Direct high-temperature regeneration method of waste lithium iron phosphate positive plate in water vapor atmosphere

By regenerating waste lithium iron phosphate cathode sheets at high temperature in a water vapor atmosphere, and using water vapor to generate reducing gas to repair the material structure, the problem of high-temperature treatment in traditional lithium iron phosphate battery recycling is solved, achieving low-cost and efficient material regeneration and performance restoration.

CN121812806APending Publication Date: 2026-04-07GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610135825.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-30
Publication Date
2026-04-07

AI Technical Summary

Technical Problem

Traditional lithium iron phosphate battery recycling methods suffer from problems such as high cost of cathode material stripping, carbon redundancy, uneven carbon coating, and severe degradation of the electrochemical performance of recycled materials. Furthermore, high-temperature processing can easily lead to aluminum foil melting, which limits its large-scale application.

Method used

Waste lithium iron phosphate cathode sheets are directly regenerated at high temperature in a water vapor atmosphere. Water vapor reacts with the cathode material to generate reducing gas, which repairs the material structure. The crystal structure is restored through lithium intercalation. The aluminum foil is prevented from melting at low temperature. The residual electrolyte is used as a lithium source, simplifying the pretreatment steps.

Benefits of technology

It enables complete repair of lithium iron phosphate structure at low temperatures, reduces material loss and processing costs, improves lithium-ion replenishment efficiency, enhances the electrochemical performance and cycle stability of recycled materials, and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121812806A_ABST
    Figure CN121812806A_ABST
Patent Text Reader

Abstract

The invention discloses a direct high-temperature regeneration method of a waste lithium iron phosphate positive plate in a water vapor atmosphere. The method comprises the following steps: directly placing the positive plate obtained by discharging and disassembling the waste lithium iron phosphate battery into a reaction container, directly regenerating at 600-650 DEG C by taking superheated steam as a gasification medium, and removing aluminum foil after the regeneration process is completed, thereby obtaining the regenerated lithium iron phosphate positive plate. According to the method provided by the invention, the structure of lithium iron phosphate can be completely repaired at a relatively low temperature, and aluminum foil fusion is avoided. Compared with a traditional recycling process, the method has the advantages that complex pretreatment steps such as smashing, screening and stripping are omitted, material loss is reduced, the whole process is mild and environmentally friendly, and the method is short in process and easy and convenient to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of waste lithium iron phosphate technology, and in particular to a direct high-temperature regeneration method for waste lithium iron phosphate cathode sheets under a water vapor atmosphere. Background Technology

[0002] Lithium iron phosphate (LFP) batteries have been widely used in electric vehicles (EVs) and energy storage systems due to their excellent safety performance, long cycle life, and cost-effectiveness. The typical lifespan of LFP batteries is 5 to 8 years, meaning a large number of batteries will gradually reach the end of their lifespan. It is predicted that by 2030, the total amount of spent LFP batteries will reach 498 GWh. Spent LFP batteries contain abundant metal resources, such as copper, aluminum, lithium, and iron, as well as organic electrolytes and hazardous substances. Improper handling will not only waste resources (the lithium content in spent LFP batteries is 2.0 wt%–4.5 wt%, significantly higher than that of primary lithium ore) but may also cause environmental pollution. Therefore, the recycling of LFP batteries has dual significance in achieving efficient resource reuse and environmental protection, and plays an important role in promoting the sustainable development of the lithium-ion battery industry.

[0003] Currently, traditional pyrometallurgical and hydrometallurgical technologies for recycling spent lithium-ion batteries have advantages such as mature processes and high recycling efficiency (>90%), capable of efficiently leaching valuable metals from cathode materials and converting them into metal salt compounds. However, the extraction and separation of metal elements is complex, requiring significant energy and chemical reagent consumption. Pyrometallurgical and hydrometallurgical technologies are highly applicable to processing ternary lithium batteries containing high-value metals such as lithium, cobalt, and nickel. However, due to the low cost of lithium iron phosphate (SLFP) materials, traditional recycling technologies are economically insufficient to meet the actual needs of SLFP battery recycling, limiting their widespread adoption in large-scale industrial applications. For SLFP batteries, only lithium has high recycling value, making conventional recycling methods economically unfeasible. Compared to pyrometallurgical and hydrometallurgical methods, direct regeneration of spent lithium iron phosphate materials is more efficient and cleaner. This method can completely restore the chemical composition, crystal structure, and electrochemical performance of lithium iron phosphate materials to their initial state while preserving their original structure. As a green closed-loop recycling strategy, it features a short recycling process, low carbon emissions, high cost-effectiveness, and environmental friendliness, making it one of the most promising approaches for lithium iron phosphate recycling.

