Ferritic stainless steel thin-walled spiral welded pipe and method of manufacturing the same

By employing a double-sided, double-process welding method and an arc-shaped reinforcing rib design, the welding heat input is controlled, solving the problems of grain growth and performance degradation in thin-walled spiral welded pipes of ferritic stainless steel. This enables stable production of spiral welded pipes with large diameter-to-wall ratio and high-performance welded joints.

CN121624596BActive Publication Date: 2026-11-20SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610022410.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-01-08
Publication Date
2026-11-20
Estimated Expiration
2046-01-08

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively control welding heat input, suppress ferritic stainless steel grain growth, and balance weld formation quality with joint performance. This is especially true in the manufacture of thin-walled, large-diameter spiral welded pipes, resulting in high material costs, increased weight, and decreased performance.

Method used

A double-sided, dual-process welding method is adopted, with TIG self-fusion welding on the front and MIG welding on the back. Combined with the design of arc-shaped reinforcing ribs, the welding heat input parameters are strictly controlled to ensure grain control of the weld and heat-affected zone.

Benefits of technology

Stable production of large-diameter spiral welded pipes with high wall-to-diameter ratio has been achieved, reducing material costs, improving deformation resistance and overall rigidity, ensuring good mechanical properties and corrosion resistance of welded joints, simplifying the process, and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121624596B_ABST
    Figure CN121624596B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of stainless steel welding technology, and relates to a thin-walled spiral welded pipe of ferritic stainless steel and its manufacturing method. The manufacturing method of the thin-walled spiral welded pipe of ferritic stainless steel of this invention includes the following steps: welding arc-shaped reinforcing ribs along the length of the ferritic stainless steel strip in the middle; feeding the steel strip with the reinforcing ribs into a spiral welded pipe forming device, and performing double-sided welding during the spiral forming process to obtain the thin-walled spiral welded pipe of ferritic stainless steel. The front weld facing the outer side of the steel strip is welded using TIG self-fusion welding, and the back weld facing the inner side of the steel strip is welded using MIG welding. The manufacturing method of the thin-walled spiral welded pipe of ferritic stainless steel of this invention, by using economical ferritic stainless steel instead of expensive austenitic stainless steel to manufacture thin-walled spiral welded pipes, significantly reduces raw material costs and enhances the product's market competitiveness while maintaining good corrosion resistance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of stainless steel welding and processing technology, and specifically relates to a ferritic stainless steel thin-walled spiral welded pipe and its manufacturing method. Background Technology

[0002] Spiral welded pipe is a type of welded steel pipe widely used in pipelines, pipe piles, and mechanical structures. Its manufacturing process uses strip steel coils as raw materials, which are spirally formed and then automatically welded on one or both sides. Currently, most spiral welded pipes both domestically and internationally are made of austenitic stainless steel, such as SUS304 and 316. Although austenitic stainless steel has mature welding technology and excellent overall performance, its material cost is high, and it has a large coefficient of thermal expansion and poor thermal conductivity, making it prone to significant welding stress and deformation at high temperatures.

[0003] On the other hand, ferritic stainless steels such as SUS409L, 439, and 441 have potential applications in thin-walled structures due to their high chromium content, good corrosion resistance, low coefficient of thermal expansion, and relatively low cost. However, ferritic stainless steels exhibit a significant tendency for grain growth during welding, especially in the heat-affected zone (HAZ), which can lead to a decrease in joint plasticity and toughness, limiting their widespread application in welded structures. Currently, there are no mature processes or publicly reported methods for manufacturing thin-walled, large-diameter spiral welded pipes using ferritic stainless steel. The main product form of ferritic stainless steel welded pipes is thin-walled straight seam welded pipes, and the welding methods used include TIG, plasma welding, and high-frequency induction welding.

[0004] In existing technologies, the manufacture of large-diameter spiral welded pipes typically involves increasing wall thickness or using austenitic stainless steel to ensure structural rigidity. However, this leads to increased material costs and weight, and fails to fully leverage the corrosion resistance and economic advantages of ferritic stainless steel. Furthermore, existing welding processes often employ single welding methods, making it difficult to simultaneously address weld formation quality and joint performance. This is particularly true for welding thin-walled ferritic stainless steel, where a lack of systematic and suitable process parameters and structural strengthening methods is present.

