Processing technology of anti-softening copper alloy for new energy automobile wire harness
By employing cryogenic high-energy drawing, aerosol low-temperature self-adsorption, and pulsed current skin flash diffusion processes, the thermal stress relaxation problem of copper alloy wires under the high voltage and high current environment of new energy vehicles has been solved. This has achieved gradient decoupling between the surface and core properties of the wire, improving its anti-softening performance and conductivity.
Patent Information
- Application Number
- CN202511931446.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-19
- Publication Date
- 2026-01-27
AI Technical Summary
Existing copper alloy wires are prone to thermal stress relaxation failure under the high voltage and high current environment of new energy vehicles, making it difficult to simultaneously achieve high conductivity and excellent resistance to high temperature softening. Furthermore, existing processes cannot meet the differentiated requirements for the radial properties of the wires.
The process employs cryogenic high-energy drawing, aerosol low-temperature self-adsorption, pulsed current skin flash diffusion, and gradient cooling and surface passivation steps. After cryogenic drawing, the low enthalpy carried by the wire blank itself forms a solid precursor ice film. High-frequency pulsed current is used to establish radial temperature and energy gradients on the surface of the wire blank, achieving high-temperature diffusion on the surface and medium-temperature precipitation in the core. Combined with chemical quenching process, grain growth is suppressed.
It significantly improves the softening resistance and conductivity of copper alloy wires, ensuring that they are not prone to thermal relaxation or softening failure in high-temperature environments. It also achieves gradient decoupling between the surface and core properties of the wire, meeting the high-current transmission requirements of new energy vehicles.
Abstract
Description
Technical Field
[0001] This invention relates to the field of non-ferrous metal material processing technology, specifically to a copper alloy processing technology for anti-softening new energy vehicle wiring harnesses. Background Technology
[0002] With the explosive growth of the new energy vehicle industry, the vehicle electrical system is evolving towards a high-voltage, high-current architecture, which places extremely stringent performance requirements on high-voltage wiring harnesses, the lifeblood of power transmission. During fast charging or high-power output, the wiring harness often bears a continuous high-current load, resulting in Joule heating and a significant increase in conductor temperature. Copper alloy wiring harnesses are highly susceptible to stress relaxation under such high-temperature and vibration-coupled environments, meaning that the material's internal dislocation structure recovers due to thermal activation. This manifests macroscopically as a decrease in contact pressure and tensile strength, leading to increased connector contact resistance, uncontrolled localized temperature rise, and even the risk of ablation. Therefore, improving the softening resistance of copper alloy wires under high-temperature conditions has become crucial for ensuring the electrical safety of the entire vehicle.
[0003] Currently, the industry primarily balances the strength and conductivity of copper alloys through alloying and deformation heat treatment. However, this traditional approach faces significant physical trade-offs: to improve softening resistance, it is typically necessary to increase the addition of alloying elements such as Cr, Zr, and Mg to form precipitation strengthening phases or solid solution strengthening effects. However, this significantly increases the probability of electron scattering, leading to a sharp decline in conductivity, making it difficult to meet the low transmission loss requirements of new energy vehicles. Although drastic cold working deformation can temporarily improve wire strength through work hardening, the high-energy deformed structure has extremely poor thermal stability, triggering recovery and recrystallization processes even at relatively low service temperatures, causing the wire to soften and fail rapidly, thus failing to meet the requirements for long-term high-temperature service.
[0004] More importantly, existing processing techniques typically involve uniform heat treatment of the wire as a whole, resulting in a uniform microstructure across the wire cross-section. However, in practical applications, the performance requirements of the wire differ fundamentally in the radial direction: the wire surface directly bears the contact stress and fretting wear at the connection ends, requiring extremely high resistance to creep and softening; while the wire core primarily carries current, demanding extremely high conductivity. Existing homogenization processes cannot simultaneously address these differentiated performance requirements, often sacrificing core conductivity to maintain surface strength, or limiting the improvement of surface softening resistance to ensure conductivity. Furthermore, existing surface modification technologies often rely on separate coating and high-temperature diffusion equipment, resulting in lengthy processes, high energy consumption, and difficulty in achieving a metallurgical-grade gradient transition with high adhesion between the modified layer and the substrate, thus limiting the further development and application of high-performance copper alloy wire harnesses. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a copper alloy processing technology for new energy vehicle wiring harnesses that resists softening. This technology solves the problem that existing copper alloy wires cannot simultaneously achieve high conductivity and excellent resistance to high-temperature softening, which leads to thermal stress relaxation failure under the high current transmission conditions of new energy vehicles.
