droplet angle results indicate that adding an electric field during corona treatment can significantly improve the wear resistance of the AF layer, and its effect is far superior to that of the uncorona treatment and the original corona treatment process. Table 2 shows that after 10,000 cycles, the water droplet angles of groups 3 and 4 were both above 90°, significantly higher than those of groups 1 (42.33°) and 2 (64.53°), proving that the introduction of an electric field can effectively improve the wear resistance stability of the AF layer.
[0060] To further and more accurately characterize the specific improvement in wear resistance of the sprayed AF samples after different treatments, the wear-resistant samples were placed under a 3D measuring laser microscope LEXT-OLS5000 for further observation. The four sets of microscopic results are as follows: Figure 3 The results show that: Group 1(a) and Group 2(b) samples have scratches and flakes on their surfaces, while Group 3(c) and Group 4(d) samples have only a very small amount of flakes and no scratches, further verifying the effectiveness of the process of the present invention.
[0061] The results showed that the untreated samples had lower surface energy, making it difficult for the AF layer to adhere well to the AR layer. After 10,000 abrasion cycles, the film sample surface exhibited severe scratches and pitting, and even more seriously, large-area flakes, significantly reducing product performance. After corona treatment, the AF layer adhered more stably to the AR layer. Even after 10,000 abrasion cycles, scratches were greatly reduced and less severe, pitting was significantly reduced, and no large-area flakes occurred. Subsequent improvements to the corona process, including the addition of an electric field, resulted in no scratches even after 10,000 abrasion cycles, with only a very small amount of pitting. The surface hydrophobicity did not decrease, and the AF layer adhered more stably to the AR layer, significantly improving the abrasion resistance of the PET product surface.
[0062] The standard abrasion tester tested the surface for 10,000 cycles under the conditions of steel wool (model 0000#, Japanese BONSTAR) as the abrasion head, 1000g load, 40mm stroke, and 50 cycles / minute. The surface water droplet angle remained above 90°, and the AF layer did not peel off or the surface was scratched.
[0063] To further optimize the wear resistance of the AF layer and improve its performance on different substrates, a pulsed power supply was added to the electric field to further enhance its surface roughness. The results of the roughness and wear resistance water droplet angle tests are shown in Tables 3 and 4.
[0064]
[0065]
[0066] Example 2: Using TAC substrate, a 100V electric field was applied during corona treatment, with other parameters the same as in Example 1. After 10,000 wear-resistant cycles, the finished product had a water droplet angle of 67.63°, a surface Ra of 0.066μm, and minor scratches.
[0067] Example 3: Using PMMA substrate, a 200V electric field was applied during corona treatment, with other parameters the same as in Example 1. After 10,000 wear-resistant cycles, the finished product had a water droplet angle of 65.62°, a surface Ra of 0.063μm, and minor scratches.
[0068] Example 4: Corona treatment was applied with a pulsed power supply (3000Hz, 10KW), and other parameters were the same as in Example 1. After 10,000 wear-resistant cycles, the water droplet angle of the finished product was 86.33°, and its surface roughness and adhesion were further improved compared to treatment without an introduced electric field.
[0069] Example 5: Corona treatment was performed using a 200V electric field powered by a DC pulse power supply (100Hz), with other parameters the same as in Example 1. After 10,000 wear-resistant cycles, the finished product exhibited a water droplet angle of 94.63° and a surface Ra of 0.069μm, meeting the wear resistance requirements of optical components.
[0070] Example 6: Corona treatment was performed using a 200V electric field powered by a DC pulse power supply (150Hz), with other parameters the same as in Example 1. After 10,000 wear-resistant cycles, the finished product exhibited a water droplet angle of 94.77° and a surface Ra of 0.085μm, meeting the wear resistance requirements of optical components.
[0071] Example 7: Corona treatment was performed using a 200V electric field powered by a DC pulse power supply (200Hz), with other parameters the same as in Example 1. After 10,000 wear-resistant cycles, the finished product exhibited a water droplet angle of 96.69° and a surface Ra of 0.096μm, meeting the wear resistance requirements of optical components.
[0072] Example 8: Corona treatment was performed using a 200V electric field powered by a DC pulse power supply (250Hz), with other parameters the same as in Example 1. After 10,000 wear-resistant cycles, the finished product exhibited a water droplet angle of 83.11° and a surface Ra of 0.055μm, meeting the wear resistance requirements of optical components.
[0073] Example 9: Corona treatment was performed using a 200V electric field with a DC pulse power supply (80Hz). All other parameters were the same as in Example 1. After 10,000 wear-resistant cycles, the finished product exhibited a water droplet angle of 79.65° and a surface Ra of 0.061μm, meeting the wear resistance requirements of optical components.
[0074] The final results show that TAC and PMMA substrates have very poor abrasion resistance, far inferior to PET substrates. After 2000 abrasion cycles, their water droplet angle drops below 70°. However, after optimization by introducing an electric field, the water droplet angle can be maintained above 80°. The addition of an electric field during corona treatment improves the abrasion resistance of different substrates. Further enhancement by adding a DC pulse power supply further improves the abrasion resistance of the PET anti-reflective film. The optimal process involves introducing a 200V electric field and a 200Hz DC pulse power supply during corona treatment.
[0075] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0076] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. An antireflective film comprising a substrate layer, a hardening layer, an AR layer, and an AF layer arranged sequentially, wherein the AR layer is subjected to corona treatment under an additional applied electric field after its formation, the corona treatment being performed by placing a steel plate under the film before the AF layer is formed, wherein the electric field satisfies the following conditions: the DC voltage is 50-1000V, and the electric field direction is towards the AR layer.
2. The antireflective film according to claim 1, characterized in that, The electric field is a DC pulse electric field with a pulse frequency of 80-250Hz.
3. The antireflective film according to claim 1, characterized in that, During the preparation process, the AF layer is dried immediately after coating.
4. The antireflective film according to claim 1, characterized in that, The substrate is selected from: PET, SRF, TAC, PMMA, PC, COP, and glass.
5. A method for preparing an antireflective film according to any one of claims 1-4, characterized in that, Includes the following steps: a. Corona treatment: Select a substrate coated with an anti-reflective functional layer, and perform corona discharge treatment on the surface of the substrate with a steel plate placed below it in an electric field applied by a DC power supply. The electric field satisfies the following: DC voltage is 50-1000V, and the electric field direction is towards the AR layer. b. Preparation of AF layer: Apply AF solution to the surface of the corona-treated substrate; c. Curing treatment: Place the substrate coated with AF solution into an oven for baking, and let it stand after baking.
6. The preparation method according to claim 5, characterized in that, The baking process satisfies the following conditions: the baking temperature is 100-150℃, the baking time is 3-10 minutes; and / or the resting time is 24-72 hours.
7. The application of the antireflective film according to any one of claims 1-4 on a terminal having a viewing window.
8. An electronic device, including a display and an antireflective film according to any one of claims 1-4 disposed on the display window.
Citation Information
Patent Citations
Magnetron sputtering coating treatment process
CN118726928A
KR20250057257A