3D printing ecological material based on immature soil and preparation method

By rationally proportioning the components in the raw soil material, the problems of slow curing speed and poor foundation stability of raw soil 3D printing materials have been solved, realizing a fast-curing and high-performance ecological material suitable for the rapid construction of homestays and residences.

CN121850560APending Publication Date: 2026-04-14蒋黔湘
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311363528.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2026-04-14

AI Technical Summary

Technical Problem

Existing earth-based 3D printing materials suffer from low physical properties, slow curing speed, poor foundation stability when stacked, and a lack of materials suitable for large-scale printed buildings on the market.

Method used

An eco-friendly material that can be rapidly cured is prepared by rationally proportioning components such as raw soil, calcined gypsum, sulfoaluminate cement, silica fume, Wacker dispersible mortar, water-reducing agent, retarder, water-repellent agent, defoamer, steel fiber, and crack-resistant fiber. The setting time is controlled by fast-hardening and fast-drying cement and gypsum, and the skeleton is reinforced by aggregate and steel fiber. The water-reducing agent adjusts the water demand to prevent cracking.

Benefits of technology

It enables rapid curing of ecological materials, improves the compressive strength, density, water resistance and shear strength of buildings, simplifies the construction process, reduces costs, and is suitable for construction sites such as scenic spots and mountainous areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention is suitable for the technical field of 3D ecological soil material printing, and provides a 3D printing ecological material based on immature soil and a preparation method of the 3D printing ecological material. Comprising 45%-60% of raw soil, 5%-10% of calcined gypsum, 10%-20% of aggregate, 10%-18% of sulphoaluminate cement, 5%-12% of silica fume powder, 0.2%-0.8% of Wacker dispersed rubber powder, 0.5%-1.0% of a water reducing agent, 0.8%-1.5% of a retarder, 0.5%-1.5% of a water repellent, 0.2%-0.8% of a defoaming agent, 0.5%-1% of steel fibers and 0.2%-0.5% of anti-cracking fibers. By adding the different functional components, the physical properties such as compressive strength, compactness, resilience modulus, water resistance, freezing resistance and shear strength of a wall are guaranteed, and the problems existing in current market materials are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of 3D ecological soil material printing technology, and particularly relates to a 3D printed ecological material based on raw soil and its preparation method. Background Technology

[0002] 3D printing technology has been widely applied in fields such as construction, medicine, and aerospace. 3D printing creates objects by layering materials. Using clay as a 3D printing material for construction has great potential, significantly reducing construction costs, improving efficiency, and enhancing quality. Compared to brick-and-mortar and wooden structures, it offers greater advantages in terms of recyclability, energy efficiency, and ecological health.

[0003] Soil, as an easily obtainable natural building material, is characterized by being green and environmentally friendly, recyclable, inexpensive, and simple to prepare, making it particularly suitable for the rapid construction of homestays and guesthouses.

[0004] Currently, the raw earth materials used in 3D printing generally suffer from low physical properties, slow curing speed, and poor foundation stability when stacked. Furthermore, there are no specific raw earth-based 3D printing materials on the market suitable for large-scale printed buildings. 3D printing raw earth materials must possess good flowability to pass smoothly through delivery pipes, be able to form immediately after extrusion, allowing for layer-by-layer stacking during printing, and have sufficient early strength to support their own weight and the load of the upper layers. Simultaneously, they must ensure the adhesion between each layer to guarantee the overall strength and flexural resistance of the building.

[0005] Therefore, in view of the above situation, there is an urgent need to develop a 3D printing ecological material based on raw soil and its preparation method to overcome the shortcomings in current practical applications. Summary of the Invention

[0006] The purpose of this invention is to provide a 3D printed eco-material based on raw soil and its preparation method, in order to solve the problems mentioned in the background art.

[0007] The present invention is implemented as follows: a 3D printing eco-material based on raw soil, comprising, by weight percentage: 45%-60% raw soil, 5%-10% calcined gypsum, 10%-20% aggregate, 10%-18% sulfoaluminate cement, 5%-12% silica fume, 0.2%-0.8% Wacker dispersant powder, 0.5%-1.0% water-reducing agent, 0.8%-1.5% retarder, 0.5%-1.5% water-repellent agent, 0.2%-0.8% defoamer, 0.5%-1% steel fiber, and 0.2%-0.5% crack-resistant fiber.

[0008] Further technical solutions, by weight percentage, include: 50% raw soil, 8% calcined gypsum, 16% aggregate, 15% sulfoaluminate cement, 8% silica fume, 0.3% Wacker dispersible mortar, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber.

