A method for preparing micro-nano concave structure based on ultrafast laser processing

By directly fabricating mushroom-shaped micro/nano structures on the surface of substrate materials using ultrafast laser processing technology, the problems of low processing efficiency and poor material applicability in existing methods are solved. This achieves a highly efficient and simplified fabrication process, which is applicable to fields such as superhydrophobic and superoleophobic functional surfaces, micro-optics and photonic devices, microfluidics and biochips.

CN121670164BActive Publication Date: 2026-11-20SHANDONG UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610095818.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-01-23
Publication Date
2026-11-20
Estimated Expiration
2046-01-23

AI Technical Summary

Technical Problem

Existing methods for preparing mushroom-shaped micro/nano structures suffer from low processing efficiency, poor material applicability, and complex processes, making it difficult to meet the needs of complex liquid operations in fields such as biomedical detection and drug development.

Method used

Using ultrafast laser processing technology, mushroom-shaped micro-nano structures are directly fabricated on the surface of a substrate material through a combination of tilted incidence and vertical reconstruction strategies. Laser-induced removal, sputtering, and redeposition processes are then used to form three-dimensional microstructures with specific concave surfaces.

Benefits of technology

It achieves an efficient and simplified preparation process, avoids mold dependence and complex post-processing, and has high flexibility and multifunctional interface potential, making it suitable for fields such as superhydrophobic and superoleophobic functional surfaces, micro-optics and photonic devices, microfluidics and biochips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121670164B_ABST
    Figure CN121670164B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of super-dual functional material, and particularly relates to a preparation method of micro-nano concave structure based on ultrafast laser processing. The substrate material is placed on the processing platform, the processing platform is rotated to form an inclined angle η with the X-axis plane, laser processing is performed, and a group of parallel distributed inclined grooves are induced to form; the processing platform is reversely rotated to the same inclined angle, laser processing is performed, and a T-shaped bidirectional groove structure is obtained; the processing platform is rotated to form an inclined angle η with the Y-axis plane, the laser processing mode of the X-axis plane is repeated, and the staggered arrangement of inclined groove arrays is formed; the processing platform is rotated to be horizontal, the sharp corners of the staggered arrangement of inclined grooves are removed, and the structure is deepened, and the mushroom head array micro-nano structure is obtained. The application not only simplifies the preparation process, but also avoids the dependence on the mold and the complex post-processing technology, and provides a new solution for realizing the precise control of complex liquid and constructing a new type of functional surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of superhydrophobic functional materials technology, specifically relating to a method for fabricating micro-nano concave structures based on ultrafast laser processing. Background Technology

[0002] Mushroom-shaped micro / nanostructures have become an important area of ​​research in surface wettability regulation and droplet manipulation in recent years, attracting significant attention due to their unique concave geometry, wider at the top and narrower at the bottom. These structures significantly enhance capillary support at the solid-liquid interface and create a three-phase contact line pinning effect at the structure edges, effectively suppressing the transition from the Cassie-Baxter to the Wenzel wettability state. Leveraging this advantage, mushroom-shaped surfaces exhibit excellent superhydrophobic properties for high-surface-tension water droplets while also demonstrating stable superoleophobic properties for low-surface-tension organic droplets, thus earning the title of "superbihydrophobic" functional surfaces.