[0006] To achieve the above objectives, the present invention provides the following technical solution: The first aspect of the present invention provides a copper alloy processing technology for anti-softening new energy vehicle wiring harnesses. The process includes raw material preparation and pretreatment, cryogenic high-energy state drawing, aerosol low-temperature self-adsorption, pulsed current skin flash diffusion, and gradient cooling and surface passivation steps.
[0007] Specifically, the process includes the following steps: In the raw material preparation and pretreatment steps, copper alloy wire blanks are selected, subjected to high-temperature solution treatment and quenching, and the surface of the wire blanks is purified and dried.
[0008] In the cryogenic high-energy drawing step, the pre-treated wire blank is placed in a cryogenic cooling medium for continuous drawing. The low-temperature environment suppresses the dynamic recovery of the metal lattice, allowing lattice distortion energy to accumulate inside the wire blank. At the same time, the process parameters are controlled so that the drawn wire blank is kept in a cryogenic frozen state when it enters the next process.
[0009] In the aerosol low-temperature self-adsorption step, the wire blank in a low-temperature frozen state is passed through a mist chamber filled with functional aerosol precursor liquid; by utilizing the temperature difference between the cold energy carried by the wire blank itself and the environment of the mist chamber, the functional aerosol precursor liquid is frozen in situ on the surface of the wire blank, forming a solid precursor ice film.
[0010] In the pulsed current skin flash diffusion step, a wire blank coated with a solid precursor ice film is passed through an electrode area under tension, and a high-frequency pulsed current is applied. The high-frequency pulsed current generates a skin effect on the cross-section of the wire blank, causing the current density to concentrate on the surface layer of the wire blank. The Joule heating generated by the skin effect causes the surface temperature of the wire blank to rise instantaneously, vaporizing and decomposing the solid precursor ice film on the surface, and driving the active solute to diffuse to the surface of the copper alloy matrix. At the same time, the thermal effect and electroplastic effect of the current are used to age the core of the wire blank.
[0011] In the gradient cooling and surface passivation steps, after the wire blank leaves the electrode area, it is immediately placed into a coolant containing a corrosion inhibitor for rapid cooling, followed by drying and winding.
[0012] In one specific embodiment, the components of the copper alloy wire rod, by weight percentage, include: Cr 0.1%~0.8%, Zr 0.05%~0.3%, The balance is Cu and unavoidable impurities.
[0013] In one specific embodiment, the cryogenic cooling medium is liquid nitrogen or a cryogenic ethanol circulating liquid with a temperature controlled at -196℃ to -150℃; the cryogenic freezing state refers to the temperature of the wire blank surface being maintained between -140℃ and -80℃. The total processing deformation of the continuous drawing is 60% to 95%, and the single-pass surface reduction rate is 15% to 25%.
[0014] In one specific embodiment, the functional aerosol precursor liquid is composed of an organic solvent, an active solute, and a viscosity modifier.
[0015] The organic solvent is a mixture of ethanol and isopropanol in a volume ratio of 1:1 to 3:1; the active solute is selected from at least one of titanium isopropoxide, magnesium ethoxide, or silver acetylacetonate, and its mass concentration in the organic solvent is 5wt% to 20wt%; the viscosity modifier is polyvinylpyrrolidone.
[0016] The thickness of the solid precursor ice film formed on the surface of the online billet is 2μm to 15μm.
[0017] In one specific embodiment, the frequency of the high-frequency pulsed current is 20kHz to 150kHz, the current density is 5×1035×103A / cm² to 5×1045×104A / cm², and the pulse width is 10μs to 100μs. The skin effect depth is controlled within the range of 0.05mm to 0.2mm on the surface of the billet.
[0018] In one specific implementation, a radial temperature gradient is established by controlling the pulse current parameters: the transient temperature of the wire blank surface reaches 650℃~850℃ and the duration is less than 50ms, so as to achieve surface solute diffusion. At the same time, the transient temperature of the core of the wire blank is maintained at 350℃~480℃ to achieve core precipitation strengthening.
[0019] In one specific embodiment, the coolant is an aqueous solution with a temperature of 20°C to 40°C and containing 0.1 wt% to 0.5 wt% benzotriazole, and the time interval between the wire blank leaving the electrode area and entering the coolant is controlled within 0.2 seconds.