[0004] The capacity reduction of LFP batteries is mainly due to lithium loss (lithium vacancy defects), structural defects caused by volume changes during cycling, and the reduced lithium-ion diffusion rate resulting from the formation of amorphous FePO4 phase. Introducing appropriate amounts of lithium (Li), iron (Fe), phosphorus (P), and carbon (C) as additives into the LFP cathode material can effectively improve the energy density and cycle stability of the LFP material. Among these, lithium supplementation plays a crucial role. Furthermore, during heat treatment, organic carbon sources such as glucose and sucrose are typically added as reducing agents to lower the activation energy required for iron ion migration and promote their re-occupation of the correct positions in the crystal lattice. Simultaneously, the amorphous carbon produced by the pyrolysis of these carbon sources at high temperatures can also be used to repair missing carbon layers in the material, further improving material performance. Although the capacity of regenerated lithium iron phosphate materials can be partially recovered, their electrochemical performance is still significantly inferior to that of the original material, mainly due to the presence of excessive carbon in the regenerated material. Excess carbon in the regenerated material leads to excessive electrolyte consumption, intensified interfacial side reactions, and reduced lithium-ion diffusion during cycling, resulting in insufficient electrochemical performance and poor cycle stability of the regenerated LFP material. Traditional carbon removal processes typically employ air roasting before the lithium replenishment stage. However, during this process, lithium iron phosphate materials undergo a phase transition to generate Fe2O3, increasing the technical complexity of subsequent material regeneration processes.

[0005] Therefore, developing a process for integrated purification and remediation of SLFP materials in an anaerobic environment is crucial. This process should be able to moderately remove the carbon coating on the surface of lithium iron phosphate (LFP) particles while removing the polyvinylidene fluoride (PVDF) binder. On the other hand, with the continuous expansion of the SLFP recycling industry, the cost of replenishing raw materials is becoming increasingly important, thus necessitating the development of more cost-effective alternatives. In lithium iron phosphate secondary batteries, the materials coated on the aluminum foil include not only the active material (lithium iron phosphate) but also valuable components rich in lithium and carbon, such as binders (PVDF), conductive agents (acetylene black), and electrolytes (lithium hexafluorophosphate and ester compounds). These components can serve as internal supplements for lithium iron phosphate regeneration, thereby significantly reducing the overall cost of lithium iron phosphate remediation and minimizing waste. Therefore, there is an urgent need to develop a method for in-situ high-temperature solid-phase remediation of SLFP cathode sheets in an anaerobic environment to reduce the regeneration cost of SLFP. Summary of the Invention

[0006] The purpose of this invention is to provide a direct high-temperature regeneration method for waste lithium iron phosphate cathode sheets under a water vapor atmosphere, in order to solve the technical problems existing in traditional SLFP regeneration, such as high cost of cathode material stripping, carbon redundancy, uneven carbon coating, and severe degradation of the electrochemical performance of regenerated materials. The method proposed in this invention can completely repair the structure of lithium iron phosphate at a lower temperature and avoid aluminum foil melting.

[0007] This invention is achieved through the following technical solutions:

[0008] This invention protects a direct high-temperature regeneration method for waste lithium iron phosphate cathode sheets under a water vapor atmosphere. The method includes the following steps: placing the cathode sheets obtained after discharging and dismantling waste lithium iron phosphate batteries directly into a reaction vessel, using superheated steam as the gasification medium, and directly regenerating them at 600℃-650℃. After the regeneration process is completed, the aluminum foil is removed to obtain the regenerated lithium iron phosphate cathode sheets.

[0009] This invention uses waste lithium iron phosphate cathode sheets as raw materials, employs steam as a heating medium, and uses the residual electrolyte as a supplementary lithium source. Lithium ions are re-intercalated through a reaction with the cathode material, thereby restoring its crystal structure. During this process, water molecules react with residual carbon in the cathode sheet to generate reducing gases such as carbon monoxide and hydrogen. These gases effectively reduce ferric iron to ferrous iron in the material, while simultaneously achieving appropriate carbon layer removal, fully exposing the surface of the active material. This not only improves the lithium ion replenishment efficiency but also reduces the formation of lithium-iron antisite defects.

[0010] Specifically, using superheated steam as the gasification medium, water-gas reaction (C + H2O ⇌ CO + H2), water-gas shift reaction (CO + H2O ⇌ CO2 + H2), and Boudouard reaction (C + CO2 ⇌ 2CO) occur under high-temperature conditions, thereby forming a large amount of reducing gas (CO + H2). These reducing gases are beneficial for reducing high-valence iron ions, thus effectively repairing lithium / iron antisite defects. At the same time, the reducing gases and carbothermic reduction have a synergistic effect, which can further reduce the repair temperature of SLFP.

[0011] Preferably, the regeneration time is 1-3 hours.

