Preparation method and application of cobalt hydroxide based on seed crystal circulation and special active magnesium oxide

By using seed crystal recycling and a special active magnesium oxide method, the problem of poor sedimentation performance of magnesium oxide precipitant during cobalt precipitation was solved, achieving efficient cobalt precipitation and the preparation of high-quality cobalt hydroxide, thus improving the overall technical and economic indicators of copper-cobalt smelting.

CN121823667APending Publication Date: 2026-04-10WESTERN MINING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610030642.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-12
Publication Date
2026-04-10

AI Technical Summary

Technical Problem

Existing technologies using magnesium oxide as a precipitant present the problem of difficulty in simultaneously achieving cobalt precipitation effect and sedimentation performance, especially in the treatment of low-grade copper-cobalt ore leaching solutions, where the concentration of the thickener underflow is too low, affecting the efficiency of subsequent pressure filtration and drying processes and product quality.

Method used

Highly active magnesium oxide fine powder is prepared by using a seed recycling and special active magnesium oxide method through high-temperature suspension dynamic calcination and ultra-fine grinding. Polyethylene glycol and other additives are added, and combined with the seed recycling process, the growth of cobalt hydroxide grains is promoted and the sedimentation performance is improved.

Benefits of technology

It improves the sedimentation performance and product quality of cobalt hydroxide, increases the underflow concentration to 28-30%, achieves a cobalt sedimentation rate of over 98%, reduces magnesium residue to less than 5%, lowers production costs, and adapts to different production requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121823667A_ABST
    Figure CN121823667A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of cobalt hydroxide based on seed crystal circulation and special active magnesium oxide. Through cooperation of a seed crystal circulation technology and a special auxiliary agent, the generated cobalt hydroxide is converted into a core of subsequent crystal growth, uniform and thick growth of the cobalt hydroxide is guided, and the industry bottleneck that the underflow concentration of a thickener is low when high-activity magnesium oxide is adopted for cobalt precipitation is effectively solved. The average particle size (D50) of the product is increased from 16.81 [mu] m to 21.81 [mu] m or above, the underflow concentration is increased from 27% to 28-30%, and the sedimentation and compaction performance of ore pulp is remarkably improved. While excellent physical properties are obtained, the chemical quality of the product is excellent, the cobalt content reaches 40% or above, and the magnesium residue is lower than 5%. The process economy is outstanding, the cobalt precipitation rate is increased to 98% or above, and the unit consumption of magnesium oxide is reduced to 0.70-0.71 t / t Co. According to the method, the seed crystal derives from the process, parameter regulation and control are flexible, compatibility with an existing production line is good, and large-scale industrial application prospects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of hydrometallurgy, in particular to a cobalt hydroxide preparation method based on seed crystal circulation and special active magnesium oxide and application thereof. BACKGROUND

[0002] Congo (Kinshasa) cobalt resources are mostly in the form of copper-cobalt associated oxide ore, and its hydrometallurgy usually adopts the process of grinding, stirring leaching, extraction, and electrodeposition to produce cathode copper. The cobalt-containing raffinate produced after extraction of copper needs to be further treated by impurity removal, cobalt precipitation, slurry washing, pressure filtration, and flash drying to produce crude cobalt hydroxide product. The core of the cobalt precipitation process is to add a precipitant to make cobalt ions in the solution form a difficultly soluble cobalt compound and separate from the liquid phase.

[0003] At present, magnesium oxide is commonly used as a precipitant in industrial production. However, according to the source and preparation method of magnesium oxide, its effect in practical application is significantly different. The magnesium oxide produced by the local African ore method, such as magnesite calcination method and brine-dolomite milk precipitation calcination method, has the following outstanding defects: first, the magnesium oxide prepared by the magnesite method has low activity, which is only suitable for treating high-grade copper-cobalt ore leaching solution, and has poor adaptability to low-grade mines. Second, the purity of the magnesium oxide produced by the ore method is relatively insufficient, and many impurities are introduced, which increases the impurity content in the cobalt precipitation product and seriously affects the quality of the cobalt hydroxide product. Third, the cobalt precipitation reaction efficiency of this type of magnesium oxide is low, and the amount of magnesium oxide required per cobalt precipitation is high, increasing the overall operating cost. Fourth, after using this type of magnesium oxide for cobalt precipitation, the generated cobalt hydroxide slurry shows the problems of insufficient compaction degree and low underflow concentration in the first-stage cobalt precipitation thickener, which directly leads to a decrease in the treatment capacity of the subsequent pressure filtration process, a high moisture content of the filter cake, and further affects the flash drying efficiency and the final product capacity, which has become a bottleneck restricting the smooth operation of the process.

