Sp2 hybridized nano-composite carbon material with high hardness and superelasticity and preparation method of sp2 hybridized nano-composite carbon material
The sp2 hybrid nanocomposite carbon material prepared by high temperature and high pressure molding method solves the problem of insufficient comprehensive performance of existing sp2 carbon materials, and achieves a combination of high hardness, superelasticity, excellent high temperature oxidation resistance and good conductivity, which is suitable for micro and nano electronic devices and aerospace fields.
Patent Information
- Application Number
- CN202511933715.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-19
- Publication Date
- 2026-04-14
AI Technical Summary
Existing sp2 carbon materials cannot simultaneously meet the comprehensive requirements of high hardness, high elastic recovery rate, excellent high-temperature oxidation stability, good electrical conductivity, and easy preparation into bulk materials, which limits their application in extreme conditions and high-tech fields.
A block structure of sp2 hybrid nanocomposite carbon material composed of amorphous carbon and crystalline graphite clusters was prepared by high temperature and high pressure molding method. The size distribution of crystalline graphite clusters was controlled to be below 10 nm to ensure that the mass ratio of sp2 hybrid carbon atoms was above 90%. The molding was carried out by a six-sided top press or a Kawai large-volume multi-stage anvil device.
It achieves a combination of high Vickers hardness (up to 22 GPa) and ultra-high elastic recovery rate (91~99%), and has good high temperature stability (oxidation temperature ~950℃) and conductivity (~1×105~2×105 S/m), making it suitable for high-end applications such as micro-nano electronic devices and aerospace.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon materials technology, and more particularly to a sp material with high hardness and superelasticity. 2 Hybridized nanocomposite carbon materials and their preparation methods. Background Technology
[0002] Carbon is characterized by its unique sp and sp elements. 2 and sp 3 Hybridization and bonding capabilities have led to the formation of various allotropes, including graphite, diamond, fullerenes, carbon nanotubes, graphene, and amorphous carbon. These diverse carbon materials, possessing high strength, high hardness, excellent electrical and thermal conductivity, and chemical stability, play crucial roles in modern science and industry, such as aerospace, energy storage, electronic devices, and machine tools. Particularly important are sp... 2 Hybridized carbon materials, due to their excellent electrical conductivity, chemical inertness, and tunable mechanical properties, have always been a focus of high-performance materials research. With the increasing demands of industry for material performance under extreme conditions, the development of novel sp materials capable of simultaneously meeting multiple stringent requirements is crucial. 2 Carbon-based materials have become an important development direction in this field.
[0003] However, existing sp 2 Carbon materials often suffer from significant limitations and constraints in terms of performance, making it difficult to achieve a balance of multiple excellent properties. For example, while highly crystalline graphite possesses excellent electrical conductivity and lubricity, its extremely low Vickers hardness (approximately 0.1–0.2 GPa), poor elastic recovery, and tendency to oxidize in air at approximately 400–700°C limit its application in high-temperature, high-strength environments. Although carbon nanotubes and graphene exhibit superior mechanical and electrical properties at the monomer level, the efficient and low-cost fabrication of them into macroscopic bulk materials with consistent properties remains a significant challenge, hindering their widespread industrial application. A more common problem lies in sp... 2 Carbon materials have limited high-temperature oxidation resistance, and most sp... 2 Carbon (including graphite, carbon nanotubes, amorphous carbon, etc.) oxidizes in air at temperatures ranging from 400 to 700°C, which is insufficient for applications requiring higher temperatures. Therefore, improving its intrinsic oxidation resistance is a critical challenge that urgently needs to be addressed. Furthermore, there are often complex interrelationships between a material's electrical conductivity, mechanical properties, and thermal stability. Maintaining or improving electrical conductivity while enhancing the material's mechanical properties and thermal stability is a key challenge. 2 Common challenges faced in the field of carbon materials.
[0004] To overcome the limitations of single materials, researchers have explored various modification methods. For example, CN109573979A discloses a method for molding glassy carbon (an amorphous sp) using high temperature and high pressure. 2 This method uses carbon to improve the performance of glassy carbon. Although it increases the hardness of glassy carbon to about 10 GPa and the elastic recovery rate to 86-90%, its hardness and high-temperature oxidation resistance still need to be further improved. Moreover, the material is essentially still modified amorphous carbon, which limits the improvement of its conductivity.