[0020] This invention provides a copper alloy processing technology for anti-softening wiring harnesses in new energy vehicles. It has the following beneficial effects: 1. This invention directly couples the cryogenic drawing process with the low-temperature self-adsorption process of aerosols. It utilizes the low enthalpy carried by the wire blank itself after cryogenic drawing as an in-situ cold source to induce the functional aerosol precursor liquid to freeze transiently on the surface of the wire blank to form a uniform solid precursor ice film. This design does not require additional coating binder or external energy. It utilizes the residual energy of the previous process to complete the loading of surface modification materials, realizing a closed loop of energy flow between cold working and surface treatment processes.
[0021] 2. This invention applies a high-frequency pulsed current and utilizes its skin effect to establish a significant radial temperature and energy gradient on the cross-section of the wire blank. This allows the surface of the wire blank to instantly reach the high temperature required for vaporization precursors and solute diffusion, while the core remains in the medium-temperature aging range that promotes the precipitation of nanophases. This differentiated energy input method constructs a high-concentration solid solution reinforcement layer on the surface of the wire to improve its resistance to softening, while retaining the precipitated structure of the core to maintain high conductivity. This achieves gradient decoupling between the heat resistance and conductivity of the wire.
[0022] 3. This invention combines the electroplastic effect of pulsed current with chemical quenching process to complete the indentation and diffusion of surface solute atoms and the pinning of dislocation structures within milliseconds, and rapidly freezes the non-equilibrium microstructure. This process effectively suppresses excessive grain growth in conventional heat treatment and significantly increases the recrystallization temperature of the copper alloy wire surface, making it less prone to thermal relaxation or softening failure under the high-temperature conditions generated by high current transmission in new energy vehicles. Detailed Implementation Example
[0023] This embodiment provides a copper alloy processing technology for anti-softening wiring harnesses in new energy vehicles. The specific steps are as follows: S1. Select a Cu-Cr-Zr alloy wire rod with the following composition by weight percentage: Cr 0.45%, Zr 0.18%, and the balance Cu. Heat the wire rod to 950℃ and hold for 1.5 hours for solution treatment, then quench it in water, and finally pickle and dry the surface of the wire rod.
[0024] S2. Place the pretreated wire blank in a cryogenic ethanol circulating solution at a temperature of -170℃ for continuous drawing. Control the total processing deformation to 80% and the single-pass surface reduction rate to 20%. Control the drawing speed and cooling conditions so that the surface temperature of the wire blank after the last drawing pass is maintained at -110℃ when it enters the next process.
[0025] S3. Pass the wire blank, which is frozen at -110℃, through a mist chamber filled with functional aerosol precursor liquid. The formula of the functional aerosol precursor liquid is: the organic solvent is a mixture of ethanol and isopropanol in a volume ratio of 2:1; The active solute is magnesium ethoxide, with a mass concentration of 12 wt% in the organic solvent; the viscosity modifier polyvinylpyrrolidone is added at a rate of 1.2 wt%. The precursor liquid is frozen on the surface of the billet using a temperature difference to form a solid precursor ice film with a thickness of approximately 8 μm.
[0026] S4. The wire blank, with a solid precursor ice film on its surface, is passed through a rotating electrode area under tension, and a high-frequency pulsed current is applied. The pulsed current parameters are set as follows: frequency 85kHz, current density 2.5×10⁴A / cm², and pulse width 55μs. Under these parameters, the skin effect is used to raise the transient temperature of the wire blank surface to approximately 750℃, driving magnesium atoms to diffuse into the copper matrix; simultaneously, the transient temperature of the wire blank core is maintained at approximately 415℃ for aging treatment.
[0027] S5. After the wire blank leaves the electrode area, it is rapidly cooled in an aqueous solution containing 0.3 wt% benzotriazole at 30°C within 0.15 seconds, and then dried and wound up. Example
[0028] This embodiment provides a copper alloy processing technology for anti-softening wiring harnesses in new energy vehicles. The specific steps are as follows: S1. Select a Cu-Mg alloy wire rod with the following composition by weight percentage: Mg 0.1%, P 0.001%, and balance Cu. Heat the wire rod to 920℃ and hold for 1 hour for solution treatment, then quench it in water, and finally pickle and dry the surface of the wire rod.
[0029] S2. Place the pre-treated wire blank in a cryogenic cooling medium at a temperature of -150℃ for continuous drawing. Control the total processing deformation to 60% and the single-pass surface reduction rate to 15%. Control the drawing speed and cooling conditions so that the surface temperature of the wire blank after the last drawing pass is maintained at -80℃ when it enters the next process.