[0004] To solve the sedimentation problem, the industry usually tries to increase the particle size of active magnesium oxide in order to promote the agglomeration of cobalt hydroxide particles and improve the sedimentation speed and underflow concentration. However, this method has a fundamental contradiction, i.e., when the particle size of magnesium oxide is excessively increased, its reactive surface is significantly reduced, leading to incomplete cobalt precipitation reaction, decreased cobalt precipitation rate, and difficulty in guaranteeing the main cobalt grade in the product, while the magnesium residue is likely to exceed the standard, which cannot meet the strict internal quality indicators of copper-cobalt smelting enterprises.

[0005] In recent years, the special active magnesium oxide prepared by brine precipitation method for cobalt precipitation has begun to enter the African market. The product shows significant advantages in cobalt precipitation effect. Specifically, it has high cobalt grade, low magnesium residue and low unit consumption. However, in industrial application, it also exposes the problem of poor settling performance, that is, the concentration of the bottom stream of the first-stage cobalt precipitation thickener is low, and the compaction degree of the cobalt hydroxide slurry is insufficient, which restricts the capacity release of the subsequent filter pressing and drying processes. Therefore, how to effectively solve the problem of low concentration of the bottom stream of the thickener without sacrificing the excellent cobalt precipitation effect of the salt lake method magnesium oxide has become a key technical problem to be solved for promoting the large-scale application of this high-performance precipitator.

[0006] Existing patent technologies, the current disclosed schemes mostly focus on improving the cobalt precipitation rate or reducing impurities, but lack effective and systematic solutions for how to synergistically optimize the cobalt precipitation chemical effect and physical settling performance, especially for achieving high settling concentration while ensuring low magnesium residue and low unit consumption.

[0007] In summary, the existing technology has the contradiction that the cobalt precipitation effect and the settling performance cannot be achieved at the same time. Developing a new cobalt precipitation process or a precipitator modification method that can not only maintain the high-efficiency cobalt precipitation characteristics of the salt lake method active magnesium oxide, but also significantly improve the settling and compaction performance of the cobalt hydroxide slurry, has important practical significance and industrial value for improving the overall technical and economic indicators of cobalt hydrometallurgy in Congo (DRC) and similar resource areas. SUMMARY

[0008] Based on the above technical problems, the purpose of the present application is to provide a method for preparing cobalt hydroxide based on seed crystal circulation and special active magnesium oxide and its application.

