A boride-containing ceramic for high-temperature aerobic environments and a method for producing the same

CN121627418BActive Publication Date: 2026-11-24CHINA NAT PETROLEUM CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411258121.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2026-11-24
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

[0004]本发明的目的在于克服上述现有技术的缺点,提供一种高温有氧环境用含硼碳化物陶瓷及其制备方法,以解决现有技术中对于碳化物粉体在高温环境下抗氧化性能较差的问题

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121627418B_ABST
    Figure CN121627418B_ABST
Patent Text Reader

Abstract

This invention discloses a boron-containing carbide ceramic for high-temperature aerobic environments and its preparation method, belonging to the field of carbide ceramic technology. The ceramic is (Hf... n Ta m (C) x B y Using Hf and Ta as raw materials, carbides are prepared. Based on this, boron carbide and boron oxide are added as boron sources, allowing boron atoms to fill designed carbon vacancies without altering the crystal structure of the carbides. Simultaneously, boron carbide eliminates excess oxygen introduced by boron oxide, ultimately forming boron-containing carbides. The entire preparation process requires only one high-temperature treatment to prepare the powder and one high-temperature sintering to prepare the ceramic bulk, resulting in higher preparation efficiency. Furthermore, the prepared boron-containing carbide ceramic bulk exhibits high density and strong oxidation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of carbide ceramics technology, specifically relating to a boron-containing carbide ceramic for use in high-temperature oxygen-containing environments and its preparation method. Background Technology

[0002] In the oil and petrochemical industries, downhole drill bits and high-temperature corrosive components face extreme temperatures and highly corrosive media. Carbide ultra-high temperature ceramics possess high melting points, high stability, and high-temperature strength. Utilizing these ceramics to form protective coatings can extend the service life of critical equipment. Simultaneously, the high melting point of carbide ceramics makes them an important candidate material for thermal protection systems in extreme aerospace environments. However, the poor high-temperature oxidation resistance of traditional binary carbides limits their application.

[0003] Hf-Ta carbides exhibit high strength and hardness, enabling them to withstand significant mechanical stress and wear. Furthermore, their high melting point (up to 3900℃) allows them to maintain good performance at high temperatures, while also providing excellent corrosion resistance for long-term use in harsh environments. However, their oxidation resistance is weak. For example, the HfO2 layer formed by the oxidation of HfC below 1800℃ has a porous structure, making it difficult to prevent external oxygen from oxidizing the material. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a boron-containing carbide ceramic for high-temperature aerobic environments and its preparation method, so as to solve the problem of poor oxidation resistance of carbide powder in high-temperature environments in the prior art.

[0005] To achieve the above objectives, the present invention employs the following technical solution:

[0006] A method for preparing boron-containing carbide ceramics for high-temperature aerobic environments includes the following steps:

[0007] Step 1: Mix Hf powder, Ta powder, and carbon powder, ball mill, heat treat, and crush to obtain (Hf) n Ta m C x powder;

[0008] Step 2, (Hf) n Ta m C x The powder and boron source were ball-milled and mixed, then dried to obtain a mixture. The mixture was then sintered to obtain (Hf). n Ta m (C) x B yCeramics; where n / m=1 / 1~4 / 1, 0.7≤x≤0.9, 0.05≤y≤0.3, x+y≤0.97;

[0009] The boron source includes boron carbide and boron oxide.

[0010] A further improvement of the present invention is that:

[0011] Preferably, in step 1, the heat treatment temperature is 1100~1400℃ and the heat treatment time is ≥15min.

[0012] Preferably, in step 2, the molar ratio of boron carbide to boron oxide in the boron source is 3:(2-1).

[0013] Preferably, in step 1, the ball milling speed is 50-200 rpm and the ball milling time is 1-5 h.

[0014] Preferably, in step 2, the ball mill speed is 200-300 rpm and the ball-to-material ratio is 4:1-10:1.

[0015] Preferably, in step 2, the mixture is sintered by spark plasma to obtain (Hf) n Ta m (C) x B y Ceramics; during the spark plasma sintering process, the sintering temperature is 1600~2000℃, the sintering time is 10~30min, and the pressure is 40~60MPa.

