Chip flip packaging method

By setting solder pillars and high-melting-point solder connections in the flip-chip packaging, combined with curing agent and polishing technology, the problems of lead span and packaging medium inflow are solved, realizing a highly efficient and simplified flip-chip packaging process, improving product quality and production efficiency.

CN121487621BActive Publication Date: 2026-06-23ZHONGKE HUAYI (TIANJIN) TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610018388.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-01-08
Publication Date
2026-06-23
Estimated Expiration
2046-01-08

AI Technical Summary

Technical Problem

In the current chip flip packaging process, the long span or intersection of leads leads reduce product yield and reliability. The packaging medium cannot directly enter between the frame and the chip, which increases the process flow and cost.

Method used

A solder post is placed at the solder window of the chip, and a potting gap is maintained between the end face of the solder post and the chip surface to allow the encapsulation medium to flow directly in. High melting point solder is used to connect the solder post to the frame or substrate. The solder post is wrapped with a curing agent and ground to make the surface consistent, avoiding multiple filling processes and simplifying the production steps.

Benefits of technology

It improves packaging consistency and product quality, reduces production steps, increases production efficiency and product quality, and avoids internal stress and poor connection problems caused by multiple fillings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121487621B_ABST
    Figure CN121487621B_ABST
Patent Text Reader

Abstract

This invention provides a chip flip-chip packaging method. A first solder is applied to the solder windows of a chip formed on a wafer, fixing the first end of a solder post to the solder window. A curing agent is filled between the solder posts. The solder posts are then ground so that their second ends are on the same plane, and a solderable layer is formed on the end face of the solder posts before the curing agent is removed. The second end of the solder post is fixed to a frame or substrate coated with a second solder, forming a potting gap between the second end of the solder post and the chip. Epoxy resin is then filled into the potting gap and encapsulates the chip. The melting point of the first solder is higher than that of the second solder. This invention uses solder posts on the chip solder window to create a potting gap between the chip and the frame or substrate. During a single epoxy resin filling, the epoxy resin flows directly into the potting gap and encapsulates the chip. Compared to processes requiring bottom filling with adhesive, this reduces the number of filling operations, lowers internal stress caused by varying degrees of curing of the adhesive with different filling operations, thereby simplifying production steps and improving production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chip packaging technology, and in particular relates to a chip flip-chip packaging method. Background Technology

[0002] In the process of chip integrated circuit packaging, the chip is usually fixed on the base island of the frame. Then, the solder windows of the chip are connected to the corresponding pins through leads to realize the electrical connection between the chip and the outside world. After that, epoxy is filled to combine the frame, leads and chip into a whole to complete the chip packaging production. However, in this method, some leads have long spans or crosses. The leads may also shift during the epoxy filling process, resulting in interconnection between leads, which leads to a decrease in product yield and reliability.

[0003] However, existing flip-chip technology has significant limitations. Furthermore, during the packaging process, the packaging medium cannot directly enter between the frame and the chip, requiring secondary potting, which increases the flip-chip packaging process, resulting in lower production efficiency and increased costs. Summary of the Invention

[0004] In view of this, the present invention aims to propose a chip flip-chip packaging method to simplify the chip flip-chip process and improve production efficiency.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented as follows:

[0006] A chip flip-chip packaging method, including

[0007] S1: Apply a first solder to the solder window of the chip formed on the wafer, and place one end of the solder pillar on the solder window coated with the first solder, so that the solder pillar is welded and fixed to the solder window;

[0008] S2: Fill the upper surface of the chip with curing agent, using the curing agent to fill the gaps between the solder pillars, and wait for the curing agent to solidify; there is a gap between the surface of the curing agent and the upper surface of the chip.

[0009] S3: Polish the surfaces of the curing agent and the solder pillars so that the surface of the curing agent and the end of the solder pillar furthest from the chip are on the same plane;

[0010] S4: Remove the curing agent to create a potting gap between the plane of the end of the solder pillar away from the chip and the upper surface of the chip;

[0011] S5: Fix the end of the solder pillar away from the chip to a preset position on the frame or substrate coated with the second solder;

[0012] S6: Fill with epoxy resin so that the gaps in the potting can be filled with epoxy resin, and the epoxy resin encapsulates the chip and solder post, and then the epoxy resin is cured.

[0013] The melting point of the first solder is higher than that of the second solder.

[0014] Furthermore, S3 includes

[0015] S31: Create a weldable layer on the end face of the ground weld post.

[0016] Furthermore, the first solder is a tin-lead-silver-copper solder.

[0017] Furthermore, the second solder is a tin-silver-bismuth solder.

[0018] Furthermore, the width of the potting gap between the end of the welding post furthest from the welding window and the upper surface of the chip is 1-1.5mm.

[0019] Furthermore, this encapsulation method also includes

[0020] S7: Perform electroplating or ball placement at a predetermined position on the frame or substrate.

[0021] Furthermore, the melting point of the first solder material is 10-50°C higher than that of the second solder.

[0022] Furthermore, the melting point temperature of the first solder is higher than the welding temperature of the second solder.