[0003] With the increasing demand for complex liquid micro-manipulation in fields such as biomedical detection, drug development, and chemical analysis, traditional planar superhydrophobic structures are no longer sufficient to meet application requirements in terms of adaptability and stability. Mushroom-shaped structures, with their low adhesion and high stability, offer a new solution for the pickup, transfer, and release of complex liquids. Currently, methods for fabricating mushroom-shaped structures mainly include two-photon polymerization micro / nano printing, silicon-based etching, and transfer molding. Two-photon polymerization is one of the most common methods for fabricating mushroom-shaped structures. It utilizes a high-precision focused laser to solidify layer by layer in photosensitive resin, enabling the creation of complex three-dimensional micro / nano structures with almost arbitrary morphologies. However, its printing speed is extremely low (generally less than 1 mm). 3 Fabricating large-area arrays using methods that are time-consuming, difficult to guarantee consistency, and only applicable to photosensitive materials is feasible. Transfer printing typically relies on etching silicon-based or glass molds, followed by casting elastomers such as polydimethylsiloxane (PDMS) to replicate the mold's surface structure. This method is suitable for mass production, but the mold fabrication process is complex, involving high-cost processes such as reactive ion etching (RIE) and deep reactive ion etching (DRIE), and structural damage or deformation is easily caused during demolding, affecting repeatability. Traditional microfabrication methods such as wet etching and dry etching can also form recessed structures that are wider at the top and narrower at the bottom, but the process time is long (e.g., SiO2 etching rate is about 4 nm / min), the processing efficiency is low, and it is mainly limited by silicon-based materials. Therefore, existing methods for fabricating mushroom-shaped micro / nano structures often suffer from low processing efficiency, poor material applicability, and complex processes. Summary of the Invention

[0004] The purpose of this invention is to provide a method for fabricating micro / nano concave structures based on ultrafast laser processing. This method directly fabricates mushroom-shaped micro / nano structures on the surface of a substrate material through a laser-induced removal, sputtering, and redeposition process. This method not only simplifies the fabrication process but also avoids mold dependence and complex post-processing, providing a new solution for the precise manipulation of complex liquids and the construction of novel functional surfaces.

[0005] The present invention solves the above-mentioned technical problems through the following technical solutions.

[0006] The purpose of this invention is to provide a method for fabricating micro / nano concave structures based on ultrafast laser processing, comprising the following steps: S1. Place the substrate material on the processing platform and rotate the processing platform to form an inclination angle η with the X-axis plane, where η is 15° to 25°. Perform laser processing so that the laser is incident on the surface of the substrate material in a vertical manner, inducing the formation of a set of parallel inclined grooves.

[0007] S2. Reverse rotation of the machining platform to make the tilt angle of the machining platform the same in the X-axis plane, and laser processing is performed to induce the formation of reverse cross grooves on each tilted groove to obtain a T-shaped bidirectional groove structure.

[0008] S3. Rotate the processing platform until it forms an angle η with the Y-axis plane, and repeat the laser processing method on the X-axis plane so that the grooves in the X-axis direction and the Y-axis direction are orthogonally superimposed to form an array of staggered inclined grooves.

[0009] S4. Rotate the processing platform to a horizontal position so that the laser is incident vertically. Remove the sharp corners and deepen the structure of the staggered inclined grooves to obtain the mushroom head array micro-nano structure. The top width of each mushroom head micro-nano structure is 50μm to 450μm, the bottom width is 50μm to 100μm, and the top width is greater than the bottom width.

[0010] Furthermore, in the mushroom-shaped array micro / nano structure, the spacing between adjacent mushroom-shaped micro / nano structures is 100μm to 500μm, and the groove width of each mushroom-shaped micro / nano structure is 50μm to 200μm.

[0011] Furthermore, the depth of each mushroom-shaped micro-nano structure is 200μm to 600μm, and the concave angle is 15° to 25°.

[0012] Furthermore, during the laser processing, the average laser power is 12W to 20W, the laser pulse frequency is 100kHz to 500kHz, and the laser beam wavelength is 353nm.

[0013] Furthermore, during the laser processing, reciprocating scanning is performed at a speed of 2000–5000 mm / s and the number of scans is 10–50.

[0014] Furthermore, the substrate material is a (polydimethylsiloxane) film.

[0015] Furthermore, the thickness of the matrix material is 1mm to 2mm.

[0016] Furthermore, the mushroom-shaped array micro / nano structure exhibits superhydrophobic properties, with a water droplet contact angle greater than 150° and an oil droplet contact angle greater than 150°.

