Carrier supported multi-metal sulfide state nickel-based catalyst as well as preparation method and application thereof

By preparing a supported multimetallic sulfide nickel-based catalyst, the problems of high cost, low activity, and insufficient stability of existing catalysts in the preparation of long-chain olefins were solved, achieving high selectivity and long lifespan catalytic performance, suitable for bio-based fatty acid decarbonylation-dehydration reactions.

CN121775870APending Publication Date: 2026-04-03FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610028068.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-09
Publication Date
2026-04-03

AI Technical Summary

Technical Problem

Existing catalysts for the preparation of long-chain olefins suffer from problems such as high cost, low activity, poor selectivity and insufficient stability. In particular, when processing bio-based fatty acids or their derivatives, there is a lack of suitable multi-metallic sulfide nickel-based catalysts and their efficient preparation processes.

Method used

Using a supported multimetallic sulfide-state nickel-based catalyst, a Ni-MS ternary coordination or Ni-SM bridging structure is formed through multimetallic synergistic effect and specific morphology control. The preparation method includes pretreatment, loading, calcination, sulfidation and activation steps to form sheet-like or petal-like nanostructures, which are suitable for bio-based fatty acid decarbonylation-dehydration reactions.

Benefits of technology

It significantly improves catalytic activity and olefin selectivity, with a target long-chain olefin selectivity of over 90%. The catalyst exhibits excellent stability, with a decay rate of less than 5% after 100 hours of continuous operation, reducing preparation costs and making it suitable for various renewable resources.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a carrier supported multi-metal sulfide state nickel-based catalyst as well as a preparation method and application thereof. The catalyst is composed of a porous carrier loaded NixMySz active phase, M is a combination of at least one metal element of Co, Fe, Cu, Zn or Mn, multiple metal components form a synergistic structure in the vulcanization process, and through construction of Ni-S-M bonds, pinning effect generation and electron interaction, controllable adjustment of the sulfide structure is achieved, and the stability of the catalyst is improved. The catalyst is obtained by loading a nickel-second metal precursor on a porous carrier, roasting to form an oxide, vulcanizing in a sulfur-containing atmosphere, and activating. The obtained catalyst has an adjustable Ni: M molar ratio, a sheet-like or petal-like nanostructure and high-density sulfur defects. The catalyst is suitable for decarbonylation-dehydration reaction of bio-based fatty acid or derivatives thereof, and can efficiently convert C10-C20 fatty acid, methyl ester or ethyl ester thereof, and animal and vegetable oil or waste oil containing the components into long-chain olefin at 200-350 DEG C under 0.1-3 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalyst technology, specifically to a supported multimetallic sulfide nickel-based catalyst and its preparation method, as well as the application of this catalyst in the decarbonylation-dehydration reaction of bio-based fatty acids or their derivatives to prepare long-chain olefins. Background Technology

[0002] Long-chain olefins are key raw materials for the synthesis of surfactants, lubricating oil base oils, plasticizers, and specialty polymers, and are widely used in several strategic industries such as fine chemicals, materials manufacturing, and new energy, with consistently stable market demand. Currently, the industrial production of long-chain olefins mainly relies on fossil resource routes such as naphtha cracking, Fischer-Tropsch synthesis, and alkane dehydrogenation. However, these processes have significant drawbacks: dispersed carbon chain distribution in the products, low selectivity for target products, high energy consumption, and complete dependence on non-renewable petroleum resources. Driven by the "dual carbon" goals (carbon reduction and emission reduction), traditional fossil routes can no longer meet the demands of green and sustainable industrial development. Developing long-chain olefin production technologies based on renewable resources has become a core industry demand.

[0003] Renewable resources such as animal and vegetable oils and waste cooking oil are rich in C10-C20 fatty acids and their esters. Their molecular structures naturally possess long-chain alkane skeletons, which can be directionally converted into target long-chain olefins simply through a decarbonylation-dehydration reaction. This makes them ideal renewable carbon sources to replace fossil resources. Compared to traditional fossil routes, the decarbonylation-dehydration method for fatty acids or their derivatives has advantages such as shorter reaction steps, lower theoretical hydrogen consumption, and a direct carbon conversion pathway. However, the key bottleneck for its industrial application lies in the insufficient performance of the catalyst system.