[0005] Therefore, how to provide a manufacturing method for thin-walled spiral welded pipes of ferritic stainless steel that can effectively control welding heat input, suppress grain growth, and ensure the mechanical properties of the welded pipe has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a ferritic stainless steel thin-walled spiral welded pipe and its manufacturing method.

[0007] Specifically, the manufacturing method of the ferritic stainless steel thin-walled spiral welded pipe of the present invention includes the following steps: (1) Weld a reinforcing rib with an arc-shaped edge along the length of the ferritic stainless steel strip in the middle part of the strip; (2) The steel strip with reinforcing ribs is fed into the spiral welded pipe forming equipment. During the spiral forming process, double-sided welding is performed to obtain a ferritic stainless steel thin-walled spiral welded pipe. The front weld facing the outside of the steel strip is welded using the TIG self-fusion welding process, and the back weld facing the inside of the steel strip is welded using the MIG welding method.

[0008] In the above-mentioned manufacturing method of thin-walled spiral welded pipe of ferritic stainless steel, the wall thickness of the reinforcing rib is 1.8~3 mm, and the ratio of arc height to chord length is 0.2~0.4.

[0009] The above-mentioned manufacturing method of thin-walled spiral welded pipe of ferritic stainless steel involves welding the reinforcing ribs using the TIG filler wire welding method for fillet welds, with the welding torch fixed at an angle of 35~55°, the welding current at 150~180A, and the welding speed at 0.9~1.1 m / min.

[0010] In the above-mentioned manufacturing method of thin-walled spiral welded pipe of ferritic stainless steel, the current of the TIG self-fusion welding process is 180~260A and the welding speed is 0.9~1.1 m / min.

[0011] The above-mentioned manufacturing method for thin-walled spiral welded pipes of ferritic stainless steel uses ER308L welding wire, an arc voltage of 21~24V, a welding current of 110~160A, and a welding speed of 0.9~1.1 m / min.

[0012] The above-mentioned method for manufacturing thin-walled spiral welded pipes of ferritic stainless steel has a wall thickness of 1.8~3 mm and a diameter of 273~478 mm.

[0013] The ferritic stainless steel thin-walled spiral welded pipe provided by the present invention includes a pipe body formed by spirally rolling ferritic stainless steel strip, and the outer surface of the pipe body is provided with spiral arc-shaped reinforcing ribs extending along its axial direction.

[0014] The aforementioned ferritic stainless steel thin-walled spiral welded pipe has a weld seam consisting of an outer TIG self-fusion weld seam and an inner MIG filler weld seam.

[0015] The aforementioned thin-walled spiral welded pipe made of ferritic stainless steel is a single-phase ferritic stainless steel.

[0016] The aforementioned thin-walled spiral welded pipe made of ferritic stainless steel is of the grade SUS439M, SUS409L, SUS429, SUS441, SUS443, SUS445 or SUS446.

[0017] The technical solution of the present invention has the following beneficial effects: (1) The manufacturing method of the ferritic stainless steel thin-walled spiral welded pipe of the present invention uses economical ferritic stainless steel to replace expensive austenitic stainless steel to manufacture thin-walled spiral welded pipe, which significantly reduces the cost of raw materials and enhances the market competitiveness of the product while maintaining good corrosion resistance and mechanical properties. (2) The manufacturing method of the thin-walled spiral welded pipe of the present invention significantly improves the deformation resistance and overall rigidity of the thin-walled welded pipe by pre-welding arc-shaped edge reinforcing ribs on the steel strip, so that the welded pipe with a wall thickness of only 1.8 to 3 mm can be stably manufactured to a diameter of 273 to 478 mm, realizing the reliable production of spiral welded pipe with large diameter-to-wall ratio, and broadening the application of ferritic stainless steel in the field of structural pipes. (3) The manufacturing method of the ferritic stainless steel thin-walled spiral welded pipe of the present invention adopts a double-sided double-process welding method combining front TIG self-fusion welding and back MIG filler wire welding, and strictly controls the welding heat input parameters, which effectively suppresses the excessive growth of ferrite grains in the weld and heat-affected zone, and ensures good mechanical properties and corrosion resistance of the welded joint. (4) The manufacturing method of the thin-walled spiral welded pipe of ferritic stainless steel of the present invention has the characteristics of small thermal expansion coefficient and single phase structure at both high temperature and room temperature. Therefore, the thermal stress and structural stress during welding are very small, and no heat treatment is required after welding, which simplifies the process and reduces energy consumption and production cost. (5) The manufacturing method of the ferritic stainless steel thin-walled spiral welded pipe of the present invention has been fully verified by systematic welding theory analysis, process test and example verification. It has been fully demonstrated that the welded pipe produced by the method has good weld formation, joint performance meets the standard and excellent corrosion resistance, and has clear industrial feasibility and technical reliability. Attached Figure Description