[0005] In summary, existing SPs 2 Carbon materials, including graphite, carbon nanotubes, graphene, and modified glassy carbon, struggle to simultaneously meet the comprehensive requirements of high hardness, high elastic recovery, excellent high-temperature oxidation stability, good electrical conductivity, and ease of fabrication into bulk materials. This performance limitation severely restricts the development of SP... 2 Applications of carbon materials in extreme conditions and high-tech fields. Summary of the Invention
[0006] This invention provides an sp with high hardness and superelasticity 2 Hybrid nanocomposite carbon materials and their preparation methods are proposed to address the shortcomings of existing technologies that cannot simultaneously meet the comprehensive requirements of high hardness, high elastic recovery rate, excellent high-temperature oxidation stability, good electrical conductivity, and easy preparation into bulk materials.
[0007] This invention provides a carbon material bulk material, comprising: using sp 2 Hybrid carbon raw materials are formed under temperature and pressure, and the sp... 2 The reaction of hybrid carbon raw materials forms a bulk structure mainly composed of amorphous carbon and crystalline graphite clusters; the size distribution of the crystalline graphite clusters is less than 1 nm; sp in the block structure 2 Hybridized carbon atoms account for more than 90% of the total mass.
[0008] According to the carbon material bulk provided by the present invention, the size of the crystalline graphite clusters is 2~10 nm.
[0009] Preferably, the volume content of the crystalline graphite clusters in the bulk structure is 10-90%.
[0010] More preferably, the volume content of the crystalline graphite clusters in the bulk structure is 20% or more, and the volume content of the amorphous carbon matrix is 20% or more.
[0011] More preferably, the total volume content of other structures in the block structure is less than 10%, and the other structures include sp 3 Hybridized carbon, non-carbon impurity elements, and the aforementioned sp2 Hybrid carbon feedstock.
[0012] According to the carbon material block provided by the present invention, the molding under temperature and pressure includes high temperature and high pressure molding, wherein the pressure of the high temperature and high pressure molding is 5~15GPa; and the heat preservation temperature of the high temperature and high pressure molding is 400~1800℃.
[0013] According to the carbon material block provided by the present invention, the temperature control process of the high temperature and high pressure forming includes: heating to the holding temperature, holding for a time t, and cooling down after the holding is completed; wherein, the value of t is 30~120min, the heating rate is 60~200℃ / min, and the cooling rate is 60~200℃ / min or direct quenching.
[0014] According to the carbon material bulk body provided by the present invention, the sp 2 Hybrid carbon raw materials are selected from graphite, graphene, and fullerene C. 60 One or more of the following: carbon nanotubes, amorphous carbon; preferably, the sp 2 The hybrid carbon feedstock is fullerene C 60 powder.
[0015] According to the carbon material bulk body provided by the present invention, the volume of the bulk structure is 20 mm. 3 The above is preferably 20~1000mm 3 More preferably, the block structure is a cylinder with a height of 3-10 mm and a diameter of 3-10 mm.
[0016] According to the carbon material bulk body provided by the present invention, the sp 2 The hybrid carbon raw material is pre-compressed before being formed, the pre-compressing including the sp 2 The hybrid carbon raw material is formed into a preform under a pressure of 5~100MPa, and the size of the preform is consistent with the size of the sample cavity during molding. Preferably, the molding is performed after the blank is dried to a constant weight.
[0017] According to the carbon material block provided by the present invention, the molding is carried out by a six-sided top press or a Kawai large-volume multi-stage pressing anvil device, and the assembly method is single-stage assembly or two-stage assembly.
[0018] Secondly, the present invention also provides a method for preparing the carbon material bulk as described above, comprising: using sp 2 Hybrid carbon raw materials are formed under temperature and pressure, and the sp... 2 The reaction of hybrid carbon feedstocks forms a bulk structure mainly composed of amorphous carbon and crystalline graphite clusters.
[0019] Thirdly, the present invention also provides a composite material, comprising the carbon material block as described above or the carbon material block prepared by the preparation method as described above, or particles or powder obtained by processing the carbon material block.
[0020] The present invention provides a sp with high hardness and superelasticity 2 Hybridized nanocomposite carbon materials and their preparation methods, through the control of pressure, temperature, and temperature regulation processes in the high-temperature and high-pressure synthesis steps, achieved sp... (the text abruptly ends here, likely due to an incomplete sentence or missing information). 2 The preparation of hybrid carbon materials, which possess a unique nanocomposite structure with uniformly alternating distribution of crystalline graphite clusters and amorphous carbon phases, wherein the size distribution of the crystalline graphite clusters is less than 10 nm, giving them excellent comprehensive performance and great application potential in high-tech fields such as micro-nano electronic devices and aerospace.
