Large-area ultrathin perovskite single crystal and preparation method thereof
By combining etching and a low-density solvent system with mechanical thinning techniques, large-area ultrathin perovskite single crystals were successfully prepared, solving the preparation problems in existing technologies and realizing efficient and low-cost preparation of ultrathin single crystals, thereby improving photoelectric performance and production efficiency.
Patent Information
- Application Number
- CN202511662315.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-13
- Publication Date
- 2026-03-31
AI Technical Summary
Existing technologies are insufficient for efficiently preparing large-area, high-quality ultrathin perovskite single crystals. Traditional methods are time-consuming and have difficulty controlling the thickness, which limits their application in optoelectronic devices.
By etching the surface of perovskite seed crystals and using a low-density solvent to form a stable layered solution system, combined with mechanical thinning techniques, ultrathin perovskite single crystals with large lateral dimensions and moderate thickness are prepared. Area expansion is achieved by using a growth-thinning-cycle strategy.
It has achieved efficient preparation of large-area ultrathin perovskite single crystals with excellent crystal quality, reduced defect density, improved photoelectric performance and production efficiency, reduced cost, and is suitable for large-scale production.
Smart Images

Figure CN121760051A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor materials technology, and particularly relates to a large-area ultrathin perovskite single crystal and its preparation method. Background Technology
[0002] In recent years, halide perovskite materials have been considered as optoelectronic functional materials with extremely high application potential due to their advantages such as high absorption coefficient, long carrier diffusion length, and high carrier mobility. However, most current devices use perovskite polycrystalline thin films, which contain a large number of grain boundaries and pores. Defects at grain boundaries and pores can easily form carrier trapping centers, and grain boundaries are sensitive to water and oxygen, serving as channels for ion migration, thus leading to a decrease in device performance and stability. Compared to perovskite polycrystalline thin films, perovskite single crystals have no grain boundaries, and they have advantages such as higher carrier mobility, longer carrier recombination lifetime, lower defect density, and better resistance to environmental interference such as humidity and heat.
[0003] Currently, various solution-based techniques, such as solution cooling crystallization, antisolvent vapor-assisted crystallization, and reverse-temperature crystallization, have successfully grown large-size perovskite single crystals (Adv. Mater. 2018, 30, 1707314; Angew. Chem.,Int. Ed. 2016, 55, 3447; Science 2015,347,519.). However, these methods are typically time-consuming and produce relatively thick single crystals, limiting their application in vertical optoelectronic devices. To effectively control crystal thickness, spatial confinement growth techniques, which confine the perovskite precursor solution between two substrates with a micrometer-level gap, have been widely adopted. However, the lateral dimensions of single crystals prepared by this method are typically less than 2 mm, the transport of the precursor solution is slow and disordered, and the growth rate is limited, making it difficult to be compatible with large-scale optoelectronic device fabrication techniques. Therefore, developing a simple, efficient, and high-quality method for producing large-area, ultrathin perovskite single crystals is crucial for promoting the widespread application of perovskite materials in the optoelectronic field. Summary of the Invention
[0004] In view of this, the present invention provides a large-area ultrathin perovskite single crystal and its preparation method. The perovskite seed crystal surface is etched to remove the surface atomic layer, thereby activating the seed crystal surface, so that the perovskite single crystal can be rapidly nucleated and grown on the seed crystal surface, and a large-area ultrathin perovskite single crystal is obtained by using a second solvent with a density lower than that of the perovskite precursor growth solution.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows: The first aspect of this invention provides a method for preparing large-area ultrathin perovskite single crystals, comprising the following steps: S1: Obtain perovskite seed crystals; S2: Place the perovskite seed crystal from step S1 into the first solvent and heat it to perform heat treatment, thereby changing the surface microstructure. S3: Place the treated perovskite seed crystal in a glass container, add the second solvent and the perovskite precursor growth solution in sequence, place the glass container on a hot stage, and obtain a perovskite single crystal with a lateral dimension of 1-2 cm and a thickness of 2-8 mm. S4: The perovskite single crystal is fixed on a glass plate with paraffin wax, the seed crystal inside the perovskite single crystal is removed with a blade, and the perovskite single crystal is thinned to obtain a large-area ultrathin perovskite single crystal wafer. In step S3, the second solvent is immiscible with the perovskite precursor growth solution, and the density of the second solvent is less than that of the perovskite precursor growth solution.