[0018] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention.

[0019] Figure 1 This is a schematic diagram of the reinforcing rib and its welding according to the present invention; Figure 2 Results of a simulated bending test on a SUS439M stainless steel specimen at 1350℃; Figure 3 The location of weld metal with a fusion ratio of 25% in the Schaeffler diagram; Figure 4 This is a schematic diagram illustrating the welding and manufacturing of thin-walled spiral welded pipes according to the present invention; Figure 5 The microstructure of the welded joint in Example 1; Figure 6 Tensile specimen of welded joint in Example 1; Figure 7 This is a positive bending specimen of the welded joint in Example 1; Figure 8 Example 1: Welded joint back bend specimen; Figure 9 The results of 72 hours of salt spray corrosion on the front weld of Example 1; Figure 10 The results of 72 hours of salt spray corrosion on the back weld of Example 1; Figure 11 shows the electrochemical corrosion results of the weld in Example 1. Detailed Implementation

[0020] To fully understand the purpose, features, and effects of this invention, the following detailed embodiments are provided. Except as described below, the process methods of this invention employ conventional methods or apparatus in the art. Unless otherwise specified, the terms and expressions used below have the meanings commonly understood by those skilled in the art.

[0021] Based on a deep understanding of the composition, microstructure, and properties of ferritic stainless steel, this invention has achieved a comprehensive and systematic understanding of the welding process and weldability of ferritic stainless steel through extensive welding process experiments and welding mechanism research. It has also determined the scientific validity and feasibility of replacing austenitic stainless steel and established a reasonable range of welding process parameters.

[0022] Specifically, the manufacturing method of the ferritic stainless steel thin-walled spiral welded pipe of the present invention includes welding of arc-shaped edge reinforcing ribs and a double-sided double-process welding method. According to relevant national standards, steel pipes with a wall thickness of 2-3mm correspond to diameters ranging from 63.5 to 219mm. However, by employing reinforced spiral welded pipe manufacturing methods, welded pipes with a large diameter-to-wall ratio can be produced. Thin-walled spiral welded pipes have a large diameter-to-wall ratio, resulting in poor rigidity. To improve the rigidity of the welded pipe, arc-shaped reinforcing ribs are welded to the outer surface of the steel strip to enhance the rigidity of the finished welded pipe. Figure 1 As shown, the steel strip is processed into an arc-shaped edge using a forming roller. The thickness of the stiffening plate is the same as the wall thickness of the welded pipe. The fillet weld is welded using the TIG filler wire welding method. The welding torch is fixed with an inclination angle α of 35~55°. The welding current is 150~180A, the welding speed is 0.9~1.1 m / min, the shielding gas is industrial pure argon, and the welding speed is the same as the steel strip conveying speed.

[0023] To maximize stiffness, the ratio of the arc height to the chord length of the stiffener is... t / lThe thickness should be controlled between 0.2 and 0.4; too high or too low a thickness will weaken the effect. Ferritic stainless steel spiral welded pipes are manufactured using a reinforcing rib process, with a wall thickness ranging from 1.8 to 3 mm, corresponding to a diameter range of 273 to 478 mm.

[0024] This invention improves the rigidity and deformation resistance of thin-walled, large-diameter spiral welded pipes by welding arc-shaped reinforcing ribs to the steel strip before spiral forming, thereby obtaining spiral welded pipes with a large diameter-to-wall ratio, reducing costs and unit weight of welded pipes, and making full use of the corrosion resistance and wear resistance of stainless steel.