[0021] The method provided by this invention has abundant raw material sources, uses mature high-temperature and high-pressure equipment, is simple to operate, has easy-to-control high-pressure synthesis conditions, and a simple process route, and has the potential for large-scale industrial production. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in this invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0023] Figure 1 This is one of the test result diagrams of the carbon material block obtained in Example 1 of the present invention.
[0024] Figure 2 This is the second image showing the test results of the carbon material block obtained in Example 1 of the present invention.
[0025] Figure 3 This is the third figure showing the test results of the carbon material block obtained in Example 1 of the present invention.
[0026] Figure 4 This is the fourth figure showing the test results of the carbon material block obtained in Example 1 of the present invention.
[0027] Figure 5 This is the fifth figure showing the test results of the carbon material block obtained in Example 1 of the present invention.
[0028] Figure 6 This is Figure 6, which shows the test results of the carbon material block obtained in Example 1 of the present invention.
[0029] Figure 7 This is one of the test result diagrams of the carbon material block obtained in Example 2 of the present invention.
[0030] Figure 8 This is the second image showing the test results of the carbon material block obtained in Example 2 of the present invention.
[0031] Figure 9 This is the third figure showing the test results of the carbon material block obtained in Example 2 of the present invention.
[0032] Figure 10 This is the fourth figure showing the test results of the carbon material block obtained in Example 2 of the present invention.
[0033] Figure 11 This is the fifth figure showing the test results of the carbon material block obtained in Example 2 of the present invention.
[0034] Figure 12 This is one of the test result diagrams of the carbon material block obtained in Comparative Example 1 provided by the present invention.
[0035] Figure 13 This is the second image showing the test results of the carbon material block obtained in Comparative Example 1 provided by the present invention.
[0036] Figure 14 This is the third figure showing the test results of the carbon material block obtained in Comparative Example 1 provided by the present invention. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0038] In a specific embodiment of the present invention, a carbon material bulk material is first provided, comprising: using sp 2 Hybrid carbon raw materials are formed under temperature and pressure, and the sp... 2 The reaction of hybrid carbon raw materials forms a bulk structure mainly composed of amorphous carbon and crystalline graphite clusters; the size distribution of the crystalline graphite clusters is less than 10 nm. sp in the block structure 2 The mass percentage of hybrid carbon atoms is over 90%. As an example, in the bulk structure, sp... 2The mass percentage of hybrid carbon atoms can also be any value or a range of values from 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, and 99%.
[0039] The amorphous carbon exhibits disordered sp. 2 Hybrid state.
[0040] The crystalline graphite clusters exhibit ordered sp... 2 Hybrid state.
[0041] In the aforementioned bulk structure, from a microscopic perspective (specifically, observation using instruments such as scanning electron microscopy or transmission electron microscopy), the material contains multiple phase structures separated by clearly defined interfaces. Its unique microstructure is mainly composed of crystalline graphite clusters (ordered sp... 2 Hybridized) and amorphous carbon (disordered sp) 2 The two phases are not simply physically mixed, but rather formed into a uniform, alternating nanocomposite structure through the action of temperature and pressure.
[0042] The carbon material bulk in this invention can also be referred to as sp. 2 Hybridized superelastic nanocomposite carbon materials.
[0043] In this invention, "bulk" material is understood as a single material body with a certain macroscopic size that can exist independently, and its volume is at least 1 mm. 3 For example, it can reach at least 5mm 3 At least 10mm 3 At least 20mm 3 At least 50mm 3 At least 100mm 3 At least 200mm 3 At least 500mm 3 Even at least 1000mm 3 Or even larger. The upper limit of the volume of bulk materials is mainly limited by the effective cavity size and process uniformity control capability of the high-temperature and high-pressure synthesis equipment used, and can be selected according to actual needs and equipment processing capabilities.