[0009] A further technical solution is that the raw soil includes uncontaminated yellow clay, red clay, and other undisturbed soil or construction waste soil free of branches, weeds, and foreign matter, with a liquid limit (the standard consistency limit of the cone particle size analyzer for clayey soil) of 26%-45% and a plasticity index (characterizing the physical properties of fine-grained soil) of 16%-35%. It is dried to a moisture content of less than 5% and crushed to a maximum particle size of less than 3mm using a bottomless screen crusher.

[0010] A further technical solution is provided, wherein the calcined gypsum is building gypsum (2CaSO4·H2O), conforming to the superior grade high-strength gypsum of GB / T8776—2008 "Building Gypsum", and may be calcined gypsum or calcined phosphogypsum; the aggregate is sand or recycled construction waste with a continuous gradation of particle size of 1mm-3mm.

[0011] In a further technical solution, the sulfoaluminate cement is a rapid-hardening high-strength cement with a strength of not less than 42.5.

[0012] In a further technical solution, the Wacker dispersant powder is a Wacker water-retaining and thickening dispersible latex powder.

[0013] In a further technical solution, the water-repellent agent is a German Wacker silicone water-repellent agent; the water-reducing agent is a polycarboxylate powder water-reducing agent; the retarder is a polymeric amino acid protein retarder; and the defoamer is a polyether silicone defoamer powder.

[0014] In a further technical solution, the crack-resistant fiber comprises plant straw fiber and polypropylene fiber with a length of 3mm-6mm; the steel fiber comprises steel fiber or stainless steel fiber filament with a length of 10mm-30mm.

[0015] Another objective of this invention is to provide a method for preparing 3D-printed eco-materials based on raw soil, comprising the following steps:

[0016] The raw soil is dried and crushed into soil powder with a particle size of less than 3mm. High-strength calcined gypsum powder, silica fume powder, sulfoaluminate cement, aggregate, Wacker dispersible mortar powder, water-reducing agent, retarder, water-repellent agent, defoamer, steel fiber and crack-resistant fiber are added and stirred evenly for 5-10 minutes. After stopping the machine for 2 minutes, it is sealed in a moisture-proof bag for later use.

[0017] A further technical solution involves adding water to the above-mentioned material at a ratio of 50%-60% of the mixture weight and stirring it into a thin paste. The fluidity should be controlled at 160mm-180mm, and the stirring time should be 2-3 minutes. Then, the mixture is fed into the hopper of the printing equipment. The uniformly mixed raw soil-based slurry material with a certain moisture content is extruded through a screw extruder or air compressor. The time from adding water to stacking and extruding the material until the hopper is used up should be controlled at 15-20 minutes (not too early or too late). The raw soil paste material is continuously and uniformly extruded and layered along the path of the designed 3D model coordinate points through the printer nozzle, ultimately forming a 3D printed building.

[0018] This invention provides a method for preparing a 3D-printed eco-material based on raw soil. The method involves a rational proportioning of raw soil, high-strength calcined gypsum powder, silica fume, sulfoaluminate cement, aggregates, Wacker dispersible mortar, water-reducing agent, retarder, water-repellent agent, defoamer, steel fiber, and crack-resistant fiber. Considering the appropriate open time requirements for the material's setting time, fast-hardening and quick-drying cement and gypsum are used. Water-reducing agents are employed to adjust water demand and ensure fluidity. Aggregates, steel fibers, and polypropylene fibers are used to enhance the skeleton connection, ensuring the connection and stability of the superimposed structure and meeting the requirements of water resistance, safety, and constructability for buildings.

[0019] The use of fast-setting, high-strength gypsum and sulfoaluminate cement ensures the rapid curing speed of the substrate. The addition of silica fume increases the strength of the cured soil and reduces the heat of intense hydration during rapid reaction, preventing cracking during curing. Using 1mm-3mm aggregate provides skeletal support and enhances physical strength, while also preventing cracking during curing. Water-reducing agents primarily reduce the amount of water used in the substrate, increasing strength and reducing cracking. Wacker dispersant powder's main function is to prevent insufficient hydration of the cementitious material due to excessively strong hydration reactions, thus maintaining the strength of the cured soil. This particular type of Wacker dispersant powder... It has excellent bonding properties to ensure the adhesion between the upper and lower layers of the extruded substrate; the retarder's main principle is to control and delay the initial setting time of gypsum and sulfate cement, and the appropriate ratio ensures the extrusion stacking time and the stability of the foundation during printing; the water-repellent agent mainly improves the water resistance of the wall, thereby ensuring the safety, stability and frost resistance of the building wall; the defoamer reduces the air bubbles generated during the mixing process and extrusion stacking, ensuring the density of the wall and making the wall's compressive strength, resilient modulus and other properties better; the addition of steel fiber greatly improves the shear and flexural strength; the addition of crack-resistant fiber solves the micro-cracks of the cured body, which greatly helps to improve the overall strength and shear capacity.