[0016] A boron-containing carbide ceramic for high-temperature aerobic environments, prepared by any one of the above methods, wherein the structural formula of the boron-containing carbide ceramic is (Hf n Ta m (C) x B y The boron-containing carbide ceramic has a face-centered cubic structure, in which some carbon vacancy lattice spaces are replaced by boron.

[0017] Where, n / m=1 / 1~4 / 1, 0.7≤x≤0.9, 0.05≤y≤0.3, x+y≤0.97.

[0018] Preferably, n / m is 3 / 1 or 4 / 1.

[0019] Preferably, 0.70≤x≤0.80, 0.20≤y≤0.30, and x+y≤0.90.

[0020] Preferably, the boron-containing carbide ceramic is (Hf 0.50 Ta 0.50 (C) 0.80 B 0.10 ), (Hf 2 / 3Ta 1 / 3 (C) 0.60 B 0.30 ) or (Hf 0.75 Ta 0.25 (C) 0.88 B 0.09 Any one of them.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] This invention discloses a method for preparing boron-containing carbide ceramics for high-temperature aerobic environments. Addressing the problem of how to efficiently and easily prepare bulk boron-containing carbide ceramics, the method first involves high-temperature heat treatment to prepare Hf-Ta system carbides with carbon vacancies (Hf...). n Ta m C x The powder provides the basis for subsequent boron atom diffusion. Then, using boron carbide and boron oxide as boron sources, boron carbide eliminates the impurity oxygen introduced by boron oxide, and (Hf) n Ta m C x After the powder is ball-milled and mixed with a boron source, it is sintered to form boron-containing carbides (Hf). n Ta m (C) x B y This method introduces boron into the Hf-Ta powder system, improving the oxidation resistance of the carbides. Furthermore, the entire preparation process requires only one high-temperature treatment to prepare the powder and one high-temperature sintering to prepare the ceramic bulk. Using a dual boron source, boron is introduced into the carbides while simultaneously removing impurity oxygen, preventing the formation of porous structures. Compared to existing technologies, this method is simpler, significantly reduces process requirements, has a streamlined process, and high preparation efficiency, making it suitable for large-scale production.

[0023] This invention also discloses a boron-containing carbide ceramic for use in high-temperature aerobic environments, wherein the ceramic is (Hf n Ta m (C) x B y This ceramic uses Hf and Ta as raw materials to prepare carbides. Based on this, boron carbide and boron oxide are added as boron sources, allowing boron atoms to fill designed carbon vacancies without altering the crystal structure of the carbides. Simultaneously, boron carbide eliminates excess oxygen introduced by boron oxide, ultimately forming boron-containing carbides. This ceramic material has a face-centered cubic structure, high bulk density (>96%), and exhibits strong oxidation resistance at 1600℃ in an oxygen-rich environment. Attached Figure Description

[0024] Figure 1 Macroscopic morphology image of the ceramic block prepared in Example 1;

[0025] Figure 2 This is a scanning electron microscope image of the surface of the ceramic bulk material prepared in Example 1;

[0026] Figure 3 X-ray diffraction pattern of the ceramic bulk material prepared in Example 1;

[0027] Figure 4 Macroscopic morphology image of the ceramic block prepared in Example 2;

[0028] Figure 5 The image shows a scanning electron microscope (SEM) image of the surface of the ceramic bulk material prepared in Example 2.

[0029] Figure 6 The image shows the X-ray diffraction pattern of the ceramic bulk material prepared in Example 2. Detailed Implementation

[0030] The present invention will now be described in further detail with reference to the accompanying drawings:

[0031] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0032] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0033] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0034] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0035] The first aspect of this invention provides a method for preparing boron-containing carbide ceramics for high-temperature aerobic environments, comprising the following steps:

[0036] (1) Preparation of carbide powder: Hf powder (purity ≥99wt%, particle size in micrometers or nanometers) and Ta powder (purity ≥99wt%, particle size in micrometers or nanometers) are mixed with carbon powder (purity ≥99wt%, particle size in micrometers or nanometers) in a certain proportion. The mixture is mixed in a planetary ball mill instead of mechanical alloying. After mixing, the powder is dried at 30-50℃ and sieved to obtain a mixed powder. The mixed powder is placed in a graphite jar for high-temperature heat treatment, then cooled to room temperature and removed. The powder is then manually crushed to obtain carbide ((Hf) n Ta m C x Powder.

