Hydration heat inhibiting particles for concrete and preparation method thereof

By preparing shell composite materials to coat phase change material particles, the problems of leakage and poor thermal stability of phase change materials in concrete were solved, achieving efficient hydration heat suppression, reducing the risk of concrete cracking and improving the state of the mixture.

CN121800457APending Publication Date: 2026-04-07CHANGJIANG RIVER SCI RES INST CHANGJIANG WATER RESOURCES COMMISSION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202512054890.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-31
Publication Date
2026-04-07

AI Technical Summary

Technical Problem

Existing phase change materials have problems such as leakage, corrosion and poor thermal stability when applied to concrete, making it difficult to effectively control the heat of hydration during the construction of large-volume concrete and leading to temperature cracks.

Method used

By encapsulating 65-75 wt% phase change material particles with 25-35 wt% shell composite material powder, and controlling granulation parameters and sol impregnation process, hydration heat suppression particles with uniform shell thickness, high structural stability, and good sealing performance are prepared. The synergistic melting and pore-forming of the two phase change materials and the sol impregnation process enhance the sealing and reduce the hydration heat of concrete.

Benefits of technology

It significantly reduces the risk of concrete cracking, improves the state of concrete mix, reduces the temperature gradient during hydration, improves compatibility and sealing efficiency, and can withstand 100 thermal cycles at 20~80℃ without cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to hydration heat inhibition particles for concrete and a preparation method thereof. The hydration heat inhibition particles are prepared by wrapping 65-75 wt% of phase change material particles with 25-35 wt% of shell layer composite material powder; the phase-change material particles are composed of 20-40 wt% of a low-temperature phase-change material and 60-80 wt% of a high-temperature phase-change material, the low-temperature phase-change material and the high-temperature phase-change material are subjected to high-temperature melting and uniform mixing, ice water is dripped into the mixture through a dripping nozzle for cooling granulation to prepare the phase-change material particles, then the phase-change material particles are placed in a disc granulator, and the shell composite material is added for granulation. The hydration heat inhibition particle for concrete prepared by the invention is uniform in shell thickness, high in structural stability, high in strength, good in sealing property, excellent in sphericity degree and good in concrete compatibility, and can tolerate 100 times of heat cycles at 20-80 DEG C without cracks; after being doped into concrete, the concrete admixture state can be improved, the temperature gradient in the concrete hydration period is remarkably reduced, and the cracking risk is remarkably reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water-based heat suppression technology for concrete. Specifically, it relates to a water-based heat suppression particle for concrete and its preparation method. Background Technology

[0002] After large-volume concrete is poured, the cement generates a large amount of heat through hydration. Due to the low thermal conductivity of concrete, heat dissipation is slow, causing internal heat to accumulate and the temperature to rise continuously. When the temperature reaches its peak and then decreases, shrinkage stress is generated inside the concrete. When the shrinkage stress exceeds the tensile stress, cracks form. Temperature cracks are one of the harmful mechanisms of crack formation in large-volume concrete. They not only affect the integrity and stiffness of the concrete structure but also provide channels for harmful substances to invade, accelerating concrete carbonation and steel corrosion, seriously affecting the service life of the project. Currently, almost all existing or under-construction large-volume concrete structures have temperature cracks to varying degrees, such as the large-volume concrete structures of the Donghai Bridge piers and the Three Gorges Dam project, requiring significant manpower and resources to repair structural damage. Phase change materials (PCMs) utilize latent heat to store energy and can absorb or release heat through their own morphological changes within a certain temperature range, thereby achieving the purpose of temperature regulation. Introducing PCMs into large-volume concrete is expected to significantly reduce the heat of hydration during concrete construction and reduce temperature cracks on the concrete surface and inside the concrete.

[0003] In recent years, there has been a great deal of research on the regulation of hydration heat using phase change materials (PCMs). For example, Chinese patent ZL202110067512.X discloses a patent technology for "a highly efficient self-compensating hydration heat regulator and its preparation method and application." This technology uses starch, paraffin-based PCMs, and amylase as raw materials, adding hydrogen peroxide, sodium hydroxide dilution, and borax solution, mixing them evenly, and then vacuum cooling and drying to obtain a highly efficient self-compensating hydration heat regulator. Chinese patent ZL201810602362.6 discloses a patent technology for "a preparation method of zeolite-based hydration heat slow-release material." This technology involves heating the PCM and organic acid to mix it with zeolite powder, and then cooling and pulverizing the mixed zeolite powder, paraffin, and organic acid to obtain the zeolite-based hydration heat slow-release material. While these technologies have their advantages, PCMs still suffer from problems such as leakage, corrosion, and poor thermal stability during application.