[0017] Compared with the prior art, the present invention has the following advantages: The present invention provides a method for fabricating micro / nano concave structures based on ultrafast laser processing. By adjusting the tilt angle of the laser in the XY plane, a combined processing strategy of tilted incidence and vertical reconstruction is adopted. Through dynamic adjustment of the incident angle, the spatial control of energy distribution and melting direction is achieved, enabling controllable modulation of the melting morphology of the substrate material surface. The laser-induced removal of substrate material causes the groove edges to gradually evolve into a mushroom-shaped structure, thereby directly forming a three-dimensional microstructure with a specific concave surface. The concave structure formed by tilted incidence enhances the mechanical stability and liquid support capacity of the surface, providing a more optimized geometric basis for constructing superhydrophobic, superoleophobic, antifouling, and wear-resistant interfaces. This geometric feature can generate a strong three-phase contact line pinning effect when droplets come into contact, thereby significantly enhancing the stability of the Cassie-Baxter state and making the surface exhibit superhydrophobic properties to both water and oil. This process avoids the heat-affected zone and carbonization phenomena commonly found in picosecond laser etching. The fabrication process can achieve stable superhydrophobic properties without chemical modification. This method not only simplifies the fabrication process but also avoids mold dependence and complex post-processing, providing a new solution for the precise control of complex liquids and the construction of novel functional surfaces.

[0018] This invention is based on ultrafast laser processing, which can achieve precise design and repeatable processing through parameter adjustment. The morphological stability and consistency are significantly better than those of stress-induced processing. It has high flexibility, scalability and multifunctional interface potential, and has broad application prospects, such as superhydrophobic and superoleophobic functional surfaces, micro-optics and photonic devices, as well as microfluidics and biochips. Attached Figure Description

[0019] Figure 1 This is a process flow diagram for preparing the micro / nano concave structure of the present invention.

[0020] Figure 2 The microstructure diagram of the micro-nano concave structure prepared in Example 1 of the present invention is shown.

[0021] Figure 3 The image shows the superhydrophobic properties of the micro / nano concave array structure prepared in Example 1 of this invention. Figure 3 In the figure, a is the water droplet contact angle and b is the oil droplet contact angle. Detailed Implementation

[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] It should be noted that the technical terms used in this invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this invention. Unless otherwise specified, all raw materials, reagents, instruments and equipment used in the following embodiments of this invention can be purchased from the market or prepared by existing methods.

[0024] Currently, methods for fabricating mushroom-shaped structures mainly include two-photon polymerization micro / nano printing, silicon-based etching and transfer molding, etc. However, these methods often suffer from low processing efficiency, poor material applicability, and complex processes. With the deepening research on droplet manipulation and surface wetting control, developing a novel processing method that is simple, efficient, and applicable to a wide range of materials has become an urgent problem to solve. This invention is based on ultrafast laser processing technology, which has advantages such as non-contact operation, high flexibility, high processing efficiency, no need for masks, and wide applicability to materials. It can directly fabricate mushroom-shaped micro / nano structures on the surface of polymers, metals, or inorganic materials through laser-induced removal, sputtering, and redeposition processes. This method not only simplifies the fabrication process but also avoids mold dependence and complex post-processing, providing a new solution for the precise manipulation of complex liquids and the construction of novel functional surfaces.

[0025] Based on this, the present invention provides a method for fabricating micro / nano concave structures based on ultrafast laser processing, comprising the following steps: S1. Construct mushroom-shaped micro / nano structures (i.e., micro / nano structures that are wider at the top and narrower at the bottom, with the top width > the bottom width). The spacing between adjacent mushroom-shaped micro / nano structures is 100μm to 500μm. The geometric features of each mushroom-shaped micro / nano structure are as follows: top width is 50μm to 450μm, bottom width is 50μm to 100μm, groove width is 50μm to 200μm, structure depth is 200μm to 600μm, and concave angle is 15° to 25°.

[0026] S2. Place the substrate material on the processing platform and rotate the processing platform to form an inclination angle η with the X-axis plane, where η is 15° to 25°. Perform laser processing so that the laser is incident on the surface of the substrate material in a vertical manner, inducing the formation of a set of parallel inclined grooves.

[0027] In this invention, the processing platform is a five-axis linkage motion platform capable of movement, rotation, and tilting along the X and Y axes, and is equipped with a high-precision camera positioning system. The motion platform is an ARM Precision Control SSOOi-C2.