[0020] The addition of these different functional components ensures the physical properties of the wall, such as compressive strength, density, resilient modulus, water resistance, freeze resistance, and shear strength, thus solving the problems existing in current market materials.

[0021] This invention utilizes factory-produced moisture-proof packaging bags for direct delivery to the construction site, solving the problem of construction in many scenic areas, mountainous regions, and lakeside areas where necessary processes such as on-site soil extraction, drying, and crushing cannot be carried out. Construction is simple and fast; a single building covering 100 square meters... 2 A 3-meter-long homestay can be printed in just 2 days; using the material of this invention to print and build houses not only has a fast curing speed and excellent performance, but also low cost and good green and energy-saving effect, which plays a revolutionary role in effectively promoting the application of clay 3D printing technology in homestays and residences. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0023] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.

[0024] Example 1

[0025] Step 1: Select clean, uncontaminated clay with a liquid limit of 26%-45% and a plasticity index of 16%-35%, and dry it until the moisture content is below 5%; use a bottomless screen crusher to crush it into clay powder with a particle size of less than 3mm, and set it aside.

[0026] Step 2: Take 45% of the above clay powder by weight, and add in sequence 8% high-strength calcined gypsum powder, 8% silica fume powder, 15% sulfoaluminate cement, 19% aggregate, 0.3% Wacker dispersant powder, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber into a sealed mixer and mix thoroughly for 5-8 minutes. After stopping the machine for 2 minutes, seal the mixture in a bag and store it for later use.

[0027] Step 3: Take 100 portions of the above-mentioned finished mixture and slowly add it into the hopper. Add water and stir simultaneously for 2-3 minutes. Control the amount of water added to 50% of the weight of the mixed material, until it becomes a thin paste with a flowability of about 160 mm. Then, put it into the hopper of the printing equipment and extrude the uniformly mixed paste-like raw soil slurry material through the screw extruder. The time from adding water to stacking to complete extrusion and use of this hopper should be controlled within 15 minutes.

[0028] Example 2

[0029] Step 1: Select clean, uncontaminated clay with a liquid limit of 26%-45% and a plasticity index of 16%-35%, and dry it until the moisture content is below 5%; use a bottomless screen crusher to crush it into clay powder with a particle size of less than 3mm, and set it aside.

[0030] Step 2: Take 50% of the above clay powder by weight, and add 8% high-strength calcined gypsum powder, 7% silica fume powder, 15% sulfoaluminate cement, 15% aggregate, 0.3% Wacker dispersant powder, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber into a sealed mixer and mix thoroughly for 5-8 minutes. After stopping the machine for 2 minutes, seal the mixture in a bag and store it for later use.

[0031] Step 3: Take 100 portions of the above-mentioned finished mixture and slowly add it into the hopper. Add water and stir simultaneously for 2-3 minutes. Control the amount of water added to 50% of the weight of the mixed material, until it becomes a thin paste with a flowability of about 160 mm. Then, put it into the hopper of the printing equipment and extrude the uniformly mixed paste-like raw soil slurry material through the screw extruder. The time from adding water to stacking to complete extrusion and use of this hopper should be controlled within 15 minutes.

[0032] Example 3

[0033] Step 1: Select clean, uncontaminated clay with a liquid limit of 26%-45% and a plasticity index of 16%-35%, and dry it until the moisture content is below 5%; use a bottomless screen crusher to crush it into clay powder with a particle size of less than 3mm, and set it aside.

[0034] Step 2: Take 55% of the above clay powder by weight, and add in sequence 5% high-strength calcined gypsum powder, 7% silica fume powder, 15% sulfoaluminate cement, 13% aggregate, 0.3% Wacker dispersible mortar powder, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber into a sealed mixer. Mix thoroughly for 5-8 minutes, stop the machine for 2 minutes, and then seal and package in a bag for later use.