[0006] Preferably, step S1 specifically involves: dissolving perovskite raw materials AX and BX2 in a third solvent at a preset molar ratio, and then filtering to obtain the perovskite precursor growth solution of ABX3; adding the perovskite precursor growth solution to a glass container, placing it on a hot plate, and obtaining a perovskite seed crystal with a thickness of less than 1 mm.
[0007] Preferably, the third solvent is any one or a mixture of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), γ-butyrolactone (GBL), γ-valerolactone (GVL), chlorobenzene (CB), methylamine, or acetonitrile (ACN).
[0008] Preferably, the second solvent in step S2 is any one or a mixture of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), methanol, ethanol, isopropanol, butanol or cyclohexanol; The heat treatment temperature is 20-150°C, and the treatment time is 2 min-2 h.
[0009] Preferably, a functional additive is also added to the second solvent in step S2, and the ratio of the functional additive to the second solvent is 50 g / L to 100 g / L; The functional additives are transition metal salts, metal ions, acid and basic additives, surfactants, or organic compounds.
[0010] Preferably, the transition metal salt is selected from any one or a mixture of lead bromide (PbBr2), lead acetate trihydrate (Pb(CH3COO)2・3H2O), tin chloride (SnCl2), cadmium iodide (CdI2), or manganese bromide (MnBr2); The selected metal ion is: Pb 2+ Sn 2+Cd 2+ Mn 2+ or Co 2+ ; The acid-base additives are selected from any one or a mixture of hydrobromic acid (HBr), aqueous methylamine (CH3NH2・H2O), or pyridine. The surfactant is selected from any one or a mixture of sodium dodecylbenzenesulfonate (SDBS), hexadecyltrimethylammonium bromide (CTAB), Tween-80, or Span-60; The organic compound is acetic acid or phenol.
[0011] Preferably, the second solvent in step S3 is tetradecane or n-heptane.
[0012] Preferably, the temperature of the heating table in steps S1 and S3 is 25-60°C.
[0013] Preferably, the A-site cation in the ABX3 perovskite precursor growth solution is MA. + FA + or Cs + One or more of the following, where the B-site metal ion is Pb. 2+ Sn 2+ Bi 3+ or Mn 2+ One or more of them are mixed, and the halogen anion at the X position is Cl. - ,Br - or I - One or more of the following.
[0014] Preferably, after step S4, step S5 is further included: using the ultrathin perovskite single crystal wafer as a new seed crystal, repeating steps S3 to S4 multiple times to obtain an ultra-large area ultrathin perovskite single crystal wafer with the required area and thickness.
[0015] The second aspect of the present invention also provides a large-area ultrathin perovskite single crystal prepared by the preparation method of the above embodiments.
[0016] Because of the above technical solutions, this invention has the following advantages and positive effects compared with the prior art: (1) The present invention activates the perovskite seed crystal by etching with a first solvent. Through chemical dissolution and temperature change, it removes part of the atomic layer on the surface of the seed crystal or repairs lattice defects, thereby changing the microstructure of the seed crystal surface, effectively activating the seed crystal surface, and promoting the subsequent large-area epitaxial growth of perovskite single crystals.
[0017] (2) This invention utilizes a low-density second solvent to form a stable layered solution system. The resulting physical mass transfer barrier effect effectively inhibits crystal growth in the vertical direction, thereby actively guiding the crystal to expand laterally. This method successfully overcomes the problems of easy free growth of crystals and difficulty in separately controlling thickness and lateral dimensions in traditional solution methods. It can directly grow high-quality single crystals with large lateral dimensions (1-2 cm) and moderate thickness (2-8 mm), laying the foundation for subsequent processing.
[0018] (3) By combining the mechanical post-processing strategy of "precise removal of internal seed crystals with blades" with "gradual thinning with sandpaper", the original seed crystals that serve as initial nucleation points can be completely removed, thus avoiding their impact on the final device performance as a defect source. This method is simple to operate, low in cost, and can produce ultrathin perovskite single crystal wafers with smooth surfaces, complete structures, and uniform thickness, with crystal quality far exceeding that of polycrystalline thin films.