[0028] In this invention, after rotating the processing platform to form an inclination angle η with the X-axis plane, the laser beam is kept perpendicular to the incident surface, thereby achieving the inclination of the laser beam onto the sample surface. The laser beam is reciprocated in the X direction, and several parallel grooves are obtained in each processing. After processing is completed, the platform is controlled to move a distance in the X direction and the focal length is adjusted. The scanning is repeated to form a set of parallel inclined grooves.

[0029] In this invention, the substrate material is a polymer, inorganic material, or metallic material, and the thickness of the substrate material is 1mm to 2mm. As a preferred embodiment, the polymer is a (polydimethylsiloxane) film, the inorganic material is glass, and the metallic material is stainless steel. In one specific embodiment, the substrate material is a (polydimethylsiloxane) film, and the preparation method of the (polydimethylsiloxane) film includes the following steps: mixing polydimethylsiloxane and a curing agent (Corning DC184 original PDMS polydimethylsiloxane high-transparency optical adhesive) at a mass ratio of 10:1, stirring evenly, and then curing at 80°C for 2 hours to obtain the (polydimethylsiloxane) film.

[0030] S2. Reverse rotation of the machining platform to make the tilt angle of the machining platform the same in the X-axis plane, and laser processing is performed to induce the formation of reverse cross grooves on each tilted groove to obtain a T-shaped bidirectional groove structure.

[0031] In this invention, the processing platform has the same tilt angle on the X-axis plane. The tilted groove is positioned by the camera positioning system, and the S1 laser processing process is repeated to form a reverse cross groove in the original groove area, thereby obtaining a T-shaped bidirectional groove structure.

[0032] S3. Rotate the processing platform until it forms an angle η with the Y-axis plane, and repeat the laser processing method on the X-axis plane so that the grooves in the X-axis direction and the Y-axis direction are orthogonally superimposed to form an array of staggered inclined grooves.

[0033] In this invention, the tilt angle η between the processing platform and the Y-axis plane is the same as the tilt angle η between the processing platform and the X-axis plane. The laser beam is kept perpendicular to the incident point. Steps S1 and S2 are repeated in the Y-axis direction, so that the grooves in the X-axis direction and the Y-axis direction are orthogonally superimposed to form an array of staggered tilted grooves.

[0034] S4. Rotate the processing platform to a horizontal position so that the laser is incident vertically. Remove the sharp corners and deepen the structure of the interlaced inclined grooves to obtain the mushroom-head array micro / nano structure.

[0035] In this invention, a micro / nano concave array structure, i.e., a mushroom-shaped micro / nano array structure, is fabricated using ultrafast laser processing. The average laser power is 12W–20W, the laser pulse frequency is 100kHz–500kHz, the laser beam wavelength is 353nm, the reciprocating scanning speed is 2000mm / s–5000mm / s, and the number of scans is 10–50. This method not only simplifies the fabrication process but also avoids mold dependence and complex post-processing, providing a new solution for the precise manipulation of complex liquids and the construction of novel functional surfaces.

[0036] In this invention, the surface of the mushroom-shaped array micro / nano structure has superhydrophobic properties, wherein the contact angle of water droplets is greater than 150° and the contact angle of oil droplets is greater than 150°.