[0044] This application's sp 2Hybrid high-hardness and superelastic nanocomposite carbon materials possess a unique structure composed of uniformly interwoven nanocrystalline graphite clusters and amorphous carbon phases. The size distribution of the nanocrystalline graphite clusters plays a crucial role in elastic recovery. By optimizing the size distribution of the nanocrystalline graphite clusters to below 10 nm, the resulting bulk carbon material exhibits excellent comprehensive properties, particularly the unique combination of high Vickers hardness (up to 22 GPa) and ultra-high elastic recovery rate (91-99%). It also possesses good high-temperature stability (oxidation temperature ~950℃) and electrical conductivity (~1×10⁻⁶). 5 ~2×10 5 (S / m), thereby meeting the specific needs of various high-end applications, from micro-nano electronic devices to aerospace.
[0045] In some specific embodiments of the present invention, the size of the crystalline graphite cluster is 2~10 nm. As an example, the size of the crystalline graphite cluster can also be any value or a range of values from 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, and 10 nm.
[0046] In some specific embodiments of the present invention, the volume content of the crystalline graphite clusters in the bulk structure is 10-90%. As an example, the volume content of the crystalline graphite clusters in the bulk structure can also be any value or a range of any values from 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, and 90%.
[0047] More preferably, the volume content of the crystalline graphite clusters in the bulk structure is 20% or more, and the volume content of the amorphous carbon matrix is 20% or more.
[0048] More preferably, the total volume content of other structures in the block structure is less than 10%, and the other structures include sp 3 Hybridized carbon, non-carbon impurity elements, and the aforementioned sp 2 Hybrid carbon feedstock.
[0049] By precisely controlling the high-temperature and high-pressure synthesis parameters (pressure, temperature, and holding time) in the preparation method of this invention, the relative volume ratio of crystalline graphite phase and amorphous carbon phase in the final material can be effectively controlled. This ratio can vary within a wide range; for example, depending on the target performance requirements, the volume content of the crystalline graphite phase can be designed to range from approximately 10% to approximately 90%, while the corresponding volume content of the amorphous carbon phase varies between approximately 90% and approximately 10%. Typically, to achieve a good combination of superelasticity and high hardness, both phases are present significantly (e.g., neither is less than 20%). This adjustability of the phase composition ratio allows technicians to design and prepare sp materials with different performance emphases (e.g., more emphasis on hardness, more emphasis on elastic recovery, or a balance of conductivity) according to specific application requirements. 2 The ability to create hybrid superelastic nanocomposite carbon materials.
[0050] Those skilled in the art will understand that the sp of this application 2 Hybridized high-hardness and superelastic nanocomposite carbon materials may contain trace amounts of other carbon structural phases (e.g., residual raw material phases, trace amounts of sp) due to the purity of the starting materials or unavoidable introduction during the manufacturing process. 3 Hybridized carbon (or other forms of carbon) or non-carbon impurity elements. The content of these non-major components is usually very low and does not affect the basic structural characteristics and main properties of the material, which are dominated by the uniform alternation of crystalline graphite clusters and amorphous carbon. The sp 2 and sp 3 Hybrid carbon structure phases can be quantitatively evaluated by analyzing the fine structure of the carbon K-edge (such as the relative intensities of π* and σ* peaks) using electron energy loss spectroscopy (EELS).
[0051] The determination of the volume fraction can be performed by those skilled in the art using conventional material characterization techniques. For example, a preferred method is to observe multiple representative micro-regions within the material using a high-resolution transmission electron microscope, distinguish and statistically analyze the area fractions of crystalline graphite regions and amorphous carbon regions, and then take the average value of multiple regions to estimate the volume fraction of the two phases.
[0052] In some specific embodiments of the present invention, the molding under temperature and pressure includes high-temperature high-pressure molding, wherein the pressure of the high-temperature high-pressure molding is 5~15 GPa. As an example, the pressure of the high-temperature high-pressure molding can also be any value or a range of any values among 5 GPa, 6 GPa, 7 GPa, 8 GPa, 9 GPa, 10 GPa, 11 GPa, 12 GPa, 13 GPa, 14 GPa, and 15 GPa.
[0053] In some specific embodiments of the present invention, the holding temperature for high-temperature and high-pressure molding is 400~1800℃. As an example, the holding temperature for high-temperature and high-pressure molding can also be any value or a range of values from 400℃, 500℃, 600℃, 700℃, 800℃, 900℃, 1000℃, 1100℃, 1200℃, 1300℃, 1400℃, 1500℃, 1600℃, 1700℃, and 1800℃.