[0035] Step 3: Take 100 portions of the above-mentioned finished mixture and slowly add it into the hopper. Add water and stir simultaneously for 2-3 minutes. Control the amount of water added to 55% of the weight of the mixed material, until it becomes a thin paste with a flowability of about 180 mm. Then, put it into the hopper of the printing equipment and extrude the uniformly mixed raw soil-based slurry material through the screw extruder. The time from adding water to stacking to completely extruding and using up this hopper should be controlled within 15 minutes.

[0036] Example 4

[0037] Step 1: Select clean, uncontaminated clay with a liquid limit of 26%-45% and a plasticity index of 16%-35%, and dry it until the moisture content is below 5%; use a bottomless screen crusher to crush it into clay powder with a particle size of less than 3mm, and set it aside.

[0038] Step 2: Take 60% of the above clay powder by weight, and add in sequence 5% high-strength calcined gypsum powder, 7% silica fume powder, 13% sulfoaluminate cement, 10% aggregate, 0.3% Wacker dispersant powder, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber into a sealed mixer. Mix thoroughly for 5-8 minutes, stop the machine for 2 minutes, and then seal and package in a bag for later use.

[0039] Step 3: Take 100 portions of the above-mentioned finished mixture and slowly add it into the hopper. Add water and stir simultaneously for 2-3 minutes. Control the amount of water added to 55% of the weight of the mixed material, until it becomes a thin paste with a flowability of about 180 mm. Then, put it into the hopper of the printing equipment and extrude the uniformly mixed raw soil-based slurry material through the screw extruder. The time from adding water to stacking to completely extruding and using up this hopper should be controlled within 15 minutes.

[0040] Example 5

[0041] Step 1: Select clean, uncontaminated clay with a liquid limit of 26%-45% and a plasticity index of 16%-35%, and dry it until the moisture content is below 5%; use a bottomless screen crusher to crush it into clay powder with a particle size of less than 3mm, and set it aside.

[0042] Step 2: Take 50% of the above clay powder by weight, and add in sequence 5% high-strength calcined gypsum powder, 7% silica fume powder, 15% sulfate cement, 18% aggregate, 0.3% Wacker dispersant powder, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber into a sealed mixer. Mix thoroughly for 5-8 minutes, stop the machine for 2 minutes, and then seal and package in a bag for later use.

[0043] Step 3: Take 100 portions of the above-mentioned finished mixture and slowly add it into the hopper. Add water and stir simultaneously for 2-3 minutes. Control the amount of water added to 55% of the weight of the mixed material, until it becomes a thin paste with a flowability of about 180 mm. Then, put it into the hopper of the printing equipment and extrude the uniformly mixed raw soil-based slurry material through the screw extruder. The time from adding water to stacking to completely extruding and using up this hopper should be controlled within 15 minutes.

[0044] To ensure the optimal composition and process of this invention, multiple sets of non-standard specimens (100*100*100mm) were prepared and printed for the above embodiments. These specimens were then cured in a curing chamber at 25±2℃ and 95% relative humidity until the required testing age. The main performance characteristics were tested according to the testing and evaluation methods specified in GB / T17671-1999 "Test Method for Strength of Cement Mortar (ISO Method)," GB / T50080-2002 "Standard for Test Methods of Performance of Ordinary Concrete Mixtures," and GB / T50107-2010 "Standard for Evaluation of Concrete Strength Testing."

[0045] Table 1 Main Indicator Tests

[0046]

[0047]

[0048] As shown in Table 1, the amount of raw soil used is approximately 45%-60%. The lower the soil content, the better the compressive strength and flexural strength. Examples 2 and 5 both used a soil ratio of 50%, and their performance was similar. Increasing the amount of gypsum can accelerate solidification, improve the speed and stability of printing and stacking, and also significantly improve early strength. However, later strength, flexural strength, and water absorption all tend to decrease. The amount of aggregate added has a significant impact on performance; when the amount of aggregate decreases, the compressive strength and flexural strength show a clear downward trend. Therefore, the components disclosed in this invention are the conclusions of cost-effectiveness derived from actual test data, wherein the following components (Example 2) are the optimal mix proportions: 50% raw soil (i.e., clay powder), 8% calcined gypsum, 16% aggregate, 15% sulfoaluminate cement, 8% silica fume, 0.3% Wacker dispersant powder, 0.8% water-reducing agent, 1% retarder, 1% water-repellent agent, 0.5% defoamer, 1% steel fiber, and 0.4% crack-resistant fiber.