[0037] This invention achieves controllable modulation of the melting morphology on a material surface by adjusting the tilt angle of the laser in the XY plane, thereby directly forming a three-dimensional microstructure with a specific concave surface. Compared with traditional vertically incident laser processing methods, this method has the following significant technical advantages: Breaking the limitations of a single vertical processing mode: Traditional laser micromachining mostly uses vertical incidence, which can only obtain vertical or top-narrow-bottom-wide groove structures. This invention, by dynamically adjusting the incident angle, achieves spatial control of energy distribution and melting direction, and can flexibly construct complex three-dimensional morphologies that are top-wide-bottom-narrow or symmetrically concave. No additional molds or multiple processing steps required: Compared with obtaining concave structures through template transfer, reverse forming, or multi-step stacking processes, this invention can form in one step, greatly simplifying the process and improving efficiency and structural consistency. Programmable energy field control: By adjusting the scanning angle, path, and focal point position, precise control of local energy deposition can be achieved, possessing digital, high-precision, and repeatable processing characteristics, and adapting to various material systems. The structure offers high design flexibility: the concave structure formed by oblique incidence enhances the surface's mechanical stability and liquid support capabilities, providing a more optimized geometric basis for constructing superhydrophobic, superoleophobic, antifouling, and wear-resistant interfaces. In summary, this invention represents a leap from "vertical etching" to "angle-adjustable spatial construction," breaking through the limitations of traditional processing geometry and demonstrating significant advancements and innovations in precision manufacturing, functional interface construction, and micro-optical component fabrication.

[0038] This invention, based on laser concave structure fabrication technology with tilt angle control, possesses high flexibility, scalability, and multifunctional interface potential, with broad application prospects: Superhydrophobic and superoleophobic functional surfaces: The concave structure can stably maintain the Cassie-Baxter state, reducing the contact area between liquids and solids, achieving long-term waterproofing, oil resistance, self-cleaning, and anti-fouling properties, suitable for fields such as construction, optical lenses, and spacecraft surface protection. Micro-optics and photonic devices: Tilted laser processing can fabricate microlens arrays, optical traps, or focusing cavity structures on transparent substrates, with significant application value in light field manipulation, micro-optical integration, and light capture. Microfluidics and biochips: It can construct droplet manipulation channels or liquid traps with specific curvatures, improving the stability and controllability of fluid interfaces, providing novel design solutions for lab-on-a-chip, precise droplet reactions, and biological detection. High-reliability functional interfaces: The concave structure exhibits excellent compressive strength and wear resistance under mechanical loading, suitable for flexible sensors, anti-slip surfaces, and highly wear-resistant engineering interfaces.

[0039] The following specific examples will provide further explanation.

[0040] Example 1 A method for fabricating micro / nano concave structures based on ultrafast laser processing includes the following steps: S1. Construct mushroom-shaped micro / nano structures with a spacing of approximately 500 μm between adjacent mushroom-shaped micro / nano structures. The geometric features of each mushroom-shaped micro / nano structure are as follows: upper width of approximately 350 μm, groove width of approximately 150 μm, structural depth of approximately 500 μm, and concave angle of approximately 15°.

[0041] S2. Preparation of matrix material: Polydimethylsiloxane (PDMS) and curing agent are mixed at a mass ratio of 10:1, stirred evenly, and cured at 80°C for 2 hours to obtain a (polydimethylsiloxane) film with a thickness of 1 mm.

[0042] S3. The (polydimethylsiloxane) film is fixed on a processing platform, which is a five-axis linkage motion platform equipped with a high-precision camera positioning system. The laser processing system used is an ultraviolet ultrafast laser with a wavelength of 355nm, an average power of 12W, a pulse frequency of 100kHz, and a pulse width of 300fs. The processing platform is rotated and tilted 15° around the X-axis to maintain perpendicular laser incidence, achieving tilted incidence on the sample surface. A reciprocating scan is performed in the X-direction at a scanning speed of 5000mm / s, for 20 scans. Each scan yields several tilted grooves. After processing, the platform is moved 100μm along the X-direction, and the focal length is adjusted. The above operation is repeated to obtain a set of parallel tilted grooves.

[0043] S4. Rotate the processing platform 15° in the opposite direction around the X-axis, locate the groove position through the camera, and perform laser processing. Keep the laser beam perpendicular to the incident point and perform reciprocating scanning in the X direction. Repeat the processing method of S3 to form a reverse cross groove in the original groove area and obtain a T-shaped bidirectional groove structure.

[0044] S5. Rotate the processing platform around the Y-axis and tilt it by 15°. After positioning the groove position through the camera, perform laser processing. Keep the laser beam perpendicular to the incident point and repeat the laser processing method of the X-axis plane in the Y-axis direction (i.e., repeat the processing methods of S3 and S4) so ​​that the grooves in the X-axis direction and the Y-axis direction are orthogonally superimposed to form an array of staggered tilted grooves.