[0004] The catalysts currently used for this reaction mainly include noble metal catalysts (such as Pd and Pt) and transition metal oxide catalysts. Although noble metal catalysts have high catalytic activity, they suffer from problems such as high cost, susceptibility to over-hydrogenation side reactions, and easy deactivation after long-term use, making it difficult to meet the cost control and stability requirements for large-scale industrial applications. Transition metal oxide catalysts, on the other hand, generally suffer from defects such as poor selectivity for target olefins, insufficient dispersion of the active phase, and easy agglomeration and deactivation at high temperatures. Furthermore, their stability decreases further when processing actual raw materials containing water, unsaturated bonds, or trace impurities (such as waste oils).

[0005] Furthermore, the active phase structure of existing catalysts is mostly simple particulate, lacking precise control over the morphology of the active phase. This results in insufficient exposure of active sites and weak metal-support interface interactions, further limiting the improvement of catalytic performance. Currently, there is no catalyst in the industry that can simultaneously solve the three core problems of "high cost, low selectivity, and poor stability," especially lacking sulfide-based nickel catalysts with specific hierarchical structures, controllable stoichiometry, and compatibility with complex renewable feedstock systems, as well as their efficient preparation processes.

[0006] Therefore, developing a catalyst that is low in cost, has high catalytic activity, excellent olefin selectivity, strong structural stability, and is suitable for the conversion of bio-based fatty acids or their derivatives is of great significance for promoting the green and sustainable development of the long-chain olefin industry. Summary of the Invention

[0007] To address the problems of existing technologies in the preparation of long-chain olefins, such as reliance on fossil resources, high cost, low activity, poor selectivity, and insufficient stability of catalysts, the present invention aims to provide a supported multi-metal sulfide nickel-based catalyst. This catalyst achieves simultaneous improvement in catalytic activity, olefin selectivity, and structural stability through multi-metal synergistic effects and specific morphology regulation. The invention also provides a method for preparing this catalyst, which is simple, highly controllable, and suitable for industrial production.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A supported multimetallic sulfide nickel-based catalyst, characterized in that it comprises a porous support and a multimetallic sulfide active phase supported on the support; the chemical composition of the multimetallic sulfide active phase is represented as Ni. x M y S z Where M is a combination of at least one metallic element selected from Co, Fe, Cu, Zn, and Mn; the Ni x M y S z The molar ratio of Ni to M in the active phase is 0.1–20, and the molar ratio of (Ni+M):S is 0.45–1.5. The active phase has a plate-like or petal-like nanostructure and exhibits a Ni-M synergistic configuration, including Ni-MS ternary coordination, Ni-SM bridging structures, or multi-center S bridging between M elements, forming multi-metallic active centers with tunable electronic structures. The plate-like nanostructure has a thickness of 5–10 nm, and the petal-like nanostructure has 3–5 layers.

[0009] Preferably, the porous support is a composite support composed of one or more of mesoporous carbon, activated carbon, coconut shell carbon, graphitized carbon, silica, and alumina. The porous support possesses a high specific surface area and a suitable pore structure, providing support for the uniform dispersion of the active phase while promoting the mass transfer process between reactants and products.

[0010] Preferably, the specific surface area of ​​the catalyst is 200–1000 m². 2 / g, pore volume 0.3~2.5cm 3 The support has a mesopore size of 2–50 nm. This structural parameter ensures sufficient exposure of the active phase while avoiding product diffusion restriction.

[0011] Preferably, based on the total mass of the catalyst, the total mass percentage of the metal elements Ni and M is 2% to 35%. This content range can balance the number and dispersion of active sites and avoid metal particle agglomeration.

[0012] A method for preparing a supported nickel-sulfide catalyst includes the following steps: S1. Pretreatment: The porous carrier is subjected to heat treatment at a temperature of 280-350°C for 2-3 hours to remove impurities and moisture from the surface of the carrier and enhance the interaction between the carrier and the precursor. S2. Loading: A precursor solution containing a Ni source and at least two M metal sources is loaded onto a pretreated support using at least one of the following methods: impregnation, co-precipitation, solvothermal or hydrothermal, to obtain a support-precursor composite. S3. Calcination: The composite obtained in step S2 is calcined at 280-550°C for 1-6 hours in a nitrogen-containing atmosphere to decompose the precursor and convert it into a polymetallic oxide precursor. S4. Sulfidation: The polymetallic oxide precursor obtained in step S3 is sulfided in a sulfur-containing atmosphere at 200–420°C for 1–10 hours to form polymetallic sulfide Ni. x M y S z ; S5. Activation: In a pure H2 atmosphere, the product after sulfidation in step S4 is activated at 250-420℃ for 0.5-1.5h to obtain the desired catalyst.