[0030] S3. The wire blank, frozen at -80℃, is passed through a mist chamber filled with a functional aerosol precursor solution. The formulation of the functional aerosol precursor solution is as follows: the organic solvent is a mixture of ethanol and isopropanol in a 1:1 volume ratio; the active solute is titanium isopropoxide, with a mass concentration of 5 wt% in the organic solvent; and the viscosity modifier, polyvinylpyrrolidone, is added at a rate of 0.5 wt%. The temperature difference causes the precursor solution to freeze on the surface of the wire blank, forming a solid precursor ice film with a thickness of approximately 2 μm.
[0031] S4. The wire blank, with a solid precursor ice film on its surface, is passed through the rotating electrode area under tension, and a high-frequency pulsed current is applied. The pulsed current parameters are set as follows: frequency 20kHz, current density 5×1035×103A / cm², and pulse width 10μs.
[0032] Under these parameters, the skin effect is used to bring the transient temperature of the wire blank surface to about 650°C, driving titanium atoms to diffuse into the copper matrix; at the same time, the transient temperature of the wire blank core is maintained at about 350°C for aging treatment.
[0033] S5. After the wire blank leaves the electrode area, it is rapidly cooled in an aqueous solution containing 0.1 wt% benzotriazole at 20°C within 0.2 seconds, and then dried and wound up. Example
[0034] This embodiment provides a copper alloy processing technology for anti-softening wiring harnesses in new energy vehicles. The specific steps are as follows: S1. Select a Cu-Cr-Zr alloy wire rod with the following composition by weight percentage: Cr 0.8%, Zr 0.3%, and the balance Cu. Heat the wire rod to 980℃ and hold for 2 hours for solution treatment, then quench it in water, and finally pickle and dry the surface of the wire rod.
[0035] S2. The pretreated wire blank is placed in liquid nitrogen at a temperature of -196℃ for continuous drawing. The total processing deformation is controlled at 95%, and the single-pass surface reduction rate is 25%. The drawing speed and cooling conditions are controlled so that the surface temperature of the wire blank after the last drawing pass is maintained at -140℃ when it enters the next process.
[0036] S3. Pass the wire blank, which is frozen at -140℃, through a mist chamber filled with functional aerosol precursor solution. The formula of the functional aerosol precursor solution is: the organic solvent is a mixture of ethanol and isopropanol in a volume ratio of 3:1; The active solute is silver acetylacetone, with a mass concentration of 20 wt% in the organic solvent; the viscosity modifier polyvinylpyrrolidone is added at a rate of 2.0 wt%. The precursor liquid is frozen on the surface of the billet using a temperature difference to form a solid precursor ice film with a thickness of approximately 15 μm.
[0037] S4. The wire blank, with a solid precursor ice film on its surface, is passed through a rotating electrode area under tension, and a high-frequency pulsed current is applied. The pulsed current parameters are set as follows: frequency 150kHz, current density 5×1045×104A / cm², and pulse width 100μs. Under these parameters, the skin effect is used to raise the transient temperature of the wire blank surface to approximately 850℃, driving silver atoms to diffuse into the copper substrate; simultaneously, the transient temperature of the wire blank core is maintained at approximately 480℃ for aging treatment.
[0038] S5. After the wire blank leaves the electrode area, it is rapidly cooled in an aqueous solution containing 0.5 wt% benzotriazole at 40°C within 0.1 seconds, and then dried and wound up.
[0039] Comparative Example 1: Compared with Example 1, the difference is that in S2, the drawing is performed in a room temperature lubricating fluid at 25°C instead of in a cryogenic ethanol circulating fluid at -170°C; since the wire blank does not have a cryogenic state, in S3, the wire blank cannot form a frozen solid precursor ice film on its surface when it passes through the fog chamber, and the other steps and parameters are the same.
[0040] Comparative Example 2: Compared with Example 1, the difference is that the pulsed current skin flash diffusion in S4 is replaced with traditional offline tube furnace heat treatment. Specifically, the wire blank coated with the precursor is placed in a tube furnace at 450°C and kept at that temperature for 30 minutes without applying pulsed current; the remaining steps and parameters are the same.
[0041] Comparative Example 3: Compared with Example 2, the difference is that the low-temperature self-adsorption of aerosol in S3 is cancelled, and the wire blank directly enters S4 for pulse current treatment after deep cryogenic drawing in S2; the remaining steps and parameters are the same.