[0037] (2) Preparation of boron-containing carbide ceramics: The above-mentioned carbide powder was ball-milled and mixed with a boron source. After uniform mixing, the mixture was dried to obtain a final product. The mixture was then subjected to high-temperature sintering under spark plasma sintering conditions to obtain boron-containing carbide (Hf). n Ta m (C) x B y )ceramics.

[0038] In this process, the composite boron source mainly serves two purposes: First, it provides a composite boron source composed of boron carbide and boron oxide. The carbon atoms in boron carbide eliminate the oxygen impurities brought by boron oxide, and under high temperature conditions, the boron atoms dissolve into the carbon vacancy lattice occupied by the carbide. Second, boron oxide has a low melting point (around 450°C), and some boron oxide will volatilize during high-temperature sintering, making it difficult to control the boron content in the product. Boron carbide has a high melting point (around 2450°C), and it will not volatilize and consume boron atoms during sintering, making it easier to design the total boron atom content in the product.

[0039] Preferably, in step (1), the mixing conditions are: mixing time of 1 to 5 hours, medium of ethanol, rotation speed of 50 to 200 rpm, and ball-to-material ratio of 4:1 to 10:1.

[0040] Preferably, in step (1), the high-temperature heat treatment conditions are: vacuum degree < 5 Pa, temperature 1100~1400℃, holding time ≥ 15 min, and heating rate 5~100℃ / min.

[0041] Preferably, in step (2), the boron source is a composite boron source of boron carbide and boron oxide, with a molar ratio of boron carbide to boron oxide of 3 / 2 to 3 / 1; the purity of boron carbide is ≥99wt%, and its particle size is nanoscale; the purity of boron oxide is ≥99.9wt%.

[0042] Preferably, in step (2), the ball milling mixing conditions are: time of 0.5 to 2 hours, medium of ethanol, rotation speed of 200 to 300 rpm, and ball-to-material ratio of 4:1 to 10:1.

[0043] Preferably, in step (2), the operating conditions for the discharge plasma sintering are: vacuum degree ≤ 5 Pa, temperature 1600~2000℃, holding time 10~30 min, heating rate 100~200℃ / min, and pressure 40~60 MPa.

[0044] A second aspect of this invention provides a boron-containing carbide ceramic for use in high-temperature aerobic environments, wherein the molecular formula of the boron-containing carbide is (Hf n Ta m (C) x B y ), where n / m=1 / 1~4 / 1, 0.7≤x≤0.9, 0.05≤y≤0.3, x+y≤0.97, has a face-centered cubic structure, and the boron-containing carbides have excellent antioxidant properties at 1600℃ in an aerobic environment.

[0045] In this structure, some carbon vacancy lattices are occupied by boron, which improves the high-temperature sintering performance of the entire boron-containing carbide ceramic without changing the face-centered cubic structure.

[0046] Preferably, n / m is 3 / 1 and 4 / 1.

[0047] Preferably, 0.70≤x≤0.80, 0.20≤y≤0.30, and x+y≤0.90.

[0048] Preferably, the molecular formula of the boron-containing carbide is (Hf 0.50 Ta 0.50 (C) 0.80 B 0.10 ), (Hf 2 / 3 Ta 1 / 3 (C) 0.60 B 0.30 ), (Hf 0.75 Ta 0.25 (C) 0.88 B 0.09 One or more of the following.

[0049] More preferably, (Hf) 0.75 Ta 0.25 (C) 0.88 B 0.09 It has the best antioxidant properties.

[0050] The following description, in conjunction with specific embodiments, provides further details.