[0019] (4) The “growth-thinning-cycle” strategy designed in this invention cleverly uses the ultrathin wafer obtained in the previous round as a new generation of seed crystal, realizing iterative amplification of the single crystal area. This fundamentally breaks through the physical limit of crystal size in a single growth, providing a general, controllable and efficient technical route for preparing inch-scale or even larger area ultrathin single crystals.
[0020] (5) The large-area ultrathin single crystals prepared by the above method exhibit significantly reduced carrier recombination rate and excellent photoelectric properties due to their low internal defect density, absence of grain boundaries, and uniform structure. At the same time, the entire process is mild and highly controllable, which significantly reduces the probability of cracks and breakage of single crystals during growth and processing, thereby greatly improving the overall yield and production efficiency of the products.
[0021] (6) The solvents (such as tetradecane, n-heptane, etc.) and processing methods (such as blades, sandpaper) used in this invention are all common or low-cost materials, which do not require complex vacuum equipment or expensive substrates, effectively reducing the cost of raw materials and equipment. The process route is simple, easy to repeat and scale up, and has good compatibility with existing semiconductor processes. Attached Figure Description
[0022] Figure 1 Optical images of the large-area ultrathin MAPbBr3 perovskite single crystal wafer obtained in Example 1 of the present invention; Figure 2 Here is a SEM image of the large-area ultrathin MAPbBr3 perovskite single crystal wafer obtained in Example 1 of this invention; Figure 3 This is a cross-sectional image of the MAPbBr3 perovskite single crystal wafer obtained in Example 1 of the present invention; Figure 4The X-ray diffraction pattern of the MAPbBr3 perovskite single crystal wafer obtained in Example 1 of this invention; Figure 5 The photoluminescence curve of the MAPbBr3 perovskite single crystal wafer obtained in Example 1 of this invention; Figure 6 The fluorescence lifetime curve of the MAPbBr3 perovskite single crystal wafer obtained in Example 1 of this invention; Figure 7 This is an optical image of the MAPbBr3 perovskite single crystal obtained in Comparative Example 1 of this invention. Detailed Implementation
[0023] The following detailed description, in conjunction with the accompanying drawings and specific embodiments, provides a further detailed explanation of the large-area ultrathin perovskite single crystal and its preparation method proposed in this invention. The advantages and features of this invention will become clearer from the following description.
[0024] Example 1 S1: Dissolve perovskite raw materials methylamine hydrobromide (MABr) and lead bromide (PbBr2) in N,N-dimethylformamide (DMF) at a molar ratio of 1:1, and then filter to obtain a perovskite precursor growth solution of MAPbBr3. S2: Add a small amount of perovskite precursor solution to a petri dish and place it on a constant temperature hot plate at 30°C for 12 hours to obtain perovskite seed crystals with three-dimensional dimensions all less than 1 mm. S3: Select methanol as the solvent, place the perovskite seed crystal in methanol, and place it in a hydrothermal reactor and heat it to 80°C for 20 minutes. S4: Place the treated perovskite seed crystal in a glass container, add tetradecane and perovskite precursor growth solution in sequence, place the glass container on a constant temperature hot stage at 42℃ for 12 hours to obtain a perovskite single crystal with a lateral dimension of 1-2cm and a thickness of 2-8mm. S5: Fix the perovskite single crystal onto a glass plate with paraffin wax, remove the seed crystal inside the perovskite single crystal with a blade, and thin the perovskite single crystal with sandpaper to obtain an ultra-thin perovskite single crystal wafer with a thickness adjustable from 1μm to 2mm. S6: Use the ultrathin perovskite single crystal wafer as the seed crystal for the next growth, and repeat steps S4-S5 once to obtain an ultra-large area ultrathin perovskite single crystal wafer with a thickness of 3-4cm and 1μm to 2mm. Figure 1 and Figure 2 These are optical and scanning electron micrographs of the obtained MAPbBr3 perovskite single crystal wafer, respectively. Figure 2The optical images show that the single crystal has a good morphology, with a smooth and flat surface and clear crystal edges, indicating that the crystal achieved good uniformity and integrity during growth. Furthermore, the single crystal wafer has high transparency, indicating fewer internal defects and excellent optical quality. Figure 2 Scanning electron microscope (SEM) images further confirmed the microstructure of the single crystal. The SEM images revealed the crystal's high surface smoothness and density, with no obvious visible cracks or defects, indicating that the fabrication process performed excellently in controlling the crystallinity and morphology of the crystal. Figure 3 The image shows a cross-section of the obtained MAPbBr3 perovskite single-crystal wafer, with a thickness of approximately 17 μm, demonstrating that this method can achieve precisely controllable thickness dimensions. This micrometer-level thickness not only provides an ideal basis for dimensional control in the subsequent integration of optoelectronic devices but also ensures their advantages in light absorption and charge transport.