[0049] This invention provides a 3D printing eco-material based on raw clay and its preparation method. The method involves sequentially mixing clay powder with gypsum powder, silica fume, sulfate cement, aggregate, Wacker dispersant powder, water-reducing agent, retarder, water-repellent agent, defoamer, steel fiber, and crack-resistant fiber in a reasonable proportion, followed by thorough mixing. This produces a transportable substrate that can be easily applied at the construction site by simply adding water and mixing. This eco-friendly material improves upon the curing speed, compressive strength, flexural strength, and water resistance of typical raw clay-based printing materials, enhancing key technical indicators for construction. Furthermore, it is cost-effective and easy to apply.

[0050] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0051] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.

Claims

1. A 3D-printed eco-material based on raw soil, characterized in that, By weight percentage, including: Raw soil 45%-60%, calcined gypsum 5%-10%, aggregate 10%-20%, sulfoaluminate cement 10%-18%, silica fume 5%-12%, Wacker dispersant powder 0.2%-0.8%, water-reducing agent 0.5%-1.0%, retarder 0.8%-1.5%, water-repellent agent 0.5%-1.5%, defoamer 0.2%-0.8%, steel fiber 0.5%-1%, crack-resistant fiber 0.2%-0.5%.

2. The 3D-printed eco-material based on raw soil according to claim 1, characterized in that, By weight percentage, including: The composition is as follows: raw soil 50%, calcined gypsum 8%, aggregate 16%, sulfoaluminate cement 15%, silica fume 8%, Wacker dispersible mortar 0.3%, water-reducing agent 0.8%, retarder 1%, water-repellent agent 1%, defoamer 0.5%, steel fiber 1%, and crack-resistant fiber 0.4%.

3. The 3D-printed eco-material based on raw soil according to claim 1 or 2, characterized in that, The raw soil includes uncontaminated yellow clay, red clay, and other undisturbed soil or construction waste soil free of branches, weeds, and foreign objects, with a liquid limit of 26%-45% and a plasticity index of 16%-35%. It is dried to a moisture content of less than 5% and crushed to a maximum particle size of less than 3mm using a bottomless screen crusher.

4. The 3D-printed eco-material based on raw soil according to claim 1 or 2, characterized in that, The calcined gypsum is either calcined gypsum or calcined phosphogypsum. The aggregate is sand or recycled construction waste with a continuous gradation of particle size between 1mm and 3mm.

5. The 3D-printed eco-material based on raw soil according to claim 1 or 2, characterized in that, The sulfoaluminate cement is a rapid-hardening high-strength cement with a strength of not less than 42.

5.

6. The 3D-printed eco-material based on raw soil according to claim 1 or 2, characterized in that, The Wacker dispersant powder is a Wacker water-retaining and thickening dispersible latex powder.

7. The 3D-printed eco-material based on raw soil according to claim 1 or 2, characterized in that, The water-repellent agent is a German Wacker silicone water-repellent agent; The water-reducing agent is a polycarboxylate powder water-reducing agent; The retarder is a polymeric amino acid protein retarder; The defoamer is a polyether silicone defoamer powder.

8. The 3D-printed eco-material based on raw soil according to claim 1 or 2, characterized in that, The crack-resistant fiber comprises plant straw fiber and polypropylene fiber with a length of 3mm-6mm; The steel fibers include steel fibers or stainless steel fibers with a length of 10mm-30mm.

9. A method for preparing a 3D-printed eco-material based on raw soil as described in any one of claims 1-8, characterized in that, Includes the following steps: The raw soil is dried and crushed into soil powder with a particle size of less than 3mm. High-strength calcined gypsum powder, silica fume powder, sulfoaluminate cement, aggregate, Wacker dispersible mortar powder, water-reducing agent, retarder, water-repellent agent, defoamer, steel fiber and crack-resistant fiber are added and stirred evenly for 5-10 minutes. After stopping the machine for 2 minutes, it is sealed in a moisture-proof bag for later use.

10. The method for preparing 3D-printed eco-materials based on raw soil according to claim 9, characterized in that, During construction, the above materials are mixed with water at a ratio of 50%-60% of the weight of the mixture to form a thin paste. The fluidity is controlled at 160mm-180mm, and the mixing time is 2-3 minutes. Then, the mixture is fed into the hopper of the printing equipment. The uniformly mixed raw soil-based slurry material with a certain moisture content is extruded through a screw extruder or air compressor. The time from adding water to stacking and extruding the material to use up the hopper is controlled at 15-20 minutes. The raw soil paste material is continuously and uniformly extruded and stacked layer by layer through the printer nozzle along the path of the designed three-dimensional model coordinate points to finally form a 3D printed building.