[0051] Example 1

[0052] (1) Hf powder, Ta powder, and C powder were mixed in a molar ratio of 0.75:0.25:0.88. The mixed powder was then ball-milled in a planetary ball mill for 5 hours. The particle size of Hf powder and Ta powder was <48μm, the particle size of C powder was <3.25μm, and the purity was ≥99%. The ball mill jar and balls were made of cemented carbide. The ball milling medium was ethanol, the rotation speed was 100rpm, and the ball-to-powder ratio was 4:1. After ball milling, the powder was removed, dried at 40℃, and sieved to obtain the mixed powder. The mixed powder was then placed in a graphite jar for high-temperature heat treatment. The process was carried out under vacuum with a vacuum degree of less than 5Pa. The temperature was raised to 1400℃ and held for 15 minutes at a heating rate of 100℃ / min. After cooling to room temperature, the powder was removed and manually crushed to obtain carbide powder.

[0053] (2) Boron carbide and boron oxide were weighed according to a molar ratio of 3:2. The atomic ratio of boron atoms in the added boron source to carbon atoms in the carbide was 0.09:0.88. The mixture was mixed in ethanol for 24 hours at a rotation speed of 200 rpm and a ball-to-material ratio of 4:1. After mixing, the mixture was dried at 40°C to obtain a mixture of boron source and carbide powder. The mixture was placed in a spark plasma sintering furnace for high-temperature sintering under the following conditions: vacuum degree <5 Pa, temperature rise to 1600°C and hold for 30 min, heating rate of 100°C / min, and sintering pressure of 40 MPa. The mixture was then cooled to room temperature and removed to obtain boron-containing carbide ceramic blocks.

[0054] (3) The macroscopic morphology of the prepared boron-containing carbide ceramic bulk is as follows: Figure 1 As shown, the microstructure of the ceramic surface is as follows: Figure 2 As shown, the ceramic surface is dense with no obvious pores, and the X-ray diffraction results of the ceramic are as follows ( Figure 3 The results showed that the boron-containing carbides were similar to TaC and HfC, exhibiting a face-centered cubic structure. ICP-OES elemental analysis revealed that the atomic ratio of Hf, Ta, C, and B in the boron-containing carbides was 0.75:0.25:0.88:0.09. The molecular formula of the boron-containing carbides is (Hf... 0.75 Ta 0.25 (C) 0.88 B 0.09 The relative density of the ceramic block is 96.7%.

[0055] Example 2

[0056] (1) Hf powder, Ta powder, and C powder were mixed in a molar ratio of 0.5:0.5:0.8. The mixed powder was then ball-milled in a planetary ball mill for 1 hour. The particle size of Hf powder and Ta powder was <48μm, the particle size of C powder was <3.25μm, and the purity was ≥99%. The ball mill jar and balls were made of cemented carbide. The ball milling medium was ethanol, the rotation speed was 200rpm, and the ball-to-powder ratio was 10:1. After ball milling, the powder was removed, dried at 40℃, and sieved to obtain the mixed powder. The mixed powder was then placed in a graphite jar for high-temperature heat treatment. The process was carried out under vacuum with a vacuum degree of less than 5Pa. The temperature was raised to 1100℃ and held for 30 minutes at a heating rate of 5℃ / min. The powder was then cooled to room temperature and manually crushed to obtain carbide powder.

[0057] (2) Boron carbide and boron oxide were weighed according to a molar ratio of 3:2. The atomic ratio of boron atoms in the added boron source to carbon atoms in the carbide was 0.1:0.8. The mixture was mixed in ethanol for 0.5 h at a rotation speed of 300 rpm and a ball-to-material ratio of 10:1. After mixing, the mixture was dried at 40 °C to obtain a mixture of boron source and carbide powder. The mixture was placed in a spark plasma sintering furnace for high-temperature sintering. The sintering conditions were: vacuum degree <5 Pa, temperature rise to 2000 °C and hold for 10 min, heating rate of 200 °C / min, and sintering pressure of 60 MPa. The mixture was then cooled to room temperature and removed to obtain boron-containing carbide ceramic blocks.