[0025] To quantitatively analyze the influence of coarse grains in the hardness zone (HAZ) of ferritic stainless steel welded joints on their mechanical properties, the inventors designed and implemented the following experiment: Ferritic stainless steel SUS439M with a thickness of 1.8 mm was processed into tensile and bending specimens. These specimens were then held in a box-type resistance furnace at 1350℃ for 5 minutes and air-cooled to room temperature to obtain a whole-body simulated specimen with a grain size close to that of the HAZ of the welded joint. Mechanical property tests were then conducted, and the results can represent the characteristics of the HAZ microregion. The test results are shown in Table 1. Compared with the mechanical properties of the base material in Table 2, the strength and elongation after fracture decreased by 8-14%. Due to the formation of more carbonitrides, the hardness increased. The bending specimen exhibited an "orange peel" texture at the maximum bending point, but no cracks were generated (see Table 1). Figure 2 The above results indicate that coarse grains reduce the mechanical properties of stainless steel. Therefore, a filler wire welding process must be used to form weld reinforcement while avoiding the fusion line being parallel to the thickness direction in order to ensure the transverse tensile strength of the weld.

[0026] Table 1 Simulated HAZ Mechanical Properties of SUS439M Stainless Steel

[0027] Table 2 Mechanical properties of SUS439M stainless steel

[0028] Therefore, when formulating the welding process for welded pipes, a double-sided welding process is adopted. The front weld uses TIG self-fusion welding to ensure a beautiful weld formation. To improve the overall performance of the welded joint and avoid the formation of coarse ferrite throughout, the back (inner) weld uses MIG welding, and austenitic stainless steel welding wire ER308L is selected. The phase composition of the weld can be calculated using the Schaeffler diagram. Assuming a weld fusion ratio of 25%, when using ER308L austenitic stainless steel welding material, the resulting weld phase composition is located in the three-phase coexistence region of austenite + martensite + high-temperature ferrite. In the Schaeffler diagram (…),… Figure 3The star-shaped point located on the red line indicates a complex weld microstructure, primarily composed of austenite with approximately 20% ferrite and a small amount of martensite. The welding process parameters were determined to control the welding heat input while ensuring good weld formation, and to maintain production efficiency, a high-current, rapid welding process was adopted. The specific welding method and process are as follows: The first weld is the front (outer) weld, using TIG self-fusion welding to achieve an aesthetically pleasing shape. Specific process parameters are: welding current 180~260A, welding speed synchronized with the steel strip conveyor speed, 0.9~1.1m / min, and shielding gas is industrial pure argon. The second weld is the back (inner) weld, using MIG welding to ensure joint performance. Specific process parameters are: welding wire ER308L, arc voltage 21~24V, welding current 110~160A, welding speed synchronized with the steel strip conveyor speed, both 0.9~1.1m / min, and shielding gas is industrial pure argon.

[0029] To ensure welding quality, all welding methods employ horizontal welding positions, such as... Figure 4 As shown, the spiral welded pipe forming equipment moves forward while rotating, thereby completing the manufacturing of the welded pipe and cutting it into a certain length.

[0030] This invention employs a double-sided, dual-process welding method combining front-side TIG self-fusion welding and back-side MIG filler wire welding, and strictly controls welding heat input parameters to effectively suppress excessive growth of ferrite grains in the weld and heat-affected zone, ensuring good mechanical properties and corrosion resistance of the welded joint. Furthermore, by using high-current rapid welding to obtain smaller heat input and welding deformation, it becomes possible to produce finished welded pipes with wall thicknesses ranging from 1.8 to 3 mm and diameters ranging from 273 to 478 mm.

[0031] Ferritic stainless steel has a low coefficient of thermal expansion; the elastic modulus of typical ferritic stainless steel is 220 kN / mm². 2 (20℃), the coefficient of thermal expansion is 11.9×10. -6 The thermal conductivity at 500℃ is 23 W / m•K, and the specific heat capacity is 430 J / kg•K. The elastic modulus of typical austenitic stainless steel is 200 KN / mm². 2 (20℃), the coefficient of thermal expansion is 18.0×10. -6 The temperature is 500℃, the thermal conductivity is 15 W / m•K, and the specific heat capacity is 500 J / kg•K. Furthermore, ferritic stainless steel is a single-phase structure at both high and room temperatures, therefore the thermal and structural stresses during welding are very small, and post-weld heat treatment is not required.