[0042] Comparative Example 4: Compared with Example 3, the difference is that the current applied in S4 is replaced by a direct current instead of a high-frequency pulse current with a frequency of 150kHz, while the current density remains the same. Since direct current has no skin effect, the current is uniformly distributed across the cross-section of the blank, making it impossible to form a temperature gradient with a high surface temperature and a low core temperature; the remaining steps and parameters are the same.
[0043] Test Example 1: Resistance to Softening Test This test example is used to determine the softening temperature of the copper alloy wires prepared in Examples 1-3 and Comparative Examples 1-4, in order to evaluate their microstructure stability under high temperature conditions.
[0044] Experimental steps Sample preparation: Several samples with a length of 200 mm were cut from the finished wire products prepared in Examples 1-3 and Comparative Examples 1-4.
[0045] Initial performance determination: Three specimens were randomly selected from each group and subjected to tensile testing using an electronic universal testing machine at room temperature (25℃). The average tensile strength was recorded as the initial tensile strength. .
[0046] High-temperature annealing: The remaining samples from each group were divided into smaller groups and placed in resistance heating furnaces for isochoric annealing. The annealing temperature range was set to 300℃ to 650℃, with temperature intervals of 50℃. The samples were held at the set temperature for 1 hour, and then removed and allowed to cool naturally to room temperature in still air.
[0047] Residual strength determination: Tensile tests were performed on the specimens after annealing at different temperatures, and the tensile strength at each annealing temperature was recorded. .
[0048] Data processing: Calculating the percentage of residual strength According to the GB / T351-2019 standard, the temperature at which the residual strength decreases to 80% of the original tensile strength is calculated by linear interpolation and defined as the softening temperature.
[0049] The experimental data are shown in Table 1. The softening temperature test results for each group of samples are shown in Table 1.
[0050] Table 1. Test data on softening temperature of copper alloy wire Group Alloy system Key process characteristics differences Original tensile strength (MPa) Softening temperature (°C) Example 1 Cu-Cr-Zr intermediate parameter combination 542 538 Example 2 Cu-Mg Lower limit parameter combination 487 465 Example 3 Cu-Cr-Zr High limit parameter combination 589 572 Comparative Example 1 Cu-Cr-Zr Room temperature pull-out (without a cooling source) 465 423 Comparative Example 2 Cu-Cr-Zr In-furnace heat treatment (without pulse) 452 458 Comparative Example 3 Cu-Mg No aerosol adsorption 478 392 Comparative Example 4 Cu-Cr-Zr Direct current (without skin effect) 496 431 Table 1 shows that the softening temperatures of the wires prepared in Examples 1-3 are significantly higher than those of the comparative examples. The softening temperatures of the Cu-Cr-Zr alloy wires in Examples 1 and 3 reached 538℃ and 572℃, respectively, while the softening temperature of Comparative Example 1, which used the same alloy system but did not establish a cryogenic state during the drawing process and did not undergo precursor adsorption, was only 423℃.
[0051] This difference indicates that the combination of cryogenic drawing and the low-temperature self-adsorption step of aerosols enables the active solute to successfully adhere to and penetrate into the wire surface. The cryogenic state provides thermodynamic conditions for the in-situ film formation of the precursor, and the subsequent diffusion process forms a high-concentration solid solution reinforcement zone on the surface. The solute atoms in this region pin the grain boundaries and dislocations, hindering grain growth and recovery processes at high temperatures, thereby improving the overall thermal stability of the material.
[0052] Compared to Comparative Example 2, which uses conventional tube furnace heat treatment, and Comparative Example 4, which uses direct current treatment, the examples show advantages in resistance to softening. Comparative Example 2, due to overall heating, cannot form a temperature gradient between the surface and the core, resulting in a uniform coarsening rate of the precipitated phase. Although Comparative Example 4 used electric current heating, the direct current was uniformly distributed across the cross-section and lacked the high surface energy density caused by the skin effect, making it impossible to drive the vaporization, decomposition, and deep diffusion of the surface precursor in a very short time.
[0053] This invention utilizes the skin effect of high-frequency pulsed current to establish a temperature gradient across the wire cross-section, with a higher temperature on the outside and a lower temperature on the inside. This causes a vigorous solute diffusion reaction on the surface layer, while the core remains within a suitable precipitation aging temperature range. This gradient heat treatment mode significantly enhances the surface layer's resistance to thermal creep while ensuring that the core does not undergo aging.