[0058] (3) The macroscopic morphology of the prepared boron-containing carbide ceramic bulk is as follows: Figure 4 As shown, the microstructure of the ceramic surface is as follows: Figure 5 As shown, the ceramic surface is dense with no obvious pores, and the X-ray diffraction results of the ceramic are as follows ( Figure 6 The results showed that the boron-containing carbides were similar to TaC and HfC, exhibiting a face-centered cubic structure. ICP-OES elemental analysis revealed that the atomic ratio of Hf, Ta, C, and B in the boron-containing carbides was 0.5:0.5:0.8:0.1. The molecular formula of the boron-containing carbides is (Hf... 0.50 Ta 0.50 (C) 0.80 B 0.10 The relative density of the ceramic block is 98.1%.

[0059] Example 3

[0060] (1) Hf powder, Ta powder, and C powder were mixed in a molar ratio of 2 / 3:1 / 3:0.6. The mixed powder was then ball-milled in a planetary ball mill for 5 hours. The particle size of Hf powder and Ta powder was <48μm, the particle size of C powder was <3.25μm, and the purity was ≥99%. The ball mill jar and balls were made of cemented carbide. The ball milling medium was ethanol, the rotation speed was 100rpm, and the ball-to-powder ratio was 4:1. After ball milling, the powder was removed, dried at 40℃, and sieved to obtain the mixed powder. The mixed powder was then placed in a graphite jar for high-temperature heat treatment. The process was carried out under vacuum with a vacuum degree of less than 5Pa. The temperature was raised to 1400℃ and held for 15 minutes at a heating rate of 100℃ / min. After cooling to room temperature, the powder was removed and manually crushed to obtain carbide powder.

[0061] (2) Boron carbide and boron oxide were weighed according to a molar ratio of 3:2. The atomic ratio of boron atoms in the added boron source to carbon atoms in the carbide was 0.3:0.6. The mixture was mixed in ethanol for 24 hours at a rotation speed of 200 rpm and a ball-to-material ratio of 4:1. After mixing, the mixture was dried at 40°C to obtain a mixture of boron source and carbide powder. The mixture was placed in a spark plasma sintering furnace for high-temperature sintering under the following conditions: vacuum degree <5 Pa, temperature rise to 1600°C and hold for 30 min, heating rate of 100°C / min, and sintering pressure of 40 MPa. The mixture was then cooled to room temperature and removed to obtain boron-containing carbide ceramic blocks.

[0062] (3) The prepared boron-containing carbides have a single-phase face-centered cubic structure. ICP-OES elemental analysis showed that the atomic ratio of Hf, Ta, C, and B in the boron-containing carbides was 2 / 3:1 / 3:0.6:0.3. The molecular formula of the boron-containing carbides is (Hf... 2 / 3 Ta 1 / 3 (C) 0.60 B 0.30 The relative density of the ceramic block is 97.0%.

[0063] The antioxidant properties of the products prepared in the examples were tested, and the results are shown in Table 1. The isothermal oxidation performance analysis of the ceramic blocks was conducted in a tubular oxidation furnace. During the experiment, the temperature was 1600℃, with a temperature control accuracy of ±1℃. A mixture of N2 and O2 gas was continuously introduced during the test, with a volume ratio of N2 / O2 = 80:20 and a gas flow rate of 200 ml / min. The isothermal oxidation rate of the ceramic was evaluated using the weight gain per unit area (ΔW / A), where ΔW = W1 - W0, W1 is the mass of the ceramic after oxidation; W0 is the mass of the ceramic before oxidation (mg); and A is the surface area of ​​the ceramic (cm²). 2 Calculate the square of the weight gain per unit area of ​​the ceramic, i.e., (ΔW / A). 2 By fitting the data, a linear relationship was found between the square of the weight gain per unit area and time, namely (ΔW / A). 2 =kp ·t,k p k is the oxidation rate constant, used to determine the oxidation resistance of ceramics. p The smaller the value, the slower the ceramic oxidation and the stronger its oxidation resistance. Table 1 shows that the oxidation rate constant of the ceramic blocks prepared in the embodiments of the present invention is less than 100 mg / L in an oxidation environment of 1600℃. 2 / (cm 4 It exhibits excellent high-temperature antioxidant properties (·min).