[0012] Preferably, the water / carbon molar ratio is 9 / 1 to 12 / 1.

[0013] Preferably, the heating rate is 5-30 °C / min.

[0014] The present invention also protects the method for obtaining a regenerated lithium iron phosphate cathode sheet.

[0015] This invention also protects a lithium iron phosphate cathode material, which is prepared by the following steps: the regenerated lithium iron phosphate cathode sheet, polyvinylidene fluoride, acetylene black and N-methylpyrrolidone are mixed to form a uniform slurry, the uniform slurry is coated on an aluminum foil, and then dried under vacuum conditions to obtain the lithium iron phosphate cathode material.

[0016] Preferably, the mass ratio of the regenerated lithium iron phosphate cathode sheet, polyvinylidene fluoride, and acetylene black is 8:1:1.

[0017] Compared with the prior art, the beneficial effects of the present invention are:

[0018] 1. The method proposed in this invention can completely repair the structure of lithium iron phosphate at a lower temperature and avoid aluminum foil melting. Compared with traditional recycling processes, it eliminates complex pretreatment steps such as crushing, screening and stripping, reduces material loss, and the overall process is mild and environmentally friendly, with the advantages of short process and simple operation.

[0019] 2. This invention uses the positive electrode sheet of SLFP as raw material and the residual electrolyte therein as a lithium source to react with the positive electrode material, restoring its structure through lithium intercalation. This integrated method combines a vapor reduction mechanism with in-situ utilization of the inherent residue, enabling efficient regeneration of LFP at a lower temperature, far lower than the temperature required by traditional methods using an inert argon atmosphere (>700°C).

[0020] 3. Lowering the temperature is a key driver of process intensification. It allows for direct regeneration of the active material while it remains attached to the aluminum current collector, thus avoiding separation caused by the melting of the aluminum foil at temperatures exceeding 650°C. Therefore, it eliminates the complex and material-loss-prone crushing, sieving, and stripping processes inherent in traditional electrode recycling.

[0021] 4. Water molecules react with carbon in SLFP to generate reducing gases (carbon monoxide and hydrogen). These gases can effectively reduce ferric iron to ferrous iron, thereby achieving moderate carbon removal, exposing the surface of the active material, improving the lithium ion replenishment efficiency, and reducing the formation of lithium iron antisite defects. Attached Figure Description

[0022] Figure 1 The X-ray diffraction patterns are of the regenerated SLFPs obtained in Examples 1-2 and Comparative Examples 1-2. Detailed Implementation

[0023] The present invention will be further described in detail below with reference to the embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions in the art or as recommended by the manufacturer; the raw materials and reagents used, unless otherwise specified, are considered to be commercially available materials and reagents that can be obtained through conventional markets and other commercial channels.

[0024] Example 1

[0025] 12 grams of SLFP positive electrode sheet were loaded into a sealed horizontal tube furnace. The reactor was first purged with argon gas for 30 minutes to purge air and prevent sample oxidation and combustion. Heating was carried out at a rate of 5 °C / min under programmed temperature control, while deionized water was continuously introduced into the high-temperature zone of the tube furnace via a syringe pump to generate steam. Water was continuously injected throughout the reaction, with a water / carbon molar ratio of 12 / 1. When the temperature reached 600 °C, the reaction was continued at this constant temperature for 3 hours. The entire reaction was conducted at atmospheric pressure, with an ice-water seal at the outlet to maintain pressure stability and facilitate the removal of residual volatile components such as hydrogen fluoride (HF) and pyrolysis oil. After the regeneration process, the aluminum foil was removed by physical stripping to obtain the regenerated lithium iron phosphate positive electrode sheet.

[0026] Example 2

[0027] 12 grams of SLFP positive electrode sheet were loaded into a sealed horizontal tube furnace. The reactor was first purged with argon gas for 30 min to purge air and prevent sample oxidation and combustion. Heating was carried out at a rate of 30 °C / min under programmed temperature control, while deionized water was continuously introduced into the high-temperature zone of the tube furnace via a syringe pump to generate steam. Water was continuously injected throughout the reaction, with a water-to-carbon molar ratio of 9:1. When the temperature reached 650 °C, the reaction was continued at this constant temperature for 1 h. The entire reaction was conducted at atmospheric pressure, with an ice-water seal at the outlet to maintain pressure stability and facilitate the removal of residual volatile components such as hydrogen fluoride (HF) and pyrolysis oil. After the regeneration process, the aluminum foil was removed by physical stripping to obtain the regenerated lithium iron phosphate positive electrode sheet.

[0028] Comparative Example 1

[0029] The direct regeneration method for SLFP described in this comparative example has basically the same operating steps as in Example 2, except that: no water vapor is introduced during the reaction process in this comparative example, and the entire regeneration reaction is carried out under an argon protective atmosphere.