[0013] Preferably, in step S2, the precursor is selected from nitrates, acetates, organometallic complexes, or nickel-M layered double hydroxides Ni-M-LDH, and a structure directing agent accounting for 1% to 10% of the total mass of the precursor is added during the loading process to form a plate-like, petal-like, or mesoporously interconnected multimetallic sulfide structure; the structure directing agent is at least one of hexadecyltrimethylammonium bromide, polyethylene glycol, or polyvinylpyrrolidone.

[0014] Preferably, in step S4, the sulfur-containing atmosphere is a combination of H2S and H2 or sulfur vapor or CS2, wherein the volume fraction of H2S is 0.1-10%.

[0015] Preferably, steps S4 and S5 employ a segmented heating method to regulate the Ni-M dispersion and interaction, as detailed below: In a sulfur-containing atmosphere, a first-stage sulfidation treatment is carried out at 200–350℃ for 0.5–5 h, followed by a second-stage sulfidation treatment at 350–420℃ for 0.5–5 h. After sulfidation, the atmosphere is switched to pure H2, and a reduction activation treatment is carried out at 250–420℃ for 0.5–1.5 h. This method can precisely control the Ni-M dispersion and interaction, and optimize the multi-metal synergistic structure.

[0016] The application of a supported sulfide-based nickel-based catalyst in the preparation of long-chain olefins includes the following steps: under the conditions of a reaction temperature of 200-350℃ and a hydrogen pressure of 0.1-3MPa, bio-based fatty acids or their derivatives are contacted with the catalyst to undergo a decarbonylation-dehydration reaction to generate long-chain olefins.

[0017] Preferably, the bio-based fatty acid or its derivative is a fatty acid with 10-20 carbon atoms, a fatty acid methyl ester with 10-20 carbon atoms, a fatty acid ethyl ester with 10-20 carbon atoms, or at least one of animal or vegetable oils or waste oils containing the above components. These raw materials are widely available, renewable, and have a high degree of matching between their carbon chain structure and the target long-chain olefin, resulting in excellent conversion efficiency.

[0018] Compared with the prior art, the technical solution of the present invention has the following advantages: A. Synergistic effect of multiple metals and excellent catalytic performance: This invention introduces at least one M metal element to form NixMySz active phase with Ni, and constructs synergistic configurations such as Ni-MS ternary coordination and Ni-SM bridging. The electronic regulation between multiple metals can significantly enhance the C=C bond formation ability, while effectively suppressing deep hydrogenation side reactions, greatly improving the rate of fatty acid decarbonylation-dehydration reaction and olefin selectivity. The selectivity of target long-chain olefins can reach more than 90%.

[0019] B. Stable structure and long cycle life: In the multi-metal sulfide structure, a "pinning effect" is formed between different metal atoms, effectively enhancing the stability of the sulfide lattice and reducing metal particle agglomeration and sulfur loss under high-temperature reaction conditions. Simultaneously, the plate-like or petal-like nano-morphology and high specific surface area structure improve the catalyst's tolerance to carbon deposition. Tests show that after 100 hours of continuous operation, the catalyst of this invention exhibits a catalytic activity decay rate of less than 5%, and after five cycles, the selectivity retention rate remains above 85%, significantly superior to existing catalysts.

[0020] C. Controllable preparation process and low cost: The present invention uses conventional impregnation or co-precipitation methods to support precursors. By adding specific structure-directing agents, the morphology of the active phase can be precisely controlled to be plate-like or petal-like. The process is simple, highly controllable, and suitable for industrial mass production. The catalyst uses Ni as the main active component and is supplemented with non-precious metal M element, which avoids the use of precious metals and greatly reduces the preparation cost.