[0009] The present application protects a method for preparing cobalt hydroxide based on seed crystal circulation and special active magnesium oxide, which specifically includes the following steps: Step 1, preparation of special active magnesium oxide for cobalt precipitation: using salt lake bischofite MgCl2·6H2O as raw material, high-purity magnesium hydroxide is produced by "brine-ammonia-lime" combined method, and high-activity magnesium oxide fine powder is obtained by high-temperature suspension dynamic calcination and ultra-fine grinding; then, additives are compounded into the active magnesium oxide fine powder, wherein the additive: active magnesium oxide fine powder = 1:0.05wt%, and mixed uniformly to obtain special active magnesium oxide for cobalt precipitation, which is ready for use; Step 2, preparation of simulated cobalt precipitation front liquid: analytical pure cobalt sulfate, manganese sulfate, magnesium sulfate, iron sulfate, copper sulfate and deionized water are used to prepare the target components, wherein Co 2 ⁺ is 13.36g / L, Mn 2 ⁺ is 2.7g / L, Mg 2 ⁺ is 8g / L, Fe 3 ⁺ is 0.0002g / L, Cu 2+ 0.06 g / L, pH is adjusted to 5.5-6.5 with dilute sulfuric acid or sodium hydroxide solution to prepare simulated pre-cobalt precipitation solution for standby; Step 3, preparation of magnesium oxide emulsion: the special active magnesium oxide for cobalt precipitation is mixed with deionized water in proportion, and stirred and slurried for 30-120 min to prepare a uniform magnesium oxide emulsion with a solid content of 5-15 wt% for standby; Step 4, seed preparation: a certain volume of simulated pre-cobalt precipitation solution is placed in a reactor, and a certain amount of magnesium oxide emulsion is measured, wherein the amount of magnesium oxide emulsion added is 0.7 times the mass of cobalt metal in the pre-cobalt precipitation solution, i.e. the molar ratio of cobalt to magnesium oxide is about 1:1, and the magnesium oxide emulsion is added into the pre-cobalt precipitation solution at a stirring speed of 700 rpm under normal temperature and pressure, and the reaction is carried out for 6 h; after the reaction is completed, the slurry is allowed to settle naturally, the supernatant is removed carefully, and the thick cobalt hydroxide solid phase slurry at the bottom is reserved, which is the initial seed for standby; Step 5, cobalt precipitation reaction: a new simulated pre-cobalt precipitation solution is placed in a reactor, and a magnesium oxide emulsion with the same stoichiometric ratio as the seed preparation is measured, and the seed is added to the reactor; wherein the amount of seed added is 100-300% of the theoretical precipitation amount of cobalt metal in the pre-cobalt precipitation solution, and the magnesium oxide emulsion is added into the reaction system at a stirring speed of 700 rpm, and the reaction temperature is controlled at 25-60°C, and the constant temperature reaction time is 4-6 h, and after the reaction is completed, a cobalt hydroxide slurry is obtained; Step 6, cobalt hydroxide slurry treatment: the above cobalt hydroxide slurry is vacuum filtered, the filter cake is washed with hot pure water at 60-80°C for 1-2 times to sufficiently remove soluble impurities, and then the filter cake is placed in an oven and dried at 100-110°C to constant weight to obtain a cobalt hydroxide product; part of the separated cobalt hydroxide solid phase can be returned to the cobalt precipitation reaction as the seed for the next batch to realize seed recycling; Step 7, settling performance evaluation: the above cobalt hydroxide product is added to 1 L of deionized water, and the slurry is prepared at a stirring speed of 700 rpm for 1-2 h to obtain a uniform and dispersed simulated slurry; 500 mL of the slurry is measured and placed in a measuring cylinder, 2 mL of anionic polyacrylamide PAM flocculant solution with a mass-volume concentration of 2‰ is added, and the mixture is immediately inverted and mixed for 5 times, and then left to stand and start timing, and the volume of the settled solid at 5 min is recorded for calculating and comparing the settling speed, and after 30 min, the supernatant is quickly removed, the concentrated underflow at the bottom is collected and weighed, and then the underflow is filtered, dried and weighed, and the mass concentration of the underflow solid is calculated by the dry weight of the solid and the total weight of the underflow.

[0010] Further, in step 1, the high-purity magnesium hydroxide can also be purchased from the market.

[0011] Further, in step 1, the activated magnesium oxide fine powder satisfies the following conditions: MgO content > 99.50%, activated MgO content > 90.0%, and particle size distribution D. 10 >1.35μm, D 50 6~8μm, D 98 >30μm, D 100 >48μm; the additive is one or more of polyethylene glycol, sodium sulfite, sodium dodecyl sulfate and ammonium chloride.

[0012] Further, in step 3, the special active magnesium oxide for cobalt precipitation is mixed with deionized water in a certain proportion and stirred at 500 rpm for 30-120 minutes to prepare a uniform magnesium oxide emulsion with a solid content of 10 wt%.

[0013] Furthermore, in step 5, the amount of seed crystals added is 100% of the theoretical amount of cobalt metal precipitated in the pre-precipitation solution, based on the mass of cobalt metal contained therein. The reaction temperature is controlled at 35°C, and the constant temperature reaction time is 6 hours.

[0014] Further, in step 6, the above cobalt hydroxide slurry is vacuum filtered, and the resulting filter cake is washed twice to fully remove soluble impurities. Then, the filter cake is placed in an oven and dried at 100°C to constant weight.

[0015] This invention also protects the preparation of cobalt hydroxide products by the above method, wherein the cobalt hydroxide product has a Co content of 40%~46%, a Mg residue of 3%~5%, and a particle size distribution of D. 10 >8μm, D 50 >20μm, D 98 >50μm, cobalt deposition rate ≥98%.

[0016] This invention also protects the application of the aforementioned cobalt hydroxide product, which is used in the fields of new energy and electronic materials, specifically in the preparation of precursors for lithium-ion battery cathode materials.