[0054] Comparing Example 2 and Comparative Example 3, although Comparative Example 3 underwent cryogenic drawing and pulsed current treatment, it lacked the adsorption step of the functional aerosol precursor liquid, and its softening temperature was 392°C, lower than 465°C in Example 2. This indicates that while simple physical field treatment can bring about a certain strengthening effect, the introduction of external microalloying elements is necessary for constructing a heat-resistant surface layer. The active solutes in the aerosol penetrate into the copper matrix under high-energy pulse driving, and the resulting solid solution or fine compounds inhibit the slip and climb of the surface lattice, constituting a physical barrier against softening.
[0055] Test Example 2: Conductivity Test This test example is used to determine the conductivity of the copper alloy wires prepared in Examples 1-3 and Comparative Examples 1-4, in order to evaluate the effect of gradient heat treatment in the process on the electron transport performance of the matrix, and in particular to verify the precipitation state of the core structure.
[0056] Experimental steps Sample cutting: Cut straight samples with a length of 1200 mm from the copper alloy wires prepared in each group.
[0057] Environmental equilibration: The cut sample was placed in a constant temperature laboratory and left to stand for 4 hours. The ambient temperature was controlled at 20℃±0.5℃ and the relative humidity was 45%~55% to eliminate the influence of temperature fluctuation on resistance measurement.
[0058] Surface pretreatment: Wipe the sample surface with anhydrous ethanol to remove oil and impurities. For the areas at both ends used to connect the electrodes, lightly sand with 1000-grit sandpaper to remove the oxide film and ensure good contact. The sanding length is limited to the electrode clamping area.
[0059] Resistance measurement: A QJ57 DC double-arm bridge was used for measurement. The sample was connected to the test circuit, and the gauge length was set to 1000 mm. After applying the test current, the resistance value R20 between the voltage terminals was recorded. Each sample was measured three times, and the arithmetic mean was taken.
[0060] Data calculation: Based on the measured resistance value, the actual length of the sample and the cross-sectional area, the volume resistivity is calculated and converted into the percentage of conductivity of international annealed copper standard.
[0061] The experimental data are shown in Table 2. The conductivity test results of each group of samples are shown in Table 2.
[0062] Table 2. Test data on conductivity of copper alloy wires Group Key process differences Conductivity (%IACS) Example 1 Intermediate parameter combination (Cu-Cr-Zr) 83.4 Example 2 Lower limit parameter combination (Cu-Mg) 76.2 Example 3 High limit parameter combination (Cu-Cr-Zr) 81.9 Comparative Example 1 Room temperature drawing 72.5 Comparative Example 2 In-furnace heat treatment 78.1 Comparative Example 3 No aerosol adsorption (Cu-Mg) 79.8 Comparative Example 4 DC current processing 68.4 Table 2 reveals the influence of different energy input methods on the final conductivity of copper alloy wires. The Cu-Cr-Zr alloy wires of Examples 1 and 3 achieved conductivity of 83.4% IACS and 81.9% IACS, respectively, indicating that sufficient aging precipitation reaction occurred within the material. In the pulsed current skin flash diffusion step, the Joule heating generated by the current coupled with the electroplastic effect, promoting the precipitation of supersaturated solid solution atoms in the core and reducing lattice distortion and electron scattering center density in the copper matrix. Although additional alloying elements were introduced into the surface layer, the skin effect confined the high-temperature region to an extremely thin surface layer, and the core of the large cross-section wire remained in the intermediate-temperature range that promoted precipitation, thus maintaining a high level of conductivity macroscopically.
[0063] Comparing Example 1 and Comparative Example 4, it can be observed that the conductivity of the sample treated with DC current is significantly reduced. This is because DC current generates uniform Joule heating across the wire cross-section, eliminating the radial temperature gradient. To achieve the same surface diffusion effect as in the examples, the overall current density must be increased, leading to excessively high core temperatures. These excessively high core temperatures cause the precipitated phases to dissolve back or become coarser, resulting in solute atoms re-dissolving in the matrix, significantly enhancing electron scattering and thus drastically reducing overall conductivity. This result conversely confirms the effectiveness of this invention in constructing a high-temperature diffusion surface and a mid-temperature precipitation core temperature field using the skin effect.
[0064] Furthermore, comparing the data from Example 2 and Comparative Example 3 reveals that, under the same Cu-Mg system, Comparative Example 3, which did not undergo aerosol adsorption, exhibits slightly higher conductivity. This difference stems from the introduction of trace amounts of heterojunction elements into the surface layer of the wire in Example 2. The diffusion of these elements into the surface lattice causes localized lattice distortion, resulting in a slight decrease in conductivity in the surface region. However, considering the softening temperature data from Test Example 1, while Comparative Example 3 shows slightly higher conductivity, its softening resistance is significantly compromised. Example 2, by sacrificing a minimal proportion of overall conductivity, achieves a significant improvement in surface thermal stability, thus realizing a comprehensive balance between softening resistance and conductivity within the gradient structure.