[0032] On the other hand, the present invention also provides a thin-walled spiral welded pipe of ferritic stainless steel prepared according to the above method, comprising a pipe body formed by spirally rolling ferritic stainless steel strip, wherein the outer surface of the pipe body is provided with spiral arc-shaped reinforcing ribs extending along its axial direction.

[0033] Preferably, the weld seam of the pipe body includes an outer TIG self-fusion weld seam and an inner MIG filler weld seam, wherein, Preferably, the ferritic stainless steel is a single-phase ferritic stainless steel with the designation SUS439M, SUS409L, SUS429, SUS441, SUS443, SUS445 or SUS446.

[0034] Based on the chemical composition and physical properties of ferritic stainless steel, this invention selects appropriate welding methods, welding processes, welding parameters, and welding materials to manufacture high-performance, low-cost thin-walled spiral welded pipes on a general spiral welded pipe production line, replacing high-cost austenitic stainless steel welded pipes. It has the advantages of simple production process, high production efficiency, and low cost.

[0035] Example The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments, unless otherwise specified, are performed according to conventional methods and conditions.

[0036] Example 1 The stainless steel used in the experiment was SUS439M ferritic stainless steel, supplied in the condition of annealed and pickled, with a thickness of 1.8 mm. The mechanical properties are shown in Table 2, and the chemical composition is shown in Table 3.

[0037] Table 3 Chemical composition of SUS439M stainless steel (wt.%)

[0038] The steel strip is 400mm wide and, after uncoiling and leveling, is transported at a speed of 1m / min. First, reinforcing ribs are welded along the length of the steel strip at its center. These ribs are made of the same material and are formed into an arc-shaped strip edge using a forming roller, with a thickness of 1.8mm, a chord length of 100mm, and an arc height of 30mm. The TIG welding current is 180A, the welding torch tilt angle is 45°, the welding speed is 1 m / min, the shielding gas is industrial pure argon, and the filler wire is ER308L austenitic stainless steel welding wire with the following specifications: Φ 1.2mm.

[0039] The welding process employed is TIG+MIG double-sided dual-process automatic welding, completing the spiral welded pipe welding online. The front (outer) weld is TIG self-fusion welding with a welding current of 190A; the back (inner) weld is MIG welding using ER308L welding wire, an arc voltage of 21V, a welding current of 110A, a fixed welding torch, and a welding speed (i.e., the steel strip conveying speed) of 1m / min. The shielding gas used is industrial pure argon. The finished welded pipe specifications are as follows: Φ 273×1.8mm, single length 6m.

[0040] Performance testing 1. Weld appearance The weld appearance was inspected, and the internal and external welds were found to be well formed with no welding defects.

[0041] 2. Microstructure Figure 5 This is the microstructure of the welded joint. The upper part is the back weld and heat-affected zone (HAZ), and the lower part is the front weld and heat-affected zone (HAZ). The performance of the front weld is reduced due to the coarsening of ferrite grains, but the back weld is dominated by austenite and the HAZ grains grow less. Therefore, the joint exhibits good overall performance, which is verified by mechanical property tests.

[0042] 3. Mechanical properties Table 4 shows the mechanical property test results obtained from two samples cut from the finished welded joint. Figure 6 These are tensile test specimens of the welded joint after testing. Figure 7 It is a positive bending test sample of a welded joint. Figure 8 The welded joint back bend specimen showed that the fracture location was in the base material, and the elongation after fracture was greater than 30%. No cracks were found in either the positive bend or back bend specimens of the weld. Therefore, the welded joint has good performance and fully meets the application requirements.