[0064] Table 1 Antioxidant Performance Test

[0065] Relative density (%) <![CDATA[Oxidation rate constant (k p , mg 2 / (cm 4 ·min))]]> Example 1 96.7 6.0 Example 2 98.1 94.4 Example 3 97.0 50.5

[0066] Example 4

[0067] (1) Hf powder, Ta powder, and C powder were mixed in a molar ratio of 2 / 3:1 / 3:0.6. The mixed powder was then ball-milled in a planetary ball mill for 5 hours. The particle size of Hf powder and Ta powder was <48μm, the particle size of C powder was <3.25μm, and the purity was ≥99%. The ball mill jar and balls were made of cemented carbide. The ball milling medium was ethanol, the rotation speed was 50rpm, and the ball-to-material ratio was 4:1. After ball milling, the powder was removed, dried at 40℃, and sieved to obtain the mixed powder. The mixed powder was then placed in a graphite jar for high-temperature heat treatment. The process was carried out under vacuum with a vacuum degree of less than 5Pa. The temperature was raised to 1200℃ and held for 15 minutes at a heating rate of 100℃ / min. The powder was then cooled to room temperature and the artificially crushed carbide powder was removed.

[0068] (2) Boron carbide and boron oxide were weighed according to a molar ratio of 3:2. The atomic ratio of boron atoms in the added boron source to carbon atoms in the carbide was 0.3:0.6. The mixture was mixed in ethanol for 24 hours at a rotation speed of 250 rpm and a ball-to-material ratio of 5:1. After mixing, the mixture was dried at 40°C to obtain a mixture of boron source and carbide powder. The mixture was placed in a spark plasma sintering furnace for high-temperature sintering under the following conditions: vacuum degree < 5 Pa, temperature rise to 1800°C and hold for 20 min, heating rate of 100°C / min, and sintering pressure of 50 MPa. The mixture was then cooled to room temperature and removed to obtain boron-containing carbide ceramic blocks.

[0069] Example 5

[0070] (1) Hf powder, Ta powder, and C powder were mixed in a molar ratio of 2 / 3:1 / 3:0.6. The mixed powder was then ball-milled in a planetary ball mill for 5 hours. The particle size of Hf powder and Ta powder was <48μm, the particle size of C powder was <3.25μm, and the purity was ≥99%. The ball mill jar and balls were made of cemented carbide. The ball milling medium was ethanol, the rotation speed was 100rpm, and the ball-to-powder ratio was 4:1. After ball milling, the powder was removed, dried at 40℃, and sieved to obtain the mixed powder. The mixed powder was then placed in a graphite jar for high-temperature heat treatment. The process was carried out under vacuum with a vacuum degree of less than 5Pa. The temperature was raised to 1200℃ and held for 15 minutes at a heating rate of 100℃ / min. After cooling to room temperature, the powder was removed and manually crushed to obtain carbide powder.

[0071] (2) Boron carbide and boron oxide were weighed according to a molar ratio of 3:1. The atomic ratio of boron atoms in the added boron source to carbon atoms in the carbide was 0.3:0.6. The mixture was mixed in ethanol for 24 hours at a rotation speed of 250 rpm and a ball-to-material ratio of 5:1. After mixing, the mixture was dried at 40°C to obtain a mixture of boron source and carbide powder. The mixture was placed in a spark plasma sintering furnace for high-temperature sintering under the following conditions: vacuum degree < 5 Pa, temperature rise to 1800°C and hold for 20 min, heating rate of 100°C / min, and sintering pressure of 50 MPa. The mixture was then cooled to room temperature and removed to obtain boron-containing carbide ceramic blocks.