[0045] S6. Rotate the processing platform to a horizontal position. After positioning the grooves using a camera, direct the laser beam vertically to further process the staggered, inclined grooves, removing sharp corners and deepening the structure. This transforms the grooves into mushroom-shaped micro / nano concave structures without sharp corners and with a predetermined depth. The microstructure is as follows: Figure 2 As shown.

[0046] The superhydrophobic properties of the micro / nano concave array structure prepared in Example 1 were tested. Figure 3 The image shows the superhydrophobic properties of the micro / nano concave array structure prepared in Example 1 of this invention. Figure 3 In the diagram, 'a' represents the contact angle of a water droplet, and 'b' represents the contact angle of an oil droplet. For example... Figure 3 As shown, the contact angle of water droplets on the surface is 152°, the contact angle of oil droplets is 151°, and the roll-off angle is less than 10°, proving that the micro-nano concave array structure based on ultrafast laser processing in Example 1 can effectively construct a stable superhydrophobic functional interface on the PDMS surface, which is suitable for precise control of droplets.

[0047] Example 2 A method for fabricating micro / nano concave structures based on ultrafast laser processing includes the following steps: S1. Construct mushroom-shaped micro / nano structures with a spacing of 200 μm between adjacent mushroom-shaped micro / nano structures. The geometric features of each mushroom-shaped micro / nano structure are: an upper width of approximately 120 μm, a groove width of approximately 80 μm, a structural depth of approximately 220 μm, and an inward concavity angle greater than 15°.

[0048] S2. Preparation of matrix material: Polydimethylsiloxane (PDMS) and curing agent are mixed at a mass ratio of 10:1, stirred evenly, and cured at 80°C for 2 hours to obtain a (polydimethylsiloxane) film with a thickness of 1 mm.

[0049] S3. Fix the (polydimethylsiloxane) film onto the processing platform, which is a five-axis linkage motion platform equipped with a high-precision camera positioning system. The laser processing system used is an ultraviolet ultrafast laser with a wavelength of 400nm, an average power of 8W, and a pulse frequency of 80kHz. Rotate the processing platform and tilt it 25° around the X-axis to keep the laser perpendicular to the incident light, so as to achieve tilted incident light on the sample surface. Perform reciprocating scanning in the X direction at a scanning speed of 3000mm / s and 20 scans. Each scan obtains several tilted grooves. After processing, move it 150μm along the X direction and adjust the focal length. Repeat the above operation to obtain a set of parallel tilted grooves.

[0050] S4. Rotate the processing platform 25° in the opposite direction around the X-axis, locate the groove position through the camera, and perform laser processing. Keep the laser beam perpendicular to the incident point and perform reciprocating scanning in the X direction. Repeat the processing method of S3 to form a reverse cross groove in the original groove area and obtain a T-shaped bidirectional groove structure.

[0051] S5. Rotate the processing platform around the Y-axis and tilt it by 25°. After positioning the groove position through the camera, perform laser processing. Keep the laser beam perpendicular to the incident point and repeat the laser processing method of the X-axis plane in the Y-axis direction (i.e., repeat the processing methods of S3 and S4) so ​​that the grooves in the X-axis direction and the Y-axis direction are orthogonally superimposed to form an array of staggered tilted grooves.

[0052] S6. Rotate the processing platform to a horizontal position. After positioning the grooves using a camera, the laser is incident vertically to further process the staggered inclined grooves, removing sharp corners and deepening the structure. The number of vertical incidents is increased to 3 to ensure the structural depth, evolving it into a mushroom-shaped micro-nano concave structure without sharp corners and with a predetermined depth.

[0053] The superhydrophobic properties of the micro-nano concave array structure prepared in Example 2 were tested. The contact angle of water droplets was 156°, the contact angle of oil droplets was 154°, and the roll-off angle was less than 10°. This proves that the micro-nano concave array structure based on ultrafast laser processing in Example 2 can effectively construct a stable superhydrophobic functional interface on the PDMS surface, which is suitable for the precise manipulation of droplets.