[0004] Some scholars have also encapsulated phase change materials into capsules, such as the patent technology disclosed in Chinese Patent ZL 202110661829.6, "A method for preparing microcapsules for controlling the heat of hydration of cement in low-temperature cementing." This technology uses phase change materials as the core material, adds a shell material solution, and then cools, filters, washes, removes impurities, and dries to obtain microcapsules. However, phase change microcapsules have low encapsulation efficiency and poor practical application results. Summary of the Invention

[0005] This invention aims to overcome the shortcomings of existing technologies and provides concrete hydration heat-inhibiting particles and their preparation method. This preparation method can precisely control the sphericity and shell uniformity of the particles, has good sealing performance, and high encapsulation efficiency. The prepared concrete hydration heat-inhibiting particles have uniform shell thickness, high structural stability, high strength, good sealing performance, excellent sphericity, and good compatibility with concrete. They can withstand 100 thermal cycles at 20~80℃ without cracking. When added to concrete, they can improve the state of the concrete mixture, reduce the temperature gradient during concrete hydration, and significantly reduce the risk of cracking.

[0006] To achieve the above objectives, the present invention provides a hydration heat-inhibiting particle for concrete, wherein the hydration heat-inhibiting particle is made by encapsulating 65-75 wt% of phase change material particles with 25-35 wt% shell composite material powder.

[0007] The phase change material particles are composed of 20-40 wt% low-temperature phase change material and 60-80 wt% high-temperature phase change material, wherein the low-temperature phase change material is any one or a mixture of n-hexadecane and n-heptadecane; and the high-temperature phase change material is any one or a mixture of n-eicosane and n-docosahexadecane.

[0008] The shell composite material is composed of 70-80 wt% stone powder, 10-15 wt% cement, 4-6 wt% alumina powder, and 6-9 wt% dextrin.

[0009] The preferred technical solution of the present invention is as follows: the stone powder is any one of granite stone powder and limestone stone powder, and the particle size of the stone powder is ≤180μm; the Al2O3 of the alumina micro powder is ≥96wt%; and the particle size of the alumina micro powder is ≤8μm.

[0010] This invention also provides a method for preparing concrete hydrated heat-inhibiting particles, the steps of which are:

[0011] S1. Place 20-40 wt% of low-temperature phase change material and 60-80 wt% of high-temperature phase change material in an oven and maintain at 50-60°C for 1-2 hours, stirring until homogeneous to obtain a phase change material melt; drip the phase change material melt into a container of ice water at a rate of 30-40 drops / min using a nozzle with a diameter of 2.5-3.5 mm, then separate it from the ice water by filtration and place it in a fume hood for 4-6 hours to air dry, thus obtaining phase change material particles;

[0012] S2. The phase change material particles prepared in step S1 are added to a disc granulator and rotated at 10-20 r / min for 0.5-1.5 h. The shell composite material powder is then placed in the disc granulator and rotated at 10-20 r / min for 1-3 h. The powder is then removed and placed in a fume hood to air dry for 4-6 h to obtain coated phase change material particles. The phase change material particles account for 65-75 wt%, and the shell composite material powder accounts for 25-35 wt%.

[0013] S3. Place the coated phase change material particles prepared in step S2 in a vacuum oven, heat them to 25-35°C at a rate of 1-3°C / min, keep them at the temperature and pressure for 3-5 hours, and let them cool naturally to room temperature to obtain a hydration heat suppression particle blank.

[0014] S4. Place the hydration heat suppression particle blank prepared in step S3 into a silica sol solution and vacuum impregnate for 3-4 hours, then dry to obtain hydration heat suppression particles.

[0015] A further technical solution of the present invention: the low-temperature phase change material is any one or a mixture of two of n-hexadecane and n-heptadecane.

[0016] A further technical solution of the present invention: the high-temperature phase change material is any one or a mixture of two of n-eicosane and n-docosahexanes.

[0017] A further technical solution of the present invention: The shell composite material in step S2 is composed of 70-80 wt% stone powder, 10-15 wt% cement, 4-6 wt% alumina micro powder, and 6-9 wt% dextrin; wherein the stone powder is any one of granite stone powder and limestone stone powder, and the particle size of the stone powder is ≤180 μm; the Al2O3 of the alumina micro powder is ≥96 wt%; and the particle size of the alumina micro powder is ≤8 μm.