[0023] Furthermore, S8: The wafer is cut according to the preset position to form multiple fully packaged chip packages.

[0024] Furthermore, steps S1 and S5 also include...

[0025] S11: Clean off excess first solder;

[0026] S51: Clean up excess second solder.

[0027] Furthermore, step S5 also includes

[0028] S51: Eliminate stress on the wafer before fixing the frame or substrate to the chip.

[0029] Compared with existing technologies, the chip flip-chip packaging method described in this invention has the following advantages:

[0030] This invention employs a method of setting solder pillars on the solder window of the chip and leaving a potting gap between the end face of the solder pillar and the chip surface, so that a gap is formed between the frame or substrate and the chip, allowing the encapsulation medium to flow directly into the potting gap. In a single process of filling the encapsulation medium, the encapsulation medium can encapsulate the chip, avoiding the internal stress caused by different curing degrees of the encapsulation medium due to multiple filling processes, improving encapsulation consistency, and reducing the number of times the encapsulation medium is filled, thereby simplifying the production steps and improving production efficiency.

[0031] By using a method where the melting point temperature of the first solder is higher than that of the second solder, the solder joints of the first solder that have already been connected are avoided during the connection process between the solder post and the frame or substrate. This prevents the solder post from detaching from the chip solder window and improves product quality.

[0032] The solder pillars are coated with a curing agent and then ground to make the distance between the end face of the solder pillar and the chip surface consistent, so as to avoid the external force during the grinding process from affecting the connection strength between the solder pillar and the chip and to prevent the solder pillar from desoldering from the solder window;

[0033] After the solder pillars are coated with a curing agent, a solderable layer is electroplated or deposited on the end face of the solder pillars to prevent the solderable layer from appearing on the side of the solder pillars, which would reduce the gap between the solder pillars and cause accidental electrical connection between the solder windows of the chip. Attached Figure Description

[0034] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0035] Figure 1 This is a schematic diagram of the process flow for this packaging method;

[0036] Figure 2 This is a schematic diagram of the process flow for grinding welded columns.

[0037] Explanation of reference numerals in the attached figures:

[0038] 1-Chip; 11-Solder window; 2-Solder post; 21-Solderable layer; 3-Curing agent; 4-Pouring gap; 5-Frame or substrate; 6-Encapsulation medium. Detailed Implementation

[0039] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.

[0040] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0041] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art will understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0042] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0043] Combination Figures 1-2 The flip-chip packaging method of the present invention includes:

[0044] S1: A first solder is applied to the solder window 11 of the chip 1 formed on the wafer, and one end of the solder post 2 is placed on the solder window 11 coated with the first solder, so that the solder post 2 is soldered and fixed to the solder window 11; for example, the first solder is tin-lead-silver-copper solder, the chip 1 is processed on the wafer, the tin-lead-silver-copper solder is applied to the solder window 11 of the chip 1, the solder post 2 made of conductive material is placed on the solder window 11, and the solder post 2 is fixedly connected to the solder window 11 by reflow soldering.

[0045] S11: Clean the wafer with solder pillars 2. After the solder pillars 2 and chip 1 are soldered, remove the excess first solder.

[0046] S2: Fill the upper surface of chip 1 with curing agent 3 and wait for the curing agent 3 to solidify; the surface of the curing agent 3 is flush with or higher than the end face of the solder post 2, and there is a gap between the surface of the curing agent 3 and the surface of chip 1, and the gap is greater than 1.5mm; thereby, the curing agent 3 enables the solder post 2 and the wafer to be connected to form a whole.

[0047] S3: Grind the surfaces of the curing agent and the solder pillar so that the surface of the curing agent and the end of the solder pillar furthest from the chip are on the same plane. This exposes the end face of the solder pillar 2 outside the curing agent 3, facilitating the subsequent connection of the solder pillar 2 to the frame or substrate 5 and the fabrication of the solder layer on the solder pillar 2. In this embodiment, the surfaces of the curing agent and the solder pillar are ground using a grinding machine. The curing agent reinforces the solder pillar, preventing the solder pillar 2 from being subjected to excessive external force when grinding the end of the solder pillar 2 furthest from the chip 1, which could cause the solder pillar 2 to detach or even fly off, affecting subsequent processing and product reliability. After grinding, in this application, a distance of 1-1.5 mm is maintained between the plane containing the end face of the solder pillar 2 and the upper surface of the chip 1.

[0048] S31: A solderable layer 21 is formed on the end face of the ground weld post 2. For example, the solderable layer 21 is formed on the surface of the ground weld post 2 by electroplating or metal deposition. The metal of the solderable layer 21 can be a conductive metal such as silver.

[0049] S4: Remove the curing agent 3. For example, the curing agent 3 can be softened and dissolved by other chemical methods such as alcohol or acetone solution, or the curing agent 3 around the solder post 2 can be separated and cut off by a grinding device or other physical methods, so that the curing agent 3 in the potting gap 4 is separated from the chip 1. Since there is a gap of 1-1.5mm between the plane where the end face of the solder post 2 is located and the upper surface of the chip 1 during the grinding process, a potting gap 4 can be formed between the end face of the solder post and the chip after the curing agent is removed.