[0021] D. Wide range of applications and green sustainability: The catalyst of this invention is applicable to a variety of bio-based raw materials such as C10-C20 fatty acids, their methyl / ethyl esters, animal and vegetable oils, and waste oils. The reaction conditions are mild (200-350℃, 0.1-3MPa), realizing the efficient conversion of renewable resources into high-value-added long-chain olefins, reducing dependence on fossil resources, and conforming to the "dual carbon" strategic goal and the trend of green chemical development. Detailed Implementation

[0022] This invention can be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the inventive concept to those skilled in the art. All other embodiments derived by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention. Example 1

[0023] This embodiment discloses the preparation and application of a supported multimetallic sulfide nickel-based catalyst. The preparation method includes the following steps: S1. Pretreatment: Take 5g of mesoporous carbon support, place it in a tube furnace, heat treat it at 300℃ for 2h under nitrogen atmosphere, and cool it to room temperature for later use. S2, Loading: Weigh 0.97 g of nickel nitrate (Ni(NO3)2・6H2O) and 1.16 g of cobalt nitrate (Co(NO3)2・6H2O) (molar ratio Ni:Co molar ratio = 1:1), dissolve in 50 mL of deionized water, add 0.5 g of hexadecyltrimethylammonium bromide (accounting for 5% of the total mass of the precursor), stir until completely dissolved to obtain a precursor solution; immerse the pretreated mesoporous carbon support in the above solution, impregnate at room temperature for 12 h, and then dry at 80 °C for 10 h to obtain the support-precursor composite; S3. Calcination: The composite was placed in a tube furnace and calcined at 400°C for 3 hours under a nitrogen atmosphere, and then naturally cooled to room temperature to obtain a multi-metal oxide precursor (total metal mass percentage 10%). S4. Sulfation: The oxide precursor is placed in a fixed-bed reactor and H2S / H2 mixed gas (H2S volume fraction 5%) is introduced. Sulfation is first carried out at 280℃ for 0.5h, and then the temperature is raised to 380℃ to continue sulfation for 2h. The gas flow rate during sulfation is 50mL / min. S5. Activation: After sulfidation, switch to pure H2 atmosphere and activate at 350℃ for 1 hour. After cooling, the target catalyst Cat-1 is obtained.

[0024] Characterization revealed a (Ni+M) / S surface molar ratio of 0.8, indicating the presence of a Ni-MS ternary coordination structure. The catalyst exhibited a specific surface area of ​​770 m². 2 / g, pore volume 2.0cm 3 / g, with a mesopore diameter of 15nm; the nickel sulfide active phase has a sheet-like nano-morphology with a thickness of approximately 5–10nm. Catalyst applications:

[0025] 5 g of Cat-1 was placed in a fixed-bed reactor. Palmitic acid (C16 fatty acid) was used as the raw material, and n-tetradecane was used as the solvent. The raw material concentration was 30%. The decarbonylation-dehydration reaction was carried out at a reaction temperature of 300℃, a hydrogen pressure of 2 MPa, and a raw material space velocity of 0.5 h⁻¹. After the reaction continued for 24 h, the products were analyzed by gas chromatography: the conversion rate of palmitic acid was 98.5%, the selectivity for long-chain olefins was 93.3%, and the conversion rate remained at 95% after continuous operation for 100 h. No obvious by-products were generated. Example 2

[0026] This embodiment discloses the preparation and application of a supported multimetallic sulfide nickel-based catalyst. The preparation method includes the following steps: S1. Pretreatment: Take 5g of alumina carrier, heat treat it at 350℃ for 3h, and cool it for later use. S2. Loading: Weigh 0.10 g of nickel nitrate (Ni(NO3)2・6H2O), 0.42 g of ferric nitrate (Fe(NO3)3・9H2O), and 0.32 g of zinc nitrate (Zn(NO3)2・6H2O) (molar ratio Ni:Fe:Zn=0.2:1:1, Ni:M=0.1), and dissolve them in 40 mL of ethanol; add 0.1 g of polyethylene glycol (1% of the total precursor mass), stir evenly, and then load it onto activated carbon by co-precipitation. Adjust the pH to 8.0, let it stand for 6 h, filter it, and dry it at 100 °C for 8 h (total metal mass percentage 2%). S3. Calcination: Calcination at 280℃ for 6 hours under an oxygen-containing atmosphere, followed by cooling to obtain the oxide precursor; S4. Sulfurization: Sulfur vapor (10% H2S volume fraction) is introduced and sulfurized at 200℃ for 1 hour, then the temperature is raised to 350℃ and sulfurized for 3 hours. S5. Activation: Activate at 250℃ for 0.5h under a pure H2 atmosphere to obtain catalyst Cat-2.