[0018] A preferred embodiment of the present invention: the pressure holding pressure in step S3 is 3 × 10⁻⁶. 2 ~5×10 2 Pa.

[0019] The preferred technical solution of the present invention is: the SiO2 content of the silica sol solution in step S4 is ≥40wt%.

[0020] A preferred embodiment of the present invention: the vacuum pressure for vacuum impregnation in step S4 is 1×10⁻⁶. 2 ~3×10 2 Pa.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] This invention controls the sphericity of phase change material particles and shell composite materials by controlling the rotational speed and time of the particles and shell composite materials in a disc granulator, thereby controlling the shell thickness and uniformity. Therefore, the prepared heat-inhibiting hydration particles have uniform shell thickness, high structural stability, and high sphericity, which improves the state of concrete mixtures.

[0023] This invention uses low-temperature phase change materials and high-temperature phase change materials as the core, coating a shell of composite material powder. During baking, the low-temperature phase change material melts and, under the influence of gravity and pressure, gradually exits from the pores in the shell, forming internal pores that provide space for the volume expansion of the high-temperature phase change material during its phase change process. Sol-impregnation seals the pores in the shell, preventing the high-temperature phase change material from escaping during phase change, while simultaneously strengthening the shell. Therefore, the prepared heat of hydration-inhibiting particles exhibit good sealing properties, strong structural stability, and high strength.

[0024] This invention uses stone powder, cement, alumina, and dextrin as shell materials. The heat of hydration inhibiting particles have good compatibility when incorporated into concrete. After being incorporated into concrete, cement can be further hydrated, and the interface between the heat of hydration inhibiting particles and concrete is reduced or even disappeared, thus reducing internal defects in the concrete. Dextrin, as a shell binder, slows down the hydration reaction rate of cement particles (especially C3A and C3S) through physical adsorption and steric hindrance effects after being incorporated into concrete, thereby delaying the peak release of heat of hydration.

[0025] This invention uses a phase change material (PCM) as the outer core. When the concrete hydration temperature rises above the melting point of the PCM, the heat of hydration inhibits the PCM in the particle core from absorbing heat, utilizing latent heat to store heat and reduce the peak temperature of the concrete. After the concrete hydration temperature rise ends and the temperature is lower than the melting point of the PCM, the heat of hydration inhibits the release of heat from the PCM in the particle core, preventing the concrete temperature from dropping too quickly, reducing the temperature gradient during concrete hydration, and forming a multi-scale effect with the dextrin in the shell to inhibit the concrete hydration temperature rise and reduce the risk of concrete cracking.

[0026] This invention can precisely control the sphericity and shell uniformity of particles by adjusting granulation parameters (rotation speed and time). The use of stone powder-based shell material improves compatibility, and the synergistic melting and pore-forming of dual-phase change materials and the sol impregnation enhance sealing. The physical preparation process is highly controllable and has high packaging efficiency. The prepared hydration heat-inhibiting particles have uniform shell thickness, high structural stability, high strength, good sealing performance, excellent sphericity, and good concrete compatibility. They can withstand 100 thermal cycles at 20~80℃ without cracking. When added to concrete, they can improve the state of the concrete mix, reduce the temperature gradient during concrete hydration, and significantly reduce the risk of cracking. Attached Figure Description

[0027] Figure 1 Image of the concrete water-heat-inhibiting particles prepared according to the present invention; Figure 2 This is a comparison chart of the thermal temperature rise curves of concrete in the benchmark example and Example 1. Detailed Implementation

[0028] The present invention will be further described below with reference to specific embodiments, but the present invention is not limited to these embodiments.

[0029] The concrete hydration heat-inhibiting particles in the following embodiments are made by encapsulating 65-75 wt% of phase change material particles with 25-35 wt% of shell composite material powder; the phase change material particles are composed of 20-40 wt% of low-temperature phase change material and 60-80 wt% of high-temperature phase change material, wherein the low-temperature phase change material is any one or a mixture of n-hexadecane and n-heptadecane; and the high-temperature phase change material is any one or a mixture of n-eicosane and n-docosahexadecane.

[0030] The shell composite material in the following embodiments is composed of 70-80 wt% stone powder, 10-15 wt% cement, 4-6 wt% alumina micro powder, and 6-9 wt% dextrin. The stone powder is any one of granite stone powder and limestone stone powder, and the particle size of the stone powder is ≤180 μm. The alumina micro powder has Al2O3 ≥96 wt% and a particle size of ≤8 μm.