[0065] Test Example 3: Surface Microhardness Test This test example is used to determine the microhardness of different regions of the cross-section of the copper alloy wires prepared in Examples 1-3 and Comparative Examples 1-4, in order to verify whether a gradient structure of composition and properties was successfully constructed in the radial direction of the wire during the process.
[0066] Experimental steps Metallographic specimen preparation: Short samples with a length of 10 mm were cut from each group of wires. The specimens were placed vertically in the center of the metallographic mounting mold, and epoxy resin cold mounting material was injected. The mold was then cured at room temperature to obtain a metallographic specimen block containing the cross-section of the wire.
[0067] Grinding and polishing: The mounted specimens were ground stepwise using wet sandpaper with grits of 400, 800, 1200, and 2000 grits respectively. Subsequently, the specimens were mechanically polished using diamond polishing paste with grits of 1.0 μm and 0.5 μm until the cross-section of the wire showed no obvious scratches and a mirror-like finish under a metallographic microscope.
[0068] Test point positioning: Place the prepared sample on the stage of the microhardness tester. Observe through the microscope eyepiece and select two characteristic test areas on the wire cross-section: the first area is located within an annular band 10μm±2μm from the outer surface of the wire; the second area is located within a radius of 0.5mm from the geometric center of the wire cross-section.
[0069] Hardness indentation test: A Vickers hardness indenter was used, with a test force of 0.49 N and a holding time of 10 seconds. Five indentation tests were performed on the surface and core areas of each sample. The center-to-center distance between adjacent indentations was greater than three times the diagonal length of the indentation to avoid interference from work hardening.
[0070] Data Acquisition: The diagonal length of the indentation is measured, and the system automatically calculates the Vickers hardness value. The arithmetic mean of the test values at 5 points in each area is taken as the final hardness data for that area.
[0071] The experimental data are shown in Table 3. The microhardness test results of the surface and core of each group of samples are shown in Table 3.
[0072] Table 3. Test data of gradient hardness of copper alloy wire cross section. Group Process characteristics Surface hardness (HV 0.05) Core hardness (HV0.05) Hardness difference (surface to core) Example 1 intermediate parameter combination 186.4 158.2 28.2 Example 2 Lower limit parameter combination 165.7 141.5 24.2 Example 3 High limit parameter combination 192.1 163.8 28.3 Comparative Example 1 No cold source / no adsorption 145.3 148.6 -3.3 Comparative Example 2 In-furnace heat treatment 118.5 116.9 1.6 Comparative Example 3 No adsorption (Cu-Mg) 134.2 140.8 -6.6 Comparative Example 4 DC current processing 131.4 129.7 1.7 The test data in Table 3 show that the wires prepared in Examples 1-3 exhibit a significant gradient of hardness on the outside and toughness on the inside in the radial direction. Taking Example 1 as an example, its surface hardness reaches 186.4 HV0.05, which is 28.2 units higher than the core hardness of 158.2 HV0.05. The formation of this hardness gradient is attributed to the synergistic effect of the skin effect induced by high-frequency pulsed current and the diffusion of surface precursors. The high-frequency current concentrates Joule heat highly on the surface of the wire, driving the adsorbed active solute atoms to rapidly penetrate into the copper matrix, resulting in strong solid solution strengthening and lattice distortion, thereby significantly improving the surface hardness. In contrast, the core, due to its lower current density and temperature maintained within a suitable aging range, mainly undergoes precipitation strengthening. Although its hardness value is lower than that of the surface, it is still higher than that of the fully annealed state, ensuring the baseline level of overall strength.
[0073] In contrast, the surface and core hardness values of Comparative Examples 2 and 4 were essentially the same, with a hardness difference of only 1.6–1.7 HV0.05, which is a uniform distribution within the measurement error range. Comparative Example 2, due to its use of an external heat source for overall heating, experienced uniform heating throughout the wire, leading to overall grain recovery and recrystallization, resulting in a significant decrease in overall hardness to approximately 118.5 HV. Although Comparative Example 4 used electric heating, the lack of skin effect from direct current meant that the current flowed across the entire cross-section, failing to establish a radial temperature gradient. This prevented the formation of a special reinforcing structure on the surface distinct from the core, confirming that utilizing the skin properties of high-frequency pulsed current is a key energy method for constructing a gradient hardness distribution.