[0027] Characterization revealed that the (Ni+M) / S surface molar ratio was 0.45, indicating the presence of a Ni-MS ternary coordination structure. The catalyst had a specific surface area of ​​710 m². 2 / g, pore volume 1.8cm 3 / g, mesopore diameter 10nm. Catalyst applications:

[0028] 5g of Cat-2 was placed in a fixed-bed reactor. Decanoic acid (C10 fatty acid) was used as the raw material and n-tetradecane was used as the solvent. The raw material mass concentration was 30%. The reaction temperature was 200℃, the hydrogen pressure was 0.1MPa, and the space velocity was 0.3h⁻¹. After 24h of reaction, the conversion rate of decanoic acid was 92.2%, and the selectivity of C9 long-chain olefins was 90.1%. After continuous operation for 100h, the conversion rate was still above 90%. Example 3

[0029] This embodiment discloses the preparation and application of a supported multimetallic sulfide nickel-based catalyst. The preparation method includes the following steps: S1. Pretreatment: Take 5g of alumina carrier, heat treat it at 280℃ for 2h in air atmosphere, and cool it for later use. S2, Loading: Weigh 5.80 g of nickel acetate (Ni(CH3COO)2・4H2O) and 0.74 g of manganese nitrate (Mn(NO3)2・4H2O) (molar ratio Ni:Mn=20:1), dissolve in 50 mL of deionized water; add 1.2 g of polyvinylpyrrolidone (accounting for 10% of the total mass of the precursor), load onto alumina by impregnation, and dry at 80 °C for 12 h (total metal mass percentage 35%). S3. Calcination: Calcination at 550℃ for 1 hour under an oxygen-containing atmosphere, followed by cooling to obtain the oxide precursor; S4. Vulcanization: Introduce H2S / H2 mixed gas (H2S volume fraction 10%), vulcanize at 350℃ for 5 hours, then raise the temperature to 420℃ and vulcanize for 5 hours (total vulcanization time 10 hours). S5. Activation: Activate at 420℃ for 1.5h under a pure H2 atmosphere, and then cool to obtain catalyst Cat-3.

[0030] Characterization revealed that the (Ni+M) / S surface molar ratio was 1.5, indicating the presence of a Ni-MS ternary coordination structure. The catalyst had a specific surface area of ​​680 m². 2 / g, pore volume 2.1cm 3 / g, mesopore diameter 20nm.

[0031] 5g of Cat-3 was placed in a fixed-bed reactor. Using arachidic acid (C20 fatty acid) as raw material and n-tetradecane as solvent, the raw material mass concentration was 30%. The reaction temperature was 350℃, the hydrogen pressure was 3MPa, and the space velocity was 0.6h⁻¹. After 24h of reaction, the conversion rate of arachidic acid was 97.8%, the selectivity of long-chain olefins was 92.7%, and the selectivity was still 89.3% after 5 cycles. Example 4

[0032] This embodiment discloses the preparation and application of a supported multimetallic sulfide nickel-based catalyst. The preparation method includes the following steps: S1. Pretreatment: Take 5g of activated carbon-alumina composite carrier (mass ratio 2:1), heat treat at 300℃ for 2h under nitrogen atmosphere, and cool for later use.

[0033] S2, Loading: Weigh 1.31 g of nickel acetate (Ni(CH3COO)2・4H2O) and 1.16 g of cobalt nitrate (Co(NO3)2・6H2O) (molar ratio Ni:Co=2:1), dissolve in 40 mL of ethanol; add 0.2 g of polyvinylpyrrolidone (3% of the total mass of the precursor), load onto the composite carrier by coprecipitation, filter, and dry at 100 °C for 8 h (total metal mass percentage 8%).

[0034] S3. Calcination: Calcination at 380℃ for 3 hours under nitrogen atmosphere, followed by cooling to obtain oxide precursor.