[0031] The preparation method of concrete hydration heat-inhibiting particles in the following embodiments specifically includes the following steps:

[0032] S1. Place 20-40 wt% of low-temperature phase change material and 60-80 wt% of high-temperature phase change material in an oven and maintain at 50-60°C for 1-2 hours, stirring until homogeneous to obtain a phase change material melt; drip the phase change material melt into a container of ice water at a rate of 30-40 drops / min using a nozzle with a diameter of 2.5-3.5 mm, then separate it from the ice water by filtration and place it in a fume hood for 4-6 hours to air dry, thus obtaining phase change material particles;

[0033] S2. The phase change material particles prepared in step S1 are added to a disc granulator and rotated at 10-20 r / min for 0.5-1.5 h. The shell composite material powder is then placed in the disc granulator and rotated at 10-20 r / min for 1-3 h. The powder is then removed and placed in a fume hood to air dry for 4-6 h to obtain coated phase change material particles. The phase change material particles account for 65-75 wt%, and the shell composite material powder accounts for 25-35 wt%.

[0034] S3. Place the coated phase change material particles prepared in step S2 in a vacuum oven, heat to 25-35℃ at a rate of 1-3℃ / min, hold at that temperature and pressure for 3-5 hours, and then allow to cool naturally to room temperature to obtain a hydration heat-inhibiting particle blank; the holding pressure is 3×10⁻⁶. 2 Pa;

[0035] S4. The hydration heat-inhibiting particle blank prepared in step S3 is placed in a silica sol solution and vacuum impregnated for 3-4 hours, then dried to obtain hydration heat-inhibiting particles; the SiO2 content of the silica sol solution is ≥40wt%; the vacuum impregnation pressure is 1×10⁻⁶. 2 Pa.

[0036] When the concrete hydration heat-inhibiting particles prepared in this invention replace 10% of the sand in concrete, they can improve the state of the concrete mix, reduce the temperature gradient during concrete hydration, and significantly reduce the risk of cracking.

[0037] Examples 1-6 were all carried out according to the above steps. The specific composition of the shell composite material powder in each example is shown in Table 1; other parameters are shown in Table 2. At the same time, the hydration heat suppression particles prepared in Examples 1 to 6 were subjected to 100 thermal cycles at 20~80℃ to observe whether the particles had cracks. The observation results are shown in Table 2. The comprehensive heat storage performance of the hydration heat suppression particles from 25℃ to 80℃ was calculated, including the sensible heat of the shell, the sensible heat of the high-temperature phase change material, and the latent heat of phase change of the high-temperature phase change material. The calculation results are shown in Table 2.

[0038] Table 1 shows the composition of the shell composite materials in Examples 1-6.

[0039]

[0040] Table 2 shows the parameters and experimental results of the prepared hydration heat-inhibiting particles in Examples 1-6.

[0041]

[0042] in, Figure 1 The image shows a photograph of the concrete prepared in Example 3, where the appearance of the particles was suppressed by the heat of hydration. As shown in the figure, the particles are intact and undamaged, with good sphericity.

[0043] The following comparative experiments further demonstrate the effectiveness of the hydration heat-inhibiting particles in this invention. Concrete was prepared according to the "Test Procedure for Hydraulic Concrete" (SL / T 352—2020) and subjected to an adiabatic temperature rise test. A comparison was made with the reference concrete (taking C30 concrete as an example, with concrete raw material usage: cement 263 kg / m³). 3 fly ash 88 kg / m³ 3 741 kg / m³ of sand3 5~20mm aggregate 563 kg / m 3 20~40mm aggregate 563 kg / m 3 Water 147 kg / m 3 ) and concrete incorporating the heat-inhibiting particles of this invention, wherein the amount of heat-inhibiting particles is 10% of the amount of sand replaced, such as Figure 2 The graphs show the adiabatic temperature rise curves of concrete in the benchmark example and Example 1. Figure 2 As shown, before the adiabatic temperature rise of concrete reaches the phase change temperature, the adiabatic temperature rise of the reference concrete and the concrete with hydration heat suppression particles is basically the same; when the adiabatic temperature rise of concrete reaches the phase change temperature, the adiabatic temperature rise curve of the concrete with hydration heat suppression particles increases more slowly and is lower than that of the reference concrete.