[0074] Furthermore, comparing the data from Example 2 and Comparative Example 3, it can be seen that, despite both being Cu-Mg alloys and undergoing electrical pulse treatment, the surface hardness of Comparative Example 3, which did not undergo aerosol adsorption, was slightly lower than the core hardness. This is because, in the absence of external alloying elements, the skin effect causes the surface temperature to be higher than the core, resulting in a greater degree of recovery or partial recrystallization softening of the surface. In contrast, Example 2 introduced a surface alloying source through a low-temperature adsorption step following cryogenic drawing. The solute diffusion effect at high temperatures offset and surpassed the thermal softening effect, achieving surface hardening through changes in chemical composition. This comparison confirms the fundamental role of the low-temperature self-adsorption step of aerosols in achieving surface strengthening.
Claims
1. A copper alloy processing technology for anti-softening wiring harnesses in new energy vehicles, characterized in that, Includes the following steps: S1: Select copper alloy wire blanks, perform high-temperature solution treatment and quenching, and clean and dry the surface of the wire blanks. S2: The wire blank treated in S1 is placed in a cryogenic cooling medium for continuous drawing, so that lattice distortion energy is accumulated inside the wire blank, and the wire blank after drawing is kept in a low-temperature frozen state when it enters the next process. S3: The low-temperature frozen wire blank obtained in S2 is passed through a mist chamber filled with functional aerosol precursor liquid. The functional aerosol precursor liquid is frozen in situ on the surface of the wire blank by utilizing the coldness carried by the wire blank itself and the temperature difference between the mist chamber environment, forming a solid precursor ice film. S4: The wire blank with a solid precursor ice film on its surface is passed through the electrode area under tension and a high-frequency pulsed current is applied. The skin effect generated by the high-frequency current is used to instantly raise the surface temperature of the wire blank to vaporize and decompose the solid precursor ice film and drive the active solute to diffuse to the surface of the copper alloy substrate. At the same time, the thermal effect and electroplastic effect of the current are used to age the core of the wire blank. S5: After the wire blank leaves the electrode area of S4, it is immediately placed into a cooling liquid containing corrosion inhibitor for rapid cooling, and then dried and wound up.
2. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The composition of the copper alloy wire rod described in S1, by weight percentage, is as follows: Cr0.1%~0.8%, Zr0.05%~0.3%, The balance is Cu and unavoidable impurities; The high-temperature solution treatment temperature is 920℃~980℃.
3. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The cryogenic cooling medium mentioned in S2 is liquid nitrogen or cryogenic ethanol circulating liquid with a temperature of -196℃ to -150℃; The low-temperature freezing state refers to the temperature of the wire blank surface being maintained between -140℃ and -80℃.
4. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The total processing deformation of the continuous drawing described in S2 is 60% to 95%, and the single-pass surface reduction rate is 15% to 25%.
5. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The functional aerosol precursor liquid described in S3 includes an organic solvent, an active solute, and a viscosity modifier; The organic solvent is composed of ethanol and isopropanol in a volume ratio of 1:1 to 3:1, the active solute is selected from at least one of titanium isopropoxide, magnesium ethoxide or silver acetylacetonate, and the viscosity modifier is polyvinylpyrrolidone.
6. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The active solute in S3 has a mass concentration of 5wt% to 20wt% in the organic solvent, and the thickness of the solid precursor ice film is 2μm to 15μm.
7. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The high-frequency pulse current described in S4 has a frequency of 20kHz to 150kHz, a current density of 5×1035×103A / cm² to 5×1045×104A / cm², and a pulse width of 10μs to 100μs.
8. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The heat generated by the skin effect described in S4 causes the transient temperature of the wire blank surface to reach 650℃~850℃, and the duration is less than 50ms. The transient temperature of the core of the wire blank during aging treatment is maintained between 350°C and 480°C.
9. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The skin effect described in S4 is controlled within the range of 0.05 mm to 0.2 mm on the surface of the billet; The electrode area employs a rotating liquid metal contact electrode or a graphite roller electrode.
10. The copper alloy processing technology for anti-softening new energy vehicle wiring harnesses according to claim 1, characterized in that, The coolant mentioned in S5 is an aqueous solution with a temperature of 20℃~40℃ and containing 0.1wt%~0.5wt% benzotriazole. The time interval between the wire blank leaving the electrode area and entering the coolant is controlled within 0.2 seconds.