[0035] S4. Vulcanization: Introduce a mixture of H2S / CS2 gas (8% by volume), vulcanize at 280℃ for 5 hours, then raise the temperature to 400℃ and vulcanize for 0.5 hours (total vulcanization time 5.5 hours).

[0036] S5. Activation: Activate at 350℃ for 1 hour under a pure H2 atmosphere, and then cool to obtain catalyst Cat-4.

[0037] Characterization revealed a (Ni+M) / S surface molar ratio of 0.9, the presence of a Ni-SM bridging structure, and a specific surface area of ​​730 m². 2 / g, pore volume 1.9cm 3 / g, with a mesopore size of 18nm; the nickel sulfide active phase has a petal-like nano-morphology and 4 layers. Catalyst applications:

[0038] 5g of Cat-4 was placed in a fixed-bed reactor. Waste catering oil (mainly containing C16-C18 fatty acid esters) was used as raw material, and n-tetradecane was used as solvent. The raw material mass concentration was 30%. The reaction temperature was 300℃, the hydrogen pressure was 1.5MPa, and the space velocity was 0.5h⁻¹. After 24 hours of reaction, the raw material conversion rate was 94.9%, and the total selectivity of long-chain olefins was 91.3%. After 100 hours of continuous operation, the conversion rate was still above 90%, and the selectivity was still 88.7% after 5 cycles. Example 5

[0039] This embodiment discloses the preparation and application of a supported multimetallic sulfide nickel-based catalyst. The preparation method includes the following steps: S1. Pretreatment: Take 5g of mesoporous carbon support, heat treat it at 320℃ for 2.5h under nitrogen atmosphere, and cool it for later use; S2. Loading: Weigh 1.83 g of nickel nitrate (Ni(NO3)2・6H2O) and 2.18 g of cobalt nitrate (Co(NO3)2・6H2O) (molar ratio Ni:Co=3:2), dissolve in 50 mL of deionized water, and stir until homogeneous to obtain a metal salt solution; add hexamethylenetetramine to the above solution to adjust the pH to 9.0, heat to 60 °C and react for 4 h to prepare Ni-Co layered double hydroxide (Ni-Co-LDH) precursor; add 0.4 g of hexadecyltrimethylammonium bromide (accounting for 4% of the total mass of the precursor), stir until homogeneous, load onto the pretreated mesoporous carbon support, let stand at 60 °C for 5 h, filter, and dry at 90 °C for 10 h (total metal mass percentage 12%). S3. Calcination: Calcination at 420℃ for 2.5h under nitrogen atmosphere, followed by cooling to obtain oxide precursor; S4. Vulcanization: Introduce a mixed gas of H2S / H2 (H2S volume fraction 6%), vulcanize at 300℃ for 2 hours, then raise the temperature to 390℃ and vulcanize for 1.5 hours (total vulcanization time 3.5 hours). S5. Activation: Activate at 360℃ for 1 hour under a pure H2 atmosphere, and then cool to obtain catalyst Cat-5.

[0040] Characterization revealed a (Ni+M) / S surface molar ratio of 0.85, indicating the presence of a Ni-MS ternary coordination structure. The catalyst exhibits a specific surface area of ​​750 m². 2 / g, pore volume 2.2cm 3 / g, with a mesopore diameter of 16nm; the nickel sulfide active phase has a petal-like nano-morphology with 3 to 4 layers. Catalyst applications:

[0041] 5g of Cat-5 was placed in a fixed-bed reactor. Methyl palmitate (C16 fatty acid methyl ester) was used as the raw material, and n-tetradecane was used as the solvent. The raw material mass concentration was 30%. The reaction temperature was 310℃, the hydrogen pressure was 3MPa, and the space velocity was 0.4h⁻¹. After 24 hours of reaction, the conversion rate of methyl palmitate was 96.7%, and the selectivity of long-chain olefins was 92.1%. After 100 hours of continuous operation, the conversion rate was still above 93%. After 5 cycles, the selectivity reached 89.5%. Comparative Example 1

[0042] A conventional NiO / Al2O3 catalyst (without sulfurization treatment, Ni content 10 wt%) was used to catalyze the decarbonylation-dehydration reaction of palmitic acid under the application conditions of Example 1. The results showed a palmitic acid conversion rate of 82.3%, a long-chain olefin selectivity of 61.6%, and a yield of only 49%. Furthermore, the catalyst exhibited significant agglomeration after the reaction, indicating poor stability.