[0025] Figure 4 The X-ray diffraction (XRD) pattern of the obtained MAPbBr3 perovskite single crystal is shown. Strong and sharp diffraction peaks are clearly observed in the XRD pattern, corresponding to the (100), (200), and (300) crystal planes of the MAPbBr3 single crystal, indicating a highly ordered crystal structure. The narrow width and high intensity of the peaks further indicate that the single crystal has a very high crystallinity and almost no obvious defects or impurities within the lattice. This superior crystal quality provides a strong structural guarantee for the optoelectronic properties of the single crystal. Figure 5 The photoluminescence (PL) spectrum of MAPbBr3 perovskite single crystal is shown. The main peak of the PL curve is located in a narrow wavelength range, indicating that the single crystal can effectively generate radiative recombination under photoexcitation, exhibiting excellent luminescence performance. In addition, the narrow peak width of the PL curve reflects that the single crystal has a low defect state density and a high-quality crystal structure, which is beneficial to reducing nonradiative recombination processes and improving photoelectric conversion efficiency. Figure 6 The fluorescence lifetime curve of the MAPbBr3 perovskite single crystal is shown, revealing the recombination dynamics of photogenerated carriers in the single crystal. The carrier lifetime of the single crystal can be determined by fitting the fluorescence decay curve. A longer fluorescence lifetime indicates less non-radiative recombination in the single crystal and a longer transport and diffusion distance for photogenerated carriers, which is crucial for improving the performance of optoelectronic devices. Combining the results of photoluminescence and fluorescence lifetime, it can be inferred that the perovskite single crystal prepared by this method has excellent application potential in photovoltaic and light-emitting devices.
[0026] Example 2 S1: Dissolve perovskite raw materials methylamine hydrobromide (MABr) and lead bromide (PbBr2) in N,N-dimethylformamide (DMF) at a molar ratio of 1:1, and then filter to obtain a perovskite precursor growth solution of MAPbBr3. S2: Add a small amount of perovskite precursor solution to a petri dish and place it on a constant temperature hot plate at 30°C for 12 hours to obtain perovskite seed crystals with three-dimensional dimensions all less than 1 mm. S3: Select ethanol as the solvent, place the perovskite seed crystal in ethanol, and place it in a hydrothermal reactor to heat to 100°C and maintain for 20 minutes. S4: Place the treated perovskite seed crystal in a glass container, add n-heptane and perovskite precursor growth solution in sequence, place the glass container on a constant temperature hot stage at 52℃ for 12 hours to obtain a perovskite single crystal with a thickness of 1-2cm. S5: The perovskite single crystal is fixed onto a glass plate with paraffin wax. The seed crystal inside the perovskite single crystal is removed with a blade, and the perovskite single crystal is thinned with sandpaper to obtain an ultra-thin perovskite single crystal wafer with a thickness adjustable from 1μm to 2mm.
[0027] Comparative Example 1. Dissolve perovskite raw materials methylamine hydrobromide (MABr) and lead bromide (PbBr2) in N,N-dimethylformamide (DMF) at a molar ratio of 1:1, and then filter to obtain a perovskite precursor growth solution with a concentration of 1.85 M MAPbBr3.
[0028] 2. Add a small amount of perovskite precursor solution to a petri dish and place it on a constant temperature hot plate at 30°C for 12 hours to obtain perovskite seed crystals with three-dimensional dimensions all less than 1 mm.
[0029] 3. Place the perovskite seed crystal in a glass bottle, add the perovskite precursor solution, and place it in an oven. The initial temperature is 25℃, and the temperature is increased to 60℃ at a rate of 2℃ per day. Perovskite single crystals with a size of 2-3cm can be obtained in about 18 days.