[0043] Table 4 Mechanical Properties of Welded Joints of SUS439M Stainless Steel Spiral Welded Pipes

[0044] 4. Corrosion resistance 4.1 Salt spray corrosion test The salt spray corrosion test was conducted according to GB / T 10125-1997 "Artificial Atmosphere Corrosion Test - Salt Spray Test Method". All reagents used in the test were chemically pure or higher. First, a NaCl solution with a concentration of 0.05 g / ml was prepared using deionized water. The test was conducted at room temperature (25°C). At the same time, pH test paper was used to measure the pH value of the collected spray solution to ensure that the solution reached a neutral state and the pH value was maintained between 6.5 and 7.2. During the test, the salt spray deposition rate was closely monitored and kept at around 1.5 ml / h.

[0045] Figure 9 This is the result of 72 hours of salt spray corrosion on the front weld. Figure 10 This is the result of 72 hours of salt spray corrosion on the back weld. Figures 9-10 It can be seen that there is only a small amount of easily removable surface rust. The corrosion resistance test results show that the welded joint has good corrosion resistance.

[0046] 4.2 Electrochemical Corrosion Test The electrochemical corrosion test was conducted using a CS350 electrochemical workstation. The electrolytic cell was a standard three-electrode system, with the sample as the working electrode, a platinum electrode as the auxiliary electrode, and a saturated calomel electrode (SCE) as the reference electrode. The potentiodynamic scanning range was -0.5 to 0.5 V, the scanning rate was 2 mV / s, and the scanning frequency was 1 Hz. The selected corrosion solution was a 3.5 wt% sodium chloride solution, and the test temperature was 25 °C.

[0047] Figure 11 The electrochemical corrosion test results show that, due to the use of austenitic stainless steel welding materials, the corrosion resistance of the back weld (corrosion potential -0.11V) is higher than that of the front weld (-0.25V). In comparison, the corrosion potential of the 439M stainless steel base material is -0.15V. Therefore, the welded joint exhibits excellent corrosion resistance.

[0048] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0049] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0050] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A method for manufacturing a thin-walled spiral welded pipe of ferritic stainless steel, characterized in that, Includes the following steps: (1) Weld a reinforcing rib with an arc-shaped edge along the length of the ferritic stainless steel strip in the middle part of the strip; The wall thickness of the reinforcing rib is 1.8~3 mm, and the ratio of arc height to chord length is 0.2~0.

4. (2) The steel strip with reinforcing ribs is fed into the spiral welded pipe forming equipment. During the spiral forming process, double-sided welding is performed to obtain a ferritic stainless steel thin-walled spiral welded pipe. The front weld facing the outside of the steel strip is welded using the TIG self-fusion welding process, and the back weld facing the inside of the steel strip is welded using the MIG welding method. The TIG self-fusion welding process uses a current of 180~260A and a welding speed of 0.9~1.1 m / min; the MIG welding method uses ER308L welding wire, an arc voltage of 21~24V, a welding current of 110~160A, and a welding speed of 0.9~1.1 m / min. The ferritic stainless steel thin-walled spiral welded pipe has a wall thickness of 1.8~3 mm and a diameter of 273~478 mm.

2. The manufacturing method according to claim 1, characterized in that, The reinforcing ribs are welded using the TIG fillet welding method, with the welding torch fixed at an angle of 35~55°, the welding current at 150~180A, and the welding speed at 0.9~1.1 m / min.

3. A thin-walled spiral welded pipe of ferritic stainless steel manufactured by the method according to any one of claims 1 to 2, characterized in that, It includes a tube formed by spirally rolling ferritic stainless steel strip, and the outer surface of the tube is provided with spiral arc-shaped reinforcing ribs extending along its axial direction.

4. The ferritic stainless steel thin-walled spiral welded pipe according to claim 3, characterized in that, The welds of the pipe body include an outer TIG self-fusion weld and an inner MIG filler weld.

5. The ferritic stainless steel thin-walled spiral welded pipe according to claim 3, characterized in that, The ferritic stainless steel is a single-phase ferritic stainless steel.

6. The ferritic stainless steel thin-walled spiral welded pipe according to claim 3, characterized in that, The ferritic stainless steel grades are SUS439M, SUS409L, SUS429, SUS441, SUS443, SUS445 or SUS446.

Citation Information

Patent Citations

  • Large-diameter spiral welded steel pipe with metal linings and manufacturing method thereof

    CN104565560A

  • Circular seam butt welding method for seamless steel pipes

    CN112122750A

  • Method of manufacturing spiral steel pipe

    JP2009226464A