[0054] In some specific embodiments of the present invention, the temperature control process of the high-temperature and high-pressure forming includes: heating to the holding temperature, holding for a time t, and cooling down after the holding is completed; wherein, t is 30~120 min, the heating rate is 60~200℃ / min, and the cooling rate is 60~200℃ / min or direct quenching.
[0055] By precisely controlling the pressure, temperature, and temperature control process in the high-temperature and high-pressure synthesis step, the ratio, distribution, and microstructure of crystalline graphite clusters and amorphous carbon within the obtained nanocomposite carbon material can be controlled, thereby achieving the regulation of its properties.
[0056] As an example, the value of t can also be any value or a range of values among 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, and 120min.
[0057] As an example, the heating rate can also be any value or a range of values from 60℃ / min, 70℃ / min, 80℃ / min, 90℃ / min, 100℃ / min, 110℃ / min, 120℃ / min, 130℃ / min, 140℃ / min, 150℃ / min, 160℃ / min, 170℃ / min, 180℃ / min, 190℃ / min, and 200℃ / min.
[0058] As an example, the cooling rate can also be any value or a range of values from 60℃ / min, 70℃ / min, 80℃ / min, 90℃ / min, 100℃ / min, 110℃ / min, 120℃ / min, 130℃ / min, 140℃ / min, 150℃ / min, 160℃ / min, 170℃ / min, 180℃ / min, 190℃ / min, and 200℃ / min.
[0059] In some specific embodiments of the present invention, the sp 2 Hybrid carbon raw materials are selected from graphite, graphene, and fullerene C. 60One or more of the following: carbon nanotubes, amorphous carbon; preferably, the sp 2 The hybrid carbon feedstock is fullerene C 60 powder.
[0060] In some specific embodiments of the present invention, the volume of the block structure is 20 mm. 3 The above is preferably 20~1000mm 3 More preferably, the block structure is a cylinder with a height of 3-10 mm and a diameter of 3-10 mm.
[0061] In some specific embodiments of the present invention, the sp 2 The hybrid carbon raw material is pre-compressed before being formed, the pre-compressing including the sp 2 The hybrid carbon raw material is pressed into a preform under a pressure of 5~100MPa, and the size of the preform is consistent with the size of the sample cavity during molding.
[0062] In some specific embodiments of the present invention, the molding is performed after the blank is dried to a constant weight.
[0063] As an example, the drying temperature is 120~180℃, and the drying time is 1~3h.
[0064] In some specific embodiments of the present invention, the molding is performed using a six-sided top press or a Kawai large-volume multi-stage anvil device, and the assembly method is either single-stage assembly or two-stage assembly.
[0065] Preferably, the assembly structure is 14 / 8 or 10 / 5.
[0066] As an example, the six-sided top press can be a domestically produced hinged six-sided top press.
[0067] In a specific embodiment of the present invention, a method for preparing the carbon material bulk as described above is also provided, comprising: using sp 2 Hybrid carbon raw materials are formed under temperature and pressure, and the sp... 2 The reaction of hybrid carbon feedstocks forms a bulk structure mainly composed of amorphous carbon and crystalline graphite clusters.
[0068] In some specific embodiments of the present invention, the preparation method includes the following steps: (1) Sp 2 The hybrid carbon raw material is pre-pressed to form a green body; (2) Place the blank obtained in step (1) into a crucible, and then make it into an assembly for high temperature and high pressure experiment. Dry the assembly. (3) The dried assembly from step (2) is placed in a high-temperature and high-pressure equipment for high-temperature and high-pressure synthesis to obtain a black, opaque carbon material block.
[0069] In some specific embodiments of the present invention, the preparation method includes the following steps: (1) Sp 2 Hybrid carbon raw materials are pre-pressed in tungsten carbide molds to form cylindrical or other desired shapes of blanks; (2) The blank obtained in step (1) is placed in a boron nitride crucible and then loaded into a high-temperature and high-pressure synthesis chamber to make an assembly for high-temperature and high-pressure experiments. The assembly is then placed in a drying oven for drying. (3) Take out the dried assembly from step (2) and cool it to room temperature. Then put it into a high temperature and high pressure device for high temperature and high pressure synthesis experiment.
[0070] (4) After the high temperature and high pressure molding is completed, the sample is first cooled to room temperature, then the pressure is slowly released, and finally it is taken out from the synthesis chamber and assembled to obtain a black opaque carbon material block.
