High-molecular adhesion promoter, preparation method thereof and conductive metal slurry
By introducing a polymeric adhesion promoter into the conductive paste and using PVB resin and isocyanate curing agent to form a cross-linking network, the problem of insufficient adhesion of conductive paste on silicon wafers was solved, achieving high adhesion and stable printing results.
Patent Information
- Application Number
- CN202610118501.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-28
- Publication Date
- 2026-04-14
AI Technical Summary
When existing conductive pastes are used to print gate lines on silicon wafers, insufficient adhesion leads to problems such as powder shedding, gate detachment, and line breakage. Existing small molecule coupling agents have limited improvement, while the solubility of polymeric adhesion promoters is limited, and their improvement ability is also limited.
By using a polymeric adhesion promoter, a high-boiling-point lipid solvent and isocyanate curing agent are added to PVB resin to prepare an adhesion promoter with a PVB backbone and a urea crosslinking network, which enhances the adhesion and crosslinking density between the metal paste and the substrate.
The adhesion of conductive silver paste after drying was improved to over 2.1 N/mm2, which enhanced the overall adhesion and bonding strength of the metal paste, prevented powdering, and improved printability and stability.
Smart Images

Figure CN121851316A_ABST
Abstract
Description
Technical Field
[0001] This disclosure belongs to the field of conductive paste technology, specifically relating to a polymeric adhesion promoter and its preparation method, and a conductive metal paste. Background Technology
[0002] Currently, most conductive pastes on the market, especially photovoltaic silver paste products, are facing increasingly stringent requirements for cost reduction and efficiency improvement. The printing of grid lines on silicon wafers is becoming increasingly narrow, leading to a significant reduction in the contact area between the grid lines and the silicon wafer. This results in insufficient adhesion during processing and manufacturing, causing defects such as powder shedding, grid detachment, and wire breakage. Therefore, it is necessary to improve the adhesion of the grid lines after drying and sintering.
[0003] In existing technologies, photovoltaic silver paste mainly improves adhesion by adding small-molecule additives, such as silane coupling agents, titanate coupling agents, or polyester and acrylic adhesion promoters. However, these existing technologies still have many problems. For example, small-molecule coupling agents mainly improve the interaction strength at the interface between the metal paste and the silicon wafer, but are insufficient in improving the adhesion strength inside the grid lines. Excessive addition can easily lead to powder agglomeration, forming large particles that affect printability. The specific mechanism is that silane or titanate groups are hydrolyzed in polar solvents such as alcohols to become hydroxyl groups, which then form hydrogen bonds with the hydroxyl groups on the surface of the silicon wafer substrate, increasing the crosslinking density and thus improving adhesion. However, because the coupling agent has a small molecular weight and short chain, its interaction with the organic carrier resin is limited, so the grid lines are prone to cracking and detachment from the inside, or powder shedding. Conventional polymeric adhesion promoters, such as SK's polyester promoters, mainly enhance adhesion by utilizing the hydrogen bonding between ester groups in the middle of the molecular chain. However, the hydrogen bonding of ester groups is weaker than that of hydroxyl and amino groups. At the same time, due to their high crystallinity, their solubility is limited, thus limiting their ability to improve adhesion. Summary of the Invention
[0004] This disclosure aims to at least solve one of the technical problems existing in the prior art, and to provide a polymeric adhesion promoter and its preparation method, as well as a conductive metal paste.
[0005] In one aspect, this disclosure provides a polymeric adhesion promoter, the structural formula of which is as follows: Wherein, n ranges from 60 to 85 mol%, x ranges from 3 to 10 mol%, y ranges from 10 to 20 mol%, and z ranges from 1 to 10 mol%.
[0006] Optionally, the polymeric adhesion promoter has the structural formula of any one of the following: z = 1 mol% (Equation 1); z = 1 mol% (Equation 2); z = 1 mol% (Equation 3); z = 2 mol% (Equation 4); z = 4mol% (Equation 5).
[0007] In another aspect, this disclosure provides a method for preparing a polymeric adhesion promoter, the method comprising: A high-boiling-point lipid solvent is added to PVB resin, and the mixture is heated and stirred until completely dissolved to obtain a PVB resin solution. An isocyanate curing agent was added to the PVB resin solution, and after stirring, the solution was cooled to room temperature to obtain a polymeric adhesion promoter.
[0008] Optionally, the content ratio of the PVB resin, the isocyanate curing agent, and the high-boiling-point lipid solvent is (16-19):(1-4):80.
[0009] Optionally, the ratio of the PVB resin