[0072] This invention discloses a boron-containing carbide ceramic for high-temperature aerobic environments and its preparation method. The method addresses the problem of how to efficiently and easily prepare bulk boron-containing carbide ceramics. First, high-temperature heat treatment is used to prepare Hf-Ta system carbides with carbon vacancies (Hf... n Ta m C x The powder provides the basis for subsequent boron atom diffusion. Then, using boron carbide and boron oxide as boron sources, boron carbide eliminates the impurity oxygen introduced by boron oxide, and (Hf) n Ta m C x After the powder is ball-milled and mixed with a boron source, it is sintered to form boron-containing carbides (Hf). n Ta m (C) x B yThis method, on the one hand, adds boron carbide and boron oxide as boron sources, allowing boron atoms to fill designed carbon vacancies without altering the crystal structure of the carbide. Simultaneously, boron carbide eliminates excess oxygen introduced by boron oxide, ultimately forming boron-containing carbides. On the other hand, the entire preparation process requires only one high-temperature treatment to prepare the powder and one high-temperature sintering to prepare the ceramic bulk. Through the dual boron sources, boron is introduced into the carbide while simultaneously removing impurity oxygen, preventing the formation of porous structures. Compared to existing technologies, this method is simpler, significantly reduces process requirements, has a simple process flow, and high preparation efficiency, making it suitable for large-scale production.

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing boron-containing carbide ceramics for use in high-temperature aerobic environments, characterized in that, Includes the following steps: Step 1: Mix Hf powder, Ta powder, and carbon powder, ball mill, heat treat, and crush to obtain (Hf) n Ta m C x Powder; heat treatment temperature is 1100~1400℃, heat treatment time is ≥15min; Step 2, (Hf) n Ta m C x The powder and boron source were ball-milled and mixed, then dried to obtain a mixture. The mixture was then sintered to obtain (Hf). n Ta m (C) x B y Ceramics; among which, n / m =1 / 1~4 / 1, 0.7≤ x ≤0.9, 0.05≤ y ≤0.3, x + y ≤0.97; By sintering the mixture with spark plasma, (Hf) was obtained. n Ta m (C) x B y Ceramics; During the spark plasma sintering process, the sintering temperature is 1600~2000℃, the sintering time is 10~30 min, and the pressure is 40~60 MPa; The boron source includes boron carbide and boron oxide.

2. The method for preparing boron-containing carbide ceramics for high-temperature aerobic environments according to claim 1, characterized in that, In step 2, the molar ratio of boron carbide to boron oxide in the boron source is 3:(2~1).

3. The method for preparing boron-containing carbide ceramics for high-temperature aerobic environments according to claim 1, characterized in that, In step 1, the ball mill speed is 50~200 rpm.

4. The method for preparing boron-containing carbide ceramics for high-temperature aerobic environments according to claim 3, characterized in that, In step 1, the ball milling time is 1 to 5 hours.

5. The method for preparing boron-containing carbide ceramics for high-temperature aerobic environments according to claim 1, characterized in that, In step 2, the ball mill speed is 200~300 rpm.

6. The method for preparing boron-containing carbide ceramics for high-temperature aerobic environments according to claim 1, characterized in that, In step 2, the ball-to-material ratio is 4:1 to 10:

1.

7. A boron-containing carbide ceramic for high-temperature aerobic environments prepared by any one of claims 1-6, characterized in that, The structural formula of the boron-containing carbide ceramic is (Hf) n Ta m (C) x B y The boron-containing carbide ceramic has a face-centered cubic structure, in which some carbon vacancy lattice spaces are replaced by boron. in, n / m =1 / 1~4 / 1, 0.7≤ x ≤0.9, 0.05≤ y ≤0.3, x + y ≤0.

97.

8. The boron-containing carbide ceramic for high-temperature aerobic environments according to claim 7, characterized in that, n / m It can be 3 / 1 or 4 / 1.

9. A boron-containing carbide ceramic for high-temperature aerobic environments according to claim 7, characterized in that, 0.70≤ x ≤0.80,0.20≤ y ≤0.30, x + y ≤0.90。 10. A boron-containing carbide ceramic for high-temperature aerobic environments according to claim 7, characterized in that, The boron-containing carbide ceramic is (Hf) 0.50 Ta 0.50 (C) 0.80 B 0.10 ) or (Hf 0.75 Ta 0.25 (C) 0.88 B 0.09 Any one of them.

Citation Information

Patent Citations

  • High-entropy transition-rare earth metal diboride ceramic material and preparation method thereof

    CN114507074A

  • Ceramic boron-containing doping paste and methods therefor

    US20120280183A1