[0071] In some specific embodiments of the present invention, in step (1), sp can be adjusted as needed. 2 The hybrid carbon raw material undergoes purification treatment.
[0072] In some specific embodiments of the present invention, in step (2), a typical assembly may include: an external pressure transmission medium (such as pyrophyllite or magnesium oxide), an internal heating element (such as graphite or metal tube), a heat insulation material (such as zirconium oxide or magnesium oxide sheath), and a thermocouple for measuring temperature. The entire assembly is then placed in an oven for drying.
[0073] In some specific embodiments of the present invention, in step (3), pressure can be gradually applied to the target synthesis pressure according to the set program. After the pressure stabilizes, the sample is heated by the heating element to the target synthesis temperature. After the target pressure and temperature are reached, the constant pressure and temperature are maintained for heat preservation treatment.
[0074] In a specific embodiment of the present invention, a composite material is also provided, comprising the carbon material block as described above, or the carbon material block prepared by the preparation method described above, or particles or powder obtained by processing the carbon material block.
[0075] Preferably, the carbon material block has a Vickers hardness of 20 GPa or higher, an indentation elastic recovery rate of 90% or higher, an initial oxidation temperature of approximately 900°C or higher, and a room temperature electrical conductivity of 1×10⁻⁶. 5 S / m or higher.
[0076] The following is combinedFigures 1-14 The sp describing the present invention 2 Hybridized high-hardness and superelastic nanocomposite carbon materials and their preparation methods. Where specific techniques or conditions are not specified in the examples, they were performed according to the techniques or conditions described in the literature in this field, or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.
[0077] The source or parameter information of some raw materials and equipment is as follows: Fullerene C 60 Powder: High purity (>99.5%) produced by Alfaisa Chemicals Ltd.
[0078] The domestically produced hinged six-sided top press is model HD-XH (GY420).
[0079] Vickers hardness tester: QATM Qness 60 A + EVO.
[0080] X-ray diffractometer: XRD, model D8 Discover, Bruker, Germany.
[0081] High-resolution transmission electron microscope: HRTEM, Talos F200S, Thermo Fisher Scientific, USA.
[0082] Nanoindenter: Agilent Nano Indenter G200.
[0083] Thermogravimetric-Differential Scanning Calorimeter: TGA-DSC, Mettler Toledo TGA / DSC3+.
[0084] Example 1 A method for preparing a bulk carbon material, comprising the following steps: (1) Weigh out fullerene C 60 The powder was loaded into a tungsten carbide mold with an inner diameter of 4 mm, and a pressure of approximately 50 MPa was applied at room temperature using a small hydraulic press for 1 minute. 60 The powder is pre-pressed into a cylindrical blank with a diameter of 4 mm and a height of about 3 mm.
[0085] (2) Place the cylindrical blank obtained in step (1) into a high-purity boron nitride crucible. Then, place this boron nitride crucible in a standard 14 / 8 high-temperature and high-pressure synthesis assembly, and place the entire assembly in an oven at 150°C for 2 hours to remove adsorbed moisture.
[0086] (3) Place the dried and cooled assembly to room temperature into the center of the cavity of a domestic hinged six-sided press. Set the high temperature and high pressure parameters as follows: pressure 8 GPa; heat to 1000℃ at a rate of 60℃ / min, hold pressure and temperature for 60 min, stop heating and allow the sample to cool naturally to room temperature, then slowly depressurize, remove the assembly and disassemble it to obtain a black, opaque, dense blocky sp. 2 Hybridized superelastic nanocomposite carbon materials.
[0087] The resulting blocky sp 2 Hybridized superelastic nanocomposite carbon materials were cut and polished, and phase analysis was performed using X-ray diffraction. The results are as follows: Figure 1 As shown, from Figure 1 It can be seen that the sample is mainly composed of broadened amorphous diffraction peaks and characteristic peaks belonging to nanocrystalline graphite (such as the (002) peak), indicating that the sample is a composite material composed of amorphous carbon and nanocrystalline graphite.
[0088] Furthermore, the microstructure of the sample was observed using a high-resolution transmission electron microscope, and the results are as follows: Figure 2 As shown, the presence of crystalline graphite clusters with a size of 2–4 nm uniformly dispersed in the amorphous carbon matrix was confirmed. Simultaneously, electron energy loss spectroscopy (EELS) analysis of the carbon K absorption edge revealed... Figure 3 As shown, this displays a typical sp 2 Hybridized carbon characteristics (strong π* peak), quantitative analysis indicates sp 2 Hybridized carbon atoms dominate (sp 2 =95±1%). Among them, the volume content of crystalline graphite clusters is more than 20%, and the volume content of amorphous carbon is more than 20%.