[0017] Compared with existing technologies, the present invention has the following beneficial effects: The method of this invention ingeniously utilizes a seed crystal recycling process and polyethylene glycol (PEG) as a dedicated cobalt-precipitating active magnesium oxide to generate nucleation sites for cobalt hydroxide and promote grain growth. The combined effect of these two processes promotes the growth of the generated cobalt hydroxide grains, resulting in a more uniform crystal size distribution. This effectively solves the problem encountered by some copper-cobalt mining companies in Africa when using high-purity, high-activity magnesium oxide prepared by salt lake chemical synthesis, where the concentration of the cobalt hydroxide at the bottom of the thickener is low (insufficient cobalt hydroxide compaction), thus affecting the output of downstream filtration and drying. A detailed analysis follows: 1. By adding seed crystals, the average particle size D50 of the cobalt hydroxide product is increased from 16.81 μm without seed crystals to more than 21.81 μm, and the underflow concentration after slurry settling is increased from 27% to 28-30%, solving the core problem of low underflow concentration of the thickener, and providing protection for efficient operation of the subsequent filter pressing and drying processes.

[0018] 2. While improving the settling, the cobalt content of the product is maintained at more than 40%, and the preferred scheme can reach 45.68%; the key impurity magnesium is stably less than 5%, and the preferred scheme can be as low as 2.53%, fully meeting the quality requirements of high-end applications.

[0019] 3. The cobalt precipitation rate is increased from less than 85% in the traditional method to more than 98%, achieving efficient recovery of cobalt, and the magnesium oxide consumption is reduced from 0.83-0.88 t / t Co in the traditional method to 0.70-0.71 t / t Co, significantly reducing production costs.

[0020] 4. The seed crystals are derived from the self-process, and do not need to be purchased, and the seed crystal addition amount can be flexibly adjusted within 100%-300% to adapt to different production requirements. Moreover, the method has good compatibility with the existing production line, is simple to modify, and has conditions for large-scale industrial application. BRIEF DESCRIPTION OF DRAWINGS

[0021] Figure 1 The process flow diagram of the present application. DETAILED DESCRIPTION

[0022] The technical solutions of the present application will be described below in conjunction with examples. Obviously, the described examples are only a part of the embodiments of the present application, rather than all the embodiments. Based on the examples in the present application, all other embodiments obtained by those skilled in the art without creative labor fall within the scope of the present application.

[0023] A cobalt hydroxide preparation method based on seed crystal circulation and special active magnesium oxide will be further described in detail below in conjunction with specific industrial examples. The raw materials used in the examples and comparative examples of the present application, unless otherwise specified, are all conventional commercially available products in the art. The reagents used, unless otherwise specified, are all analytical pure.

[0024] Example 1 A cobalt hydroxide preparation method based on seed crystal circulation and special active magnesium oxide I. Raw materials and equipment 1. Preparation of special active magnesium oxide for cobalt precipitation (1)Self-made: With salt lake water chloromagnesite MgCl2·6H2O as raw material, high-purity magnesium hydroxide produced by the combined method of "brine-ammonia-lime" as precursor, high-temperature suspension dynamic calcination furnace at 650-800℃ is used for rapid decomposition, and then ultrafine grinder is used for treatment to obtain high-activity magnesium oxide fine powder; MgO content > 99.50%, 100℃, 2h drying weight loss method, active MgO content > 90.0% (citric acid activity method), particle size distribution: D 10 >1.35μm, D 50 6-8μm, D 98 >30μm.

[0025] (2)Purchased: Directly use the commercially available products meeting the performance indicators, such as high-purity active magnesium oxide products produced by Qinghai Western Magnesium Industry Co., Ltd.

[0026] (3)Complexing of additives: Complexing additives to active magnesium oxide fine powder, wherein the additive: active magnesium oxide fine powder = 1:0.05wt%, uniformly mixed, to obtain the special active magnesium oxide for cobalt precipitation, and the additive is selected from one or more of polyethylene glycol (PEG), sodium sulfite, sodium dodecyl sulfate (SDS), and ammonium chloride.

[0027] (4)Comparison of magnesium oxide B (ore method): Commercially available magnesium oxide prepared by calcination of magnesite, with performance indicators of MgO content about 97.5%, activity about 85%, and particle size D50 of 15-20μm.