[0054] In summary, this invention utilizes a two-stage process of "laser template etching—PDMS reverse curing—laser separation and reconstruction." A regular grid of trenches is formed on the substrate using a femtosecond laser. Subsequently, the partial wetting properties of PDMS liquid are used to locally cure the top regions of the columns. A second laser separation process forms independent cap-shaped structures, achieving precise and controllable construction of the mushroom-shaped array. This geometric feature generates a strong three-phase contact line pinning effect upon droplet contact, significantly enhancing the stability of the Cassie-Baxter state and making the surface exhibit superhydrophobic properties to both water and oil. This process avoids the heat-affected zone and carbonization phenomena common in picosecond laser etching, and stable superhydrophobic and anti-repellent properties can be achieved without chemical modification. Secondly, the structural dimensions, depth, and spacing of this invention are determined by the laser scanning path, allowing for precise design and repeated processing through parameter adjustment. The morphological stability and consistency are significantly better than the stress-induced method. Finally, this invention requires only a single layer of PDMS or other curable materials, making the material system more versatile. The processing does not require complex energy field control or multilayer film dependence, thus possessing higher process controllability and engineering scalability.

[0055] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of the invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of this invention.

[0056] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for fabricating micro / nano concave structures based on ultrafast laser processing, characterized in that, Includes the following steps: The substrate material is placed on the processing platform, and the processing platform is rotated to form an inclined angle η with the X-axis plane, where η is 15° to 25°. Laser processing is then performed so that the laser is incident on the surface of the substrate material in a vertical manner, inducing the formation of a set of parallel inclined grooves. The machining platform is rotated in the opposite direction so that the tilt angle of the machining platform is the same in the X-axis plane. Laser processing is performed to induce the formation of reverse cross grooves on each tilted groove, thereby obtaining a T-shaped bidirectional groove structure. The machining platform is rotated to form an angle η with the Y-axis plane, and the laser machining method of the X-axis plane is repeated to make the grooves in the X-axis direction and the Y-axis direction orthogonally superimpose to form an array of staggered inclined grooves. The processing platform is rotated to a horizontal position so that the laser is incident vertically. The sharp corners of the staggered inclined grooves are removed and the structure is deepened to obtain the mushroom head array micro-nano structure. The top width of each mushroom head micro-nano structure is 50μm to 450μm and the bottom width is 50μm to 100μm. In the mushroom-shaped array micro-nano structure, the spacing between adjacent mushroom-shaped micro-nano structures is 100μm to 500μm, and the groove width of each mushroom-shaped micro-nano structure is 50μm to 200μm. The depth of each mushroom-shaped micro-nano structure is 200μm to 600μm, and the concave angle is 15° to 25°. During laser processing, the average laser power is 12W to 20W, the laser pulse frequency is 100kHz to 500kHz, and the laser beam wavelength is 353nm. The mushroom-shaped array micro / nano structure exhibits superhydrophobic properties, with a water droplet contact angle greater than 150° and an oil droplet contact angle greater than 150°.

2. The method for fabricating micro / nano concave structures based on ultrafast laser processing according to claim 1, characterized in that, During laser processing, reciprocating scanning is performed at a speed of 2000mm / s to 5000mm / s and a number of scans of 10 to 50.

3. The method for fabricating micro / nano concave structures based on ultrafast laser processing according to claim 1, characterized in that, The substrate material is a polydimethylsiloxane film.

4. The method for fabricating micro / nano concave structures based on ultrafast laser processing according to claim 3, characterized in that, The thickness of the matrix material is 1mm to 2mm.

Citation Information

Patent Citations

  • Anisotropic micro-nano surface based on energy adjusted femtosecond laser bionic processing

    CN106167247A

  • Preparation method of super-amphiphobic surface with inclined stepped mushroom head microcolumn structure

    CN115716928A

  • Diamond-copper composite micro-nano super-lyophilic closed concave angle evaporation heat dissipation structure, machining method and application

    CN120072770A