[0089] Furthermore, an indentation test was performed on the polished surface of the sample using a Vickers hardness tester under a load of 9.8 N (1 kgf), and the results are as follows. Figure 4 As shown, the Vickers hardness value was measured to be 22 ± 0.9 GPa.
[0090] The load-depth curve of the sample was obtained using a nanoindenter, and the results are as follows: Figure 5 As shown, the calculated elastic recovery rate of the indentation is as high as 97±1%, and the Young's modulus is 144.0±1GPa.
[0091] The test was conducted using a thermogravimetric-differential scanning calorimeter in air at a heating rate of 10 °C / min. The results are as follows: Figure 6 As shown, the material exhibits excellent high-temperature oxidation resistance, with an initial oxidation temperature of approximately 950°C.
[0092] Its room temperature conductivity, measured using the four-probe method, is approximately 1.8 × 10⁻⁶. 5 S / m.
[0093] Example 2 A method for preparing a carbon material bulk, the steps of which are basically the same as those in Example 1, except that: the parameters for high temperature and high pressure are set as follows: the pressure is 15 GPa; the temperature is increased to 1200℃ at a rate of 150℃ / min, the pressure is maintained for 30 min, and after heating is stopped, the sample is cooled to room temperature at a rate of 200℃ / min and then the pressure is slowly released.
[0094] The resulting blocky sp 2 The hybrid superelastic nanocomposite carbon material was cut and polished before testing, and the results were as follows: The XRD analysis results are similar to those in Example 1, such as... Figure 7 As shown, it appears to be a composite phase of amorphous carbon and nanocrystalline graphite, but the characteristic peaks of graphite may be more pronounced, resulting in a narrower peak width.
[0095] HRTEM observation, such as Figure 8 As shown, crystalline graphite clusters with a size of approximately 4–8 nm were confirmed to be uniformly distributed within the amorphous carbon matrix. The volume content of the crystalline graphite clusters was greater than 20%, and the volume content of the amorphous carbon was greater than 20%.
[0096] Analysis of the carbon K absorption edge using EELS, such as Figure 9 As shown, quantitative analysis indicates that sp 2 Hybridized carbon atoms dominate (sp 2 =93±1%.
[0097] Furthermore, an indentation test was performed on the polished surface of the sample using a Vickers hardness tester under a load of 9.8 N (1 kgf), and the results are as follows. Figure 10 As shown, the Vickers hardness value was measured to be 15±1 GPa.
[0098] The load-depth curve of the sample was obtained using a nanoindenter, and the test results are as follows: Figure 11 As shown, the calculated elastic recovery rate of the indentation is as high as 94±1%, and the Young's modulus is 107.6±1GPa.
[0099] Its room temperature conductivity, measured using the four-probe method, is approximately 2.0 × 10⁻⁶. 5 S / m.
[0100] Compared to Example 1, the blocky sp obtained in this example 2 In the hybrid superelastic nanocomposite carbon material, the size of the graphite crystal clusters is slightly increased, while the hardness and Young's modulus are slightly decreased, and the elastic recovery rate of the material is slightly reduced, but still remains at an extremely high level. This indicates that the structure and properties of the material can be fine-tuned by controlling the synthesis parameters.
[0101] Comparative Example 1 A method for preparing a carbon material bulk, the steps of which are basically the same as those in Example 1, except that: the parameters for high temperature and high pressure are set as follows: the pressure is 5 GPa; the temperature is increased to 1600℃ at a rate of 150℃ / min, the pressure is maintained for 30 min, and after heating is stopped, the sample is cooled to room temperature at a rate of 200℃ / min and then the pressure is slowly released.
[0102] The obtained bulk sp2 hybrid carbon material was cut and polished before testing, and the results were as follows: The XRD analysis results are similar to those of Examples 2 and 3, such as... Figure 12 As shown, it appears to be a composite phase of amorphous carbon and nanocrystalline graphite, but the characteristic peaks of graphite may be more pronounced, resulting in a narrower peak width.