[0028] 2, Preparation of simulated cobalt precipitation solution To simulate the composition of typical raffinate after copper extraction of Congo (DRC) copper-cobalt ore, analytical reagents and deionized water are used for preparation, with main target ion concentrations of Co 2 + of 13.36g / L, Mn 2 + of 2.7g / L, Mg 2 + of 8g / L, Fe 3 + of 0.0002g / L, Cu 2 + of 0.06g / L. Dilute sulfuric acid or sodium hydroxide solution is used to adjust pH to 5.5-6.5.

[0029] 3, Main equipment Reactor with stirring and temperature control, electronic balance, pH meter, vacuum filtration device, oven, laser particle size analyzer, atomic absorption spectrometer (AAS) or inductively coupled plasma emission spectrometer (ICP-OES).

[0030] II. Specific implementation steps 1, Preparation of magnesium oxide emulsion Based on stoichiometric calculation: 13.36g Co x 0.7 = 9.352g MgO, corresponding to Co:MgO molar ratio ≈ 1:1, weigh 9.352g of the above-mentioned special cobalt-deposition active magnesium oxide, add 84.0g of deionized water, and stir to slurry at a speed of 500rpm for 120min to obtain a uniform magnesium oxide emulsion A with a solid content of 10wt%; 2. Seed crystal preparation According to the above target composition, 1.0L of simulated cobalt deposition solution B was prepared using analytical pure sulfate, and the pH was adjusted to 6.0. It was measured that the cobalt content in the solution was 13.36g / L. 1L of simulated cobalt deposition solution B was taken and placed in a 2.0L reactor. According to the cobalt mass of 13.40g, it was calculated that the mass of magnesium oxide to be added was 13.36g x 0.7 = 9.352g (corresponding to a molar ratio of cobalt to magnesium oxide of about 1:1). Corresponding amount of magnesium oxide emulsion A was 93.52g. At room temperature and normal pressure, the magnesium oxide emulsion A was added to the reactor at a stirring speed of 700rpm, and the reaction was carried out for 6 hours. After the reaction was completed, it was allowed to stand and settle, and the supernatant was carefully removed to obtain a thick cobalt hydroxide slurry C. The slurry C was the initial seed crystal, and the dry basis mass (theoretical cobalt precipitation amount) was about 13.36g of cobalt.

[0031] 3. Cobalt deposition reaction A new 1.0L simulated cobalt deposition solution B was taken and placed in another 2.0L reactor. The same amount of magnesium oxide emulsion A as in the seed crystal preparation was about 93.52g, and the prepared seed cobalt hydroxide slurry C was taken. According to the dry basis cobalt mass of 13.36g, the seed crystal was added at a ratio of 100% (i.e. the amount of seed crystal cobalt: the amount of cobalt in this solution = 1:1). All were added to the reactor. The stirring was started at 700rpm, and the magnesium oxide emulsion A was added at one time. The reaction temperature was controlled at 35°C, and the constant temperature reaction was carried out for 6h. After the reaction was completed, a cobalt hydroxide slurry D was obtained.

[0032] 4. Cobalt hydroxide slurry treatment The above-mentioned cobalt hydroxide slurry D was vacuum filtered, and the filter cake was washed with hot pure water at 70°C for 2 times to sufficiently remove soluble impurities. Subsequently, the filter cake was placed in an oven and dried at 105°C until the weight was constant to obtain a cobalt hydroxide product E. The chemical composition (ICP-OES) was Co content 45.68%, Mg residue 2.53%, cobalt deposition rate 98.14%, and magnesium oxide consumption 0.71t / t Co. The particle size distribution (laser particle size analyzer) was D 10 : 8.8μm, D 50 : 21.81μm, D98: 56.42μm. The separated part of the cobalt hydroxide solid phase can be returned to the cobalt deposition reaction as the seed crystal for the next batch, realizing seed crystal circulation.

[0033] 5. Sedimentation performance evaluation Take 30.0 g of cobalt hydroxide product E, add 1.0 L of deionized water, and beat for 2 h at a speed of 700 rpm to restore it to a simulated ore slurry; measure 500 mL of this slurry in a graduated cylinder with a stopper, add 2 mL of anionic polyacrylamide PAM flocculant solution with a mass-volume concentration of 2 ‰, immediately invert and mix for 5 times, then stand still, record the volume of the settled solids at the bottom after 5 min as 125 mL, for calculation and comparison of settling speed, stand still for 30 min, then quickly remove the supernatant, collect the concentrated underflow at the bottom and weigh as 152 g (total mass of underflow slurry), then filter and dry the underflow to obtain a dry solid weight of 42.5 g (mass of underflow rod solid), and calculate the underflow solid mass concentration to be about 28.0%, with the best comprehensive performance. Among them, the underflow concentration formula is: .