[0050] S5: Fix the end of the solder post 2 away from the chip 1 to a preset position on the frame or substrate 5 coated with the second solder, and fix the frame or substrate 5 to the solder post 2 with the second solder, so that the chip 1 is fixedly connected to the frame or substrate 5; for example, the second solder is tin-silver-bismuth solder. In this embodiment, the first solder tin-silver-copper solder has a melting temperature of 227°C at 255°C-265°C, and the second solder tin-silver-bismuth solder has a welding temperature of 180°C and a melting temperature of 138°C-141°C. By using the method that the welding temperature of the second solder is higher than the melting temperature of the first solder, the solder joint between the solder post 2 and the solder window 11 of the chip 1 is avoided from being affected during the welding process of the solder post 2 and the frame or substrate 5, so as to prevent the solder post 2 and the solder window 11 from desoldering or having poor contact, which would affect the product quality.

[0051] S51: Before fixing the frame or substrate to the chip, eliminate the stress on the wafer. In this embodiment, the stress generated in the wafer during the preceding process is eliminated by a wafer stress detection device and a stress elimination device (such as a wafer thinning machine). Those skilled in the art should know that the internal stress of the wafer can also be eliminated by heat treatment, slitting, etc. The stress elimination methods are existing technologies and will not be described in detail here.

[0052] S52: Clean up excess second solder after welding.

[0053] S6: Fill the encapsulation medium 6 so that the potting gap is filled with the encapsulation medium 6, and the encapsulation medium 6 encapsulates the chip 1 and the solder post 2, and then allow the encapsulation medium 6 to cure; by using a potting gap 4 of 1-1.5mm between the plane where the end face of the solder post 2 is located and the surface of the chip 1, the encapsulation medium 6 can enter between the frame and the chip 1 through the potting gap 4 in one potting process, without the need for secondary or even multiple potting processes. Compared with secondary or multiple potting processes, this improves the overall consistency of the encapsulated product, avoids the problem of poor bonding between encapsulation media 6 due to inconsistent potting times in secondary or multiple potting processes, reduces the number of process steps in product manufacturing, improves product processing efficiency, and makes the encapsulation medium bond more tightly to the chip, preventing the encapsulation medium from loosening.

[0054] S7: Electroplating or ball placement is performed at a preset position on the frame or substrate 5 to facilitate soldering of the product to the circuit board.

[0055] S8: Cut the wafer into multiple packaged chip 1 packages according to the preset positions.

[0056] After chip 1 is packaged, the chip 1 package is cleaned and baked to keep the surface of the package clean and free of contamination. Good product testing is then conducted, and the good products are printed with codes and put into storage.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A chip flip-chip packaging method, characterized in that: include S1: Apply a first solder to the solder window of the chip formed on the wafer, and place one end of the solder pillar on the solder window coated with the first solder, so that the solder pillar is welded and fixed to the solder window; S2: Fill the upper surface of the chip with curing agent, using the curing agent to fill the gaps between the solder pillars, and wait for the curing agent to solidify; there is a gap between the surface of the curing agent and the upper surface of the chip. S3: Polish the surfaces of the curing agent and the solder pillars so that the surface of the curing agent and the end of the solder pillar furthest from the chip are on the same plane; S4: Remove the curing agent to form a potting gap between the plane of the end of the solder post away from the chip and the upper surface of the chip. The width of the potting gap between the end of the solder post away from the solder window and the upper surface of the chip is 1-1.5mm. S5: Fix the end of the solder post away from the chip to a preset position on the frame or substrate coated with the second solder; S6: Fill with epoxy resin so that the gaps in the potting can be filled with epoxy resin, and the epoxy resin encapsulates the chip and solder post, and then the epoxy resin is cured. S7: Perform electroplating or ball placement at a predetermined position on the frame or substrate; S8: Cut the wafer into multiple fully packaged chip packages according to the preset positions; The melting point of the first solder is higher than that of the second solder.

2. The chip flip-chip packaging method according to claim 1, characterized in that: The S3 includes S31: Create a weldable layer on the end face of the ground weld post.

3. The chip flip-chip packaging method according to claim 1, characterized in that: The first solder is a tin-lead-silver-copper solder.

4. The chip flip-chip packaging method according to claim 1, characterized in that: The second solder is tin-silver-bismuth solder.

5. A chip flip-chip packaging method according to claim 1, characterized in that: The melting point of the first solder material is 10-50°C higher than that of the second solder material.

6. The chip flip-chip packaging method according to claim 1, characterized in that: The melting point of the first solder is higher than the welding temperature of the second solder.

7. A chip flip-chip packaging method according to claim 1, characterized in that: Step S5 also includes S51: Eliminate stress on the wafer before fixing the frame or substrate to the chip.

Citation Information

Patent Citations

  • Non-destructive grinding method and device for welding column of CCGA device

    CN113421830A

  • Chip packaging structure and chip packaging module

    CN223501869U