[0043] Any aspects not described in this invention are applicable to existing technologies.

[0044] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A supported multimetallic sulfide-based nickel-based catalyst, characterized in that: It includes a porous support and a multi-metal sulfide active phase supported on the support; the chemical composition of the multi-metal sulfide active phase is represented as Ni. x M y S z Where M is a combination of at least one metallic element selected from Co, Fe, Cu, Zn, and Mn; the Ni x M y S z The molar ratio of Ni to M in the active phase is 0.1 to 20, and the molar ratio of (Ni+M):S is 0.45 to 1.5; the active phase has a plate-like or petal-like nanostructure.

2. The catalyst according to claim 1, characterized in that: The porous carrier is a composite carrier composed of one or more of the following: mesoporous carbon, activated carbon, coconut shell carbon, graphitized carbon, silicon dioxide, and alumina.

3. The catalyst according to claim 1, characterized in that: The catalyst has a specific surface area of ​​200–1000 m². 2 / g, pore volume 0.3~2.5cm 3 / g, the carrier has a mesopore size of 2-50nm.

4. The catalyst according to claim 1, characterized in that, Based on the total mass of the catalyst, the total mass percentage of the metal elements Ni and M is 2% to 35%.

5. The catalyst according to claim 1, characterized in that, The Ni x M y S z The presence of Ni-M cooperative configurations, including Ni-MS ternary coordination, Ni-SM bridging structures, or multi-center S bridging between M elements, forms multi-metal active centers with tunable electronic structures.

6. A method for preparing a supported multimetallic sulfide nickel-based catalyst according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Pretreatment: The porous carrier is subjected to heat treatment at a temperature of 280-350°C for 2-3 hours. S2. Loading: A precursor solution containing a Ni source and at least one M metal source is loaded onto a pretreated support using at least one of the following methods: impregnation, co-precipitation, solvothermal or hydrothermal, to obtain a support-precursor composite. S3. Calcination: The composite obtained in step S2 is calcined at 280-550°C for 1-6 hours in a nitrogen-containing atmosphere to obtain a polymetallic oxide precursor. S4. Sulfidation: The polymetallic oxide precursor obtained in step S3 is sulfided in a sulfur-containing atmosphere at 200–420°C for 1–10 hours to form polymetallic sulfide Ni. x M y S z ; S5. Activation: In a pure H2 atmosphere, the product after sulfidation in step S4 is activated at 250-420℃ for 0.5-1.5h to obtain the desired catalyst.

7. The method according to claim 6, characterized in that, In step S2, the precursor is selected from nitrates, acetates, organometallic complexes, or nickel-M layered double hydroxides, and a structure directing agent accounting for 1% to 10% of the total mass of the precursor is added during the loading process; the structure directing agent is at least one of hexadecyltrimethylammonium bromide, polyethylene glycol, or polyvinylpyrrolidone. In step S4, the sulfur-containing atmosphere is a combination of H2S and H2 or sulfur vapor or CS2, wherein the volume fraction of H2S is 0.1-10%.

8. The method according to claim 6, characterized in that, Steps S4 and S5 employ a segmented heating method to control the Ni-M dispersion and interaction, as detailed below: In a sulfur-containing atmosphere, the first stage of sulfidation treatment is carried out at 200–350℃ for 0.5–5 h, followed by a second stage of sulfidation treatment at 350–420℃ for 0.5–5 h. After sulfidation, the atmosphere is switched to pure H2 and a reduction activation treatment is carried out at 250–420℃ for 0.5–1.5 h.

9. The use of the catalyst according to any one of claims 1-5 in the preparation of long-chain olefins, characterized in that, Under the conditions of a reaction temperature of 200-350℃ and a hydrogen pressure of 0.1-3MPa, bio-based fatty acids or their derivatives are brought into contact with the catalyst described in any one of claims 1-5 to cause a decarbonylation-dehydration reaction to generate long-chain olefins.

10. The application according to claim 9, characterized in that, The bio-based fatty acid or its derivative is selected from at least one of fatty acids with 10 to 20 carbon atoms, fatty acid methyl esters with 10 to 20 carbon atoms, fatty acid ethyl esters with 10 to 20 carbon atoms, animal and vegetable oils or waste oils.