[0034] Example 2 Example 2 is consistent with the other reaction conditions of Example 1, except for the cobalt precipitation reaction: Take a new 1.0 L of simulated cobalt precipitation solution B and place it in another 2.0 L reactor, take about 93.52 g of magnesium oxide emulsion A equivalent to the amount of seed preparation, take the prepared cobalt hydroxide slurry C, according to its dry basis cobalt mass of 26.72 g, add 200% of the seed at a ratio of 1:1 (i.e. seed cobalt amount: this time's front liquid cobalt amount = 1:1), all into the reactor; start stirring at 700 rpm, then add the magnesium oxide emulsion A at one time, control the reaction temperature at 35°C, and react for 4 h at constant temperature; after the reaction is completed, cobalt hydroxide slurry D is obtained, which is detected to have a chemical composition (ICP-OES) of Co content 42.01%, Mg residual 3.25%, cobalt precipitation rate 99.95%, and magnesium oxide consumption 0.70 t / t Co; particle size distribution (laser particle size analyzer): D 10 : 9.15 μm, D 50 : 22.87 μm, D98: 50.36 μm.

[0035] Its settling test 5 min settlement volume is 110 mL, underflow concentration reaches 30.0%, and the settling and compaction performance is further improved, with the best settling performance.

[0036] Example 3 Example 3 is consistent with the other reaction conditions of Example 1, except for the cobalt precipitation reaction: A new 1.0 L simulated cobalt precipitation solution B was taken and placed in another 2.0 L reactor, about 93.52 g of magnesium oxide emulsion A equivalent to the seed preparation was taken, and the prepared cobalt hydroxide seed slurry C was taken, according to its dry basis cobalt mass of 40.08 g, and a seed addition ratio of 300% (i.e. seed cobalt amount: this time's cobalt solution amount = 1:1) was added to the reactor; the stirring was started at 700 rpm, and then the magnesium oxide emulsion A was added at one time, and the reaction temperature was controlled at 35°C, and the constant temperature reaction was carried out for 4h, and then the reaction was completed, and the cobalt hydroxide slurry D was obtained, and the chemical composition (ICP-OES) was detected: the Co content was 41.94%, the Mg residue was 3.82%, the cobalt precipitation rate was 99.98%, and the magnesium oxide consumption was 0.70t / t Co; the particle size distribution (laser particle size analyzer) was: D 10 : 9.66μm, D 50 : 23.89μm, D98: 58.83μm.

[0037] The sedimentation test was carried out for 5min, and the sediment volume was 86mL, and the underflow concentration reached 30.0%, the cobalt precipitation rate was the highest, and the grade was slightly reduced.

[0038] Comparative Example 1 The other reaction conditions of Comparative Example 1 and Example 1 were the same, except that: No additives were added, and the un-compounded active magnesium oxide fine powder was directly used; 9.352g of un-compounded magnesium oxide was weighed to prepare a magnesium oxide emulsion with a solid content of 10w%, which was added to the 1.0 L simulated cobalt precipitation solution at one time, and the reaction was carried out at 35°C and 700rpm for 4h. That is, no seed was prepared in advance, and no seed was added in the reaction.

[0039] The chemical composition (ICP-OES) was detected: the Co content was 38.52%, the Mg residue was 3.48%, the cobalt precipitation rate was 84.80%, and the magnesium oxide consumption was 0.83t / t Co; the particle size distribution (laser particle size analyzer) was: D 10 : 18.54μm, D 50 : 29.72μm, D98: 55.61μm. The sedimentation test was carried out for 5min, and the sediment volume was 82mL, and the underflow concentration reached 29.0%, the reaction was poor, the grade was low, and the particle size was abnormal.

[0040] Comparative Example 2 The other reaction conditions of Comparative Example 1 and Example 1 were the same, except that: The seed recycling step was cancelled, and 9.352g of cobalt precipitation special active magnesium oxide A (containing additives) was directly used to prepare a magnesium oxide emulsion with a solid content of 10w%, which was added to the 1.0 L simulated cobalt precipitation solution at one time, and the reaction was carried out at 35°C and 700rpm for 4h. That is, no seed was prepared in advance, and no seed was added in the reaction, but there were additives.