[0103] HRTEM observation, such as Figure 13 As shown, crystalline graphite clusters with sizes of approximately 5–20 nm are confirmed to exist within the amorphous carbon matrix. In some regions, due to the excessively large cluster size, clusters approach each other and even fuse. The volume content of crystalline graphite clusters is over 20%, and the volume content of amorphous carbon is over 20%.
[0104] The load-depth curve of the sample was obtained using a nanoindenter, and the test results are as follows: Figure 14 As shown, the calculated elastic recovery rate of the indentation is 75±1%, and the Young's modulus is 61±1 GPa.
[0105] Compared to Example 1, the blocky sp prepared in this comparative example... 2 In hybrid carbon materials, the size of graphite crystal clusters increases significantly, and the clusters exhibit structural features of mutual proximity and fusion, resulting in a significant decrease in the Young's modulus and elastic recovery rate. This indicates that the structure, spatial distribution, and interconnection state of graphite clusters have a significant impact on the material properties.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A carbon material bulk, characterized in that, include: Using sp 2 Hybrid carbon raw materials are formed under temperature and pressure, and the sp... 2 The reaction of hybrid carbon raw materials forms a bulk structure mainly composed of amorphous carbon and crystalline graphite clusters; the size distribution of the crystalline graphite clusters is less than 10 nm. sp in the block structure 2 Hybridized carbon atoms account for more than 90% of the total mass.
2. The carbon material bulk body according to claim 1, characterized in that, The size distribution of the crystalline graphite clusters is 2~10 nm; Preferably, the volume content of the crystalline graphite clusters in the bulk structure is 10-90%; More preferably, the volume content of the crystalline graphite clusters in the bulk structure is 20% or more, and the volume content of the amorphous carbon matrix is 20% or more; More preferably, the total volume content of other structures in the block structure is less than 10%, and the other structures include sp 3 Hybridized carbon, non-carbon impurity elements, and the aforementioned sp 2 Hybrid carbon feedstock.
3. The carbon material bulk body according to claim 1 or 2, characterized in that, The molding under temperature and pressure includes high-temperature high-pressure molding, wherein the pressure of the high-temperature high-pressure molding is 5~15GPa; and the heat preservation temperature of the high-temperature high-pressure molding is 400~1800℃.
4. The carbon material bulk body according to any one of claims 1 to 3, characterized in that, The temperature control process of the high-temperature and high-pressure forming includes: heating to the holding temperature, holding for a time t, and cooling down after the holding period; wherein, t is 30~120min, the heating rate is 60~200℃ / min, and the cooling rate is 60~200℃ / min or direct quenching.
5. The carbon material bulk body according to any one of claims 1 to 4, characterized in that, The sp 2 Hybrid carbon raw materials are selected from graphite, graphene, and fullerene C. 60 One or more of the following: carbon nanotubes, amorphous carbon; preferably, the sp 2 The hybrid carbon feedstock is fullerene C 60 powder.
6. The carbon material bulk body according to any one of claims 1 to 5, characterized in that, The volume of the block structure is 20 mm. 3 The above is preferably 20~1000mm 3 More preferably, the block structure is a cylinder with a height of 3-10 mm and a diameter of 3-10 mm.
7. The carbon material bulk body according to any one of claims 1 to 6, characterized in that, The sp 2 The hybrid carbon raw material is pre-compressed before being formed, the pre-compressing including the sp 2 The hybrid carbon raw material is formed into a preform under a pressure of 5~100MPa, and the size of the preform is consistent with the size of the sample cavity during molding. Preferably, the molding is performed after the blank is dried to a constant weight.
8. The carbon material bulk body according to any one of claims 1 to 7, characterized in that, The molding process employs a six-sided top press or a Kawai large-volume multi-stage anvil device, and the assembly method is either single-stage assembly or two-stage assembly.
9. A method for preparing the carbon material bulk according to any one of claims 1 to 8, characterized in that, include: Using sp 2 Hybrid carbon raw materials are formed under temperature and pressure, and the sp... 2 The reaction of hybrid carbon feedstocks forms a bulk structure mainly composed of amorphous carbon and crystalline graphite clusters.
10. A composite material, characterized in that, Includes the carbon material block as described in any one of claims 1 to 8, or the carbon material block prepared by the preparation method described in claim 9, or particles or powder obtained by processing the carbon material block.
Citation Information
Patent Citations
Novel glassy carbon preparation method
CN109573979A