[0044] Although specific embodiments of the present invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art can make various modifications or additions to the described embodiments or use similar methods to substitute them, without departing from the direction of the invention or exceeding the scope defined by the appended claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc., made to the above embodiments based on the technical essence of the present invention should be included within the protection scope of the present invention.

Claims

1. A concrete water-cooling heat-inhibiting particle, characterized in that: The hydration heat suppression particles are made by encapsulating 65-75 wt% phase change material particles with 25-35 wt% shell composite material powder. The phase change material particles are composed of 20-40 wt% low-temperature phase change material and 60-80 wt% high-temperature phase change material, wherein the low-temperature phase change material is any one or a mixture of n-hexadecane and n-heptadecane; and the high-temperature phase change material is any one or a mixture of n-eicosane and n-docosahexadecane. The shell composite material is composed of 70-80 wt% stone powder, 10-15 wt% cement, 4-6 wt% alumina powder, and 6-9 wt% dextrin.

2. The concrete water-cooling heat-inhibiting particle according to claim 1, characterized in that: The stone powder is any one of granite stone powder and limestone stone powder, and the particle size of the stone powder is ≤180μm; the Al2O3 of the alumina micro powder is ≥96wt%; and the particle size of the alumina micro powder is ≤8μm.

3. A method for preparing concrete hydrated heat-inhibiting particles, characterized in that, The method specifically includes the following steps: S1. Place 20-40 wt% of low-temperature phase change material and 60-80 wt% of high-temperature phase change material in an oven and maintain at 50-60°C for 1-2 hours, stirring until homogeneous to obtain a phase change material melt; drip the phase change material melt into a container filled with ice water at a rate of 30-40 drops / min using a nozzle with a diameter of 2-4 mm, then separate it from the ice water by filtration and place it in a fume hood for 4-6 hours to air dry, thus obtaining phase change material particles; S2. The phase change material particles prepared in step S1 are added to a disc granulator and rotated at 10-20 r / min for 0.5-1.5 h. The shell composite material powder is then placed in the disc granulator and rotated at 10-20 r / min for 1-3 h. The powder is then removed and placed in a fume hood to air dry for 4-6 h to obtain coated phase change material particles. The phase change material particles account for 65-75 wt%, and the shell composite material powder accounts for 25-35 wt%. S3. Place the coated phase change material particles prepared in step S2 in a vacuum oven, heat them to 25-35°C at a rate of 1-3°C / min, keep them at the temperature and pressure for 3-5 hours, and let them cool naturally to room temperature to obtain a hydration heat suppression particle blank. S4. Place the hydration heat suppression particle blank prepared in step S3 into a silica sol solution and vacuum impregnate for 3-4 hours, then dry to obtain hydration heat suppression particles.

4. The method for preparing concrete hydrated heat-inhibiting particles according to claim 3, characterized in that: The low-temperature phase change material is any one or a mixture of two of n-hexadecane and n-heptadecane.

5. The method for preparing concrete water-heat-inhibiting particles according to claim 3, characterized in that: The high-temperature phase change material is any one or a mixture of n-eicosane and n-docosahexanes.

6. The method for preparing concrete hydrated heat-inhibiting particles according to claim 3, characterized in that: The shell composite material in step S2 is composed of 70-80 wt% stone powder, 10-15 wt% cement, 4-6 wt% alumina micro powder, and 6-9 wt% dextrin; wherein the stone powder is any one of granite stone powder and limestone stone powder, and the particle size of the stone powder is ≤180 μm; the Al2O3 of the alumina micro powder is ≥96 wt%; and the particle size of the alumina micro powder is ≤8 μm.

7. The method for preparing concrete hydrated heat-inhibiting particles according to claim 3, characterized in that: The pressure held in step S3 is 3 × 10⁻⁶. 2 ~5×10 2 Pa.

8. The method for preparing concrete hydrated heat-inhibiting particles according to claim 3, characterized in that: In step S4, the SiO2 content of the silica sol solution is ≥40wt%.

9. The method for preparing concrete hydrated heat-inhibiting particles according to claim 3, characterized in that: The vacuum pressure for vacuum impregnation in step S4 is 1×10⁻⁶. 2 ~3×10 2 Pa.

Citation Information

Patent Citations

  • Preparation method of zeolite-based hydration heat-suppressing materials

    CN108774015B

  • A highly efficient self-compensating hydration heat regulator, its preparation method and application

    CN112830708B

  • A method for preparing microcapsules for controlling the heat of cement hydration in low-temperature cementing.

    CN113307532B