[0041] The chemical composition (ICP-OES) was detected: the Co content was 38.34%, the Mg residue was 5.04%, the cobalt precipitation rate was 79.61%, and the magnesium oxide consumption was 0.88 t / t Co; the particle size distribution (laser particle size analyzer) was as follows: D 10 : 6.95 μm, D 50 : 16.81 μm, D98: 34.12 μm. The sedimentation test was 75 mL for 5 min, and the underflow concentration reached 27.0%, the particle size was fine, the sedimentation was poor, and the efficiency was low.

[0042] In summary, examples 1-3, while maintaining the advantages of high cobalt, low magnesium, and low consumption of salt lake method magnesium oxide, successfully increased the product particle size to more than 20 μm through the seed circulation process, thereby fundamentally improving the underflow concentration of the thickener and solving the bottleneck problem in the background art. Comparative example 1 and comparative example 2 (same special cobalt precipitation special magnesium oxide A, only without seed difference), the introduction of seed circulation makes the product D50 increase from 16.81 μm to 21.81 μm, the underflow concentration increases from 27.0% to 28.0%, the cobalt precipitation rate increases from 79.61% to 98.14%, the consumption decreases from 0.88 to 0.71, which proves the decisive role of seed in improving the comprehensive performance. The amount of seed increases from 100% to 300%, the product particle size increases, the cobalt precipitation rate approaches complete, the underflow concentration remains high, but the cobalt grade decreases slightly due to seed dilution. Example 1 (100% seed) is the most optimal comprehensive performance. Comparative example 1 shows that without the aid of the seed process, the reaction is uncontrollable, and although large particle size is occasionally obtained, the quality and efficiency are very poor; comparative example 2 shows that even if high-quality magnesium oxide is used, without seed, the sedimentation and efficiency cannot be solved. This proves the necessity and creativity of the systematic solution of the present application from the negative side.

[0043] Although embodiments of the present application have been shown and described, it will be understood by those of ordinary skill in the art that various changes, modifications, substitutions and alterations can be made thereto without departing from the principles and spirit of the present application, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing cobalt hydroxide based on seed crystal recycling and special active magnesium oxide, characterized in that, Specifically, the steps include the following: Step 1, Preparation of Cobalt-Specific Activated Magnesium Oxide: Using magnesium chloride from salt lake water (MgCl2·6H2O) as raw material, high-purity magnesium hydroxide is produced by a combined "brine-ammonia-lime" method. After high-temperature suspension dynamic calcination and ultra-fine grinding, highly active magnesium oxide fine powder is obtained. Then, additives are compounded into the active magnesium oxide fine powder, wherein the ratio of additives to active magnesium oxide fine powder is 1:0.05wt%, and the mixture is homogeneous to obtain cobalt-specific activated magnesium oxide for later use. Step 2, Preparation of the simulated cobalt precipitation pretreatment solution: This solution was prepared using analytical grade cobalt sulfate, manganese sulfate, magnesium sulfate, ferric sulfate, copper sulfate, and deionized water. The target component included: Co. 2 ⁺ is 13.36 g / L, Mn 2 ⁺ is 2.7 g / L, Mg 2 ⁺ is 8 g / L, Fe 3 ⁺ is 0.0002 g / L, Cu 2 The concentration of ⁺ is 0.06 g / L. The pH is adjusted to 5.5-6.5 with dilute sulfuric acid or sodium hydroxide solution to prepare a simulated cobalt precipitation pretreatment solution for later use. Step 3, Preparation of magnesium oxide emulsion: Mix the special active magnesium oxide for cobalt precipitation with deionized water in a certain proportion, stir and slurry for 30~120min, and prepare a uniform magnesium oxide emulsion with a solid content of 5~15wt% for later use. Step 4, Seed preparation: Take a certain volume of simulated cobalt precipitation pre-liquid and place it in the reactor. Measure the amount of magnesium oxide emulsion, where the amount of magnesium oxide emulsion added is calculated as 0.7 times the mass of cobalt metal in the cobalt precipitation pre-liquid, i.e., the molar ratio of cobalt to magnesium oxide is approximately 1:

1. Under normal temperature and pressure, with a stirring speed of 700 rpm, add the magnesium oxide emulsion to the cobalt precipitation pre-liquid all at once and react for 6 hours. After the reaction is completed, let it stand to allow the slurry to settle naturally. Carefully remove the supernatant and retain the thick cobalt hydroxide solid slurry at the bottom, which is the initial seed crystal for later use. Step 5, cobalt precipitation reaction: Take a fresh simulated cobalt precipitation pre-liquid and place it in the reactor. Measure a magnesium oxide emulsion with the same stoichiometric ratio as the seed crystal preparation and add the seed crystal to the reactor. The amount of seed crystal added is based on the mass of cobalt metal contained in it, and is 100-300% of the theoretical cobalt metal precipitation amount in the pre-liquid. At a stirring speed of 700 rpm, add the magnesium oxide emulsion to the reaction system all at once. Control the reaction temperature at 25-60℃ and the constant temperature reaction time at 4-6 hours. After the reaction is completed, cobalt hydroxide slurry is obtained. Step 6, Cobalt hydroxide slurry treatment: The above cobalt hydroxide slurry is vacuum filtered, and the resulting filter cake is washed 1-2 times with hot pure water at 60-80℃ to fully remove soluble impurities. Then, the filter cake is placed in an oven and dried at 100-110℃ to constant weight to obtain the cobalt hydroxide product. A portion of the separated cobalt hydroxide solid phase can be returned to the cobalt precipitation reaction as seed crystals for the next batch, realizing seed crystal recycling. Step 7, Sedimentation performance evaluation: Add the above cobalt hydroxide product to 1L of deionized water and stir at 700rpm for 1-2 hours to obtain a uniformly dispersed simulated slurry; measure 500mL of slurry into a graduated cylinder, add 2mL of anionic polyacrylamide (PAM) flocculant solution with a mass-volume concentration of 2‰, immediately invert and mix 5 times, let stand and start timing, record the volume of bottom sedimented solids after 5 minutes for calculation and comparison of sedimentation rate, after standing for 30 minutes, quickly remove the supernatant, collect the concentrated bottom flow and weigh it, then filter, dry and weigh the bottom flow, calculate the mass concentration of bottom flow solids by the dry weight of solids and the total weight of bottom flow.

2. The method for preparing cobalt hydroxide according to claim 1, characterized in that, In step 1, the high-purity magnesium hydroxide can also be purchased commercially.

3. The method for preparing cobalt hydroxide according to claim 1, characterized in that, In step 1, the activated magnesium oxide fine powder meets the following requirements: MgO content > 99.50%, activated MgO content > 90.0%, and particle size distribution D. 10 >1.35μm, D 50 6~8μm, D 98 >30μm, D 100 >48μm; the additive is one or more of polyethylene glycol, sodium sulfite, sodium dodecyl sulfate and ammonium chloride.

4. The method for preparing cobalt hydroxide according to claim 1, characterized in that, In step 3, the special active magnesium oxide for cobalt precipitation is mixed with deionized water in a certain proportion and stirred at 500 rpm for 30-120 minutes to prepare a uniform magnesium oxide emulsion with a solid content of 10 wt%.

5. The method for preparing cobalt hydroxide according to claim 1, characterized in that, In step 5, the amount of seed crystals added is based on the mass of cobalt metal contained in them, and is 100% of the theoretical amount of cobalt metal to be precipitated in the pre-cobalt precipitation solution. The reaction temperature is controlled at 35℃, and the constant temperature reaction time is 6h.

6. The method for preparing cobalt hydroxide according to claim 1, characterized in that, In step 6, the above cobalt hydroxide slurry is vacuum filtered, and the resulting filter cake is washed twice to fully remove soluble impurities. Then, the filter cake is placed in an oven and dried at 100°C to constant weight.

7. A cobalt hydroxide product, characterized in that, The cobalt hydroxide product is prepared by the preparation method according to any one of claims 1-6, wherein the cobalt hydroxide product contains 40%~46% Co, 3%~5% Mg residue, and has a particle size distribution of D. 10 >8μm, D 50 >20μm, D 98 >50μm, cobalt deposition rate ≥98%.

8. The application of the cobalt hydroxide product according to claim 7, characterized in that, The cobalt hydroxide product is used in the fields of new energy and electronic materials, specifically in the preparation of precursors for lithium-ion battery cathode materials.