[0030] Comparative Example 2

[0031] 12 grams of SLFP positive electrode sheet were loaded into a sealed horizontal tube furnace. The reactor was first purged with argon gas for 30 min to purge air and prevent sample oxidation and combustion. Heating was carried out at a rate of 30 °C / min under programmed temperature control, while deionized water was continuously introduced into the high-temperature zone of the tube furnace via a syringe pump to generate steam. Water was continuously injected throughout the reaction, with a water-to-carbon molar ratio of 9:1. When the temperature reached 700 °C, the reaction was continued at an isothermal temperature for 1 h. The entire reaction was carried out at atmospheric pressure, with an ice-water seal at the outlet to maintain pressure stability and facilitate the removal of residual volatile components such as hydrogen fluoride (HF) and pyrolysis oil.

[0032] Test Analysis

[0033] The regenerated LFP (80 wt%), PVDF (10 wt%), acetylene black (10 wt%), and N-methylpyrrolidone obtained in Examples 1-2 and Comparative Examples 1-2 were mixed to form a homogeneous slurry. The mass ratio of regenerated LFP to N-methylpyrrolidone was 1:9. The slurry was coated onto aluminum foil and then dried under vacuum at 80°C for 24 hours. The prepared positive electrode material was then cut into circular sheets with a diameter of 14 mm. Using the prepared circular sheets as the positive electrode, lithium metal sheets as the negative electrode, and 1.0 M LiPF6 as the electrolyte, with a solvent consisting of ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) in a volume ratio of 1:1:1, button cells were assembled and their electrochemical performance was tested (test voltage range 2.5-4.2 V, ambient temperature 25°C).

[0034] Results Comparison

[0035] From the appendix Figure 1 It can be seen that the diffraction peaks of LiF and Li3PO4 appear in Comparative Example 1, indicating that the SFLP repair was not completed. Compared with Comparative Example 1, the diffraction peak positions of Examples 1, 2, and 2 are basically consistent with the standard LFP card. However, the additional Al characteristic peak in Comparative Example 2, with an aluminum content of 2.232%, indicates that the aluminum foil melted at 700°C, which is not conducive to subsequent aluminum foil peeling.

[0036] As shown in Table 1, the lithium-iron molar ratio of the regenerated LFPs obtained in Examples 1 and 2 is close to the theoretical 1:1, indicating that the structure of the regenerated LFPs was basically repaired. Simultaneously, the carbon content was reduced by more than 30% compared to SLFPs. The discharge specific capacity shows that the discharge specific capacity of Examples 1 and 2 is greater than 145 mAh / g, further demonstrating that the performance of the LFPs was effectively restored after regeneration. The discharge specific capacity of the regenerated LFPs obtained in Comparative Example 1 is much lower than that of Example 2, indicating that at the same temperature, the introduction of water vapor is beneficial to the structural repair of SLFPs. The discharge specific capacity of the regenerated LFPs obtained in Comparative Example 2 is lower than that of the examples, further demonstrating that the presence of a large amount of aluminum significantly affects the electrochemical performance of the battery.

[0037] Table 1. Elemental content and electrochemical performance of regenerated LFP

[0038] .

[0039] The above description of the embodiments is only for the purpose of helping to understand the technical solution and core idea of ​​the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

Claims

1. A method for direct high-temperature regeneration of waste lithium iron phosphate cathode sheets under a water vapor atmosphere, characterized in that, The method includes the following steps: placing the positive electrode sheet obtained after discharging and dismantling the waste lithium iron phosphate battery directly into a reaction vessel, using superheated steam as the gasification medium, and directly regenerating it at 600℃-650℃. After the regeneration process is completed, the aluminum foil is removed to obtain the regenerated lithium iron phosphate positive electrode sheet.

2. The method according to claim 1, characterized in that, The regeneration time is 1-3 hours.

3. The method according to claim 1, characterized in that, The water / carbon molar ratio is 9 / 1 to 12 / 1.

4. The method according to claim 1, characterized in that, The heating rate is 5-30 ℃ / min.

5. The method according to any one of claims 1-4 yields a regenerated lithium iron phosphate cathode sheet.

6. A lithium iron phosphate cathode material, characterized in that, The lithium iron phosphate cathode material is prepared by the following steps: the regenerated lithium iron phosphate cathode sheet as described in claim 5, polyvinylidene fluoride, acetylene black and N-methylpyrrolidone are mixed to form a uniform slurry, the uniform slurry is coated on aluminum foil, and then dried under vacuum conditions to obtain the lithium iron phosphate cathode material.

7. The lithium iron phosphate cathode material according to claim 6, characterized in that, The mass ratio of the regenerated lithium iron phosphate cathode sheet, polyvinylidene fluoride, and acetylene black is 8:1:1.