[0030] Figure 7 Optical images of the obtained perovskite single crystals reveal an irregular crystal morphology. This is due to multiple interfering factors during the long growth process, such as fluctuations in solute concentration in the solution, crystal fragmentation, and dust. These factors cause varying growth rates in different directions, resulting in irregular crystal morphology. Irregular crystals often possess internal stress, making them more susceptible to cracking or breakage under mechanical stress, which negatively impacts the material's processing and stability.
[0031] The embodiments of the present invention have been described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments. Even if various changes are made to the present invention, if these changes fall within the scope of the claims of the present invention and their equivalents, they shall still fall within the protection scope of the present invention.
Claims
1. A method for preparing a large-area ultrathin perovskite single crystal, characterized in that, The method comprises the following steps: S1: obtaining a perovskite seed crystal; S2: placing the perovskite seed crystal of step S1 into a first solvent and heating to perform heat treatment on the perovskite seed crystal to change the surface microstructure; S3: placing the treated perovskite seed crystal into a glass container, sequentially adding a second solvent and a perovskite precursor growth solution, and placing the glass container on a hot stage to obtain a perovskite single crystal with a lateral size of 1-2 cm and a thickness of 2-8 mm; S4: fixing the perovskite single crystal on a glass sheet with paraffin, removing the seed crystal inside the perovskite single crystal with a blade, and thinning the perovskite single crystal to obtain a large-area ultrathin perovskite single crystal wafer; The perovskite precursor growth solution is prepared by dissolving perovskite raw materials in a third solvent; the second solvent in step S2 is immiscible with the perovskite precursor growth solution, and the density of the first solvent is less than that of the perovskite precursor growth solution. 2.The method of claim 1, wherein the method further comprises, after the step of forming the perovskite single crystal layer, a step of forming a protective layer on the perovskite single crystal layer. The specific steps of step S1 are: dissolving perovskite raw materials AX and BX2 in a third solvent at a predetermined molar ratio, and then filtering to obtain the perovskite precursor growth solution of ABX3; adding the perovskite precursor growth solution in a glass container and placing it on a hot stage to obtain a perovskite seed crystal with a three-dimensional size of less than 1 mm and a regular shape.
3. The method of producing a large-area perovskite single crystal according to claim 1 or 2, wherein The third solvent is any one or a mixture of multiple of N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, γ-valerolactone, chlorobenzene, methylamine, or acetonitrile. 4.The method of claim 1, wherein the method further comprises a step of removing the substrate. The second solvent in step S2 is any one or a mixture of N,N-dimethylformamide, dimethyl sulfoxide, methanol, ethanol, isopropanol, butanol, or cyclohexanol; The temperature of the heat treatment is 20-150°C, and the treatment time is 2 min-2 h. 5.The method of claim 1, wherein the method further comprises: depositing a perovskite precursor solution on the substrate; and annealing the perovskite precursor solution to form the perovskite single crystal. A functional additive is also added to the second solvent in step S2, and the ratio of the functional additive to the second solvent is 50 g / L to 100 g / L; The functional additive is a transition metal salt, a metal ion, an acid-base additive, a surfactant, or an organic compound. 6.The method of claim 1, wherein the method further comprises: depositing a perovskite precursor solution on the substrate; and annealing the perovskite precursor solution to form the perovskite single crystal. The second solvent in step S3 is tetradecane or n-heptane.
7. The method for preparing large-area ultrathin perovskite single crystals according to claim 2, characterized in that, The temperature of the hot stage in steps S1 and S3 is 25-60°C. 8.The method of claim 2, wherein the method further comprises, after the step of forming the perovskite single crystal layer, a step of forming a protective layer on the perovskite single crystal layer. A is one or more of MA + , FA + , or Cs + mixed, B is one or more of Pb 2+ , Sn 2+ , Bi 3+ , or Mn 2+ mixed, and X is one or more of Cl - , Br - , or I - . 9.The method of claim 2, wherein the perovskite single crystal is a large-area and ultra-thin perovskite single crystal. After step S4, further S5: using the ultrathin perovskite single crystal wafer obtained in step S4 as a new seed crystal, repeating steps S3 to S4 one or more times to obtain a larger-area ultrathin perovskite single crystal.
10. A large-area ultrathin perovskite single crystal prepared by the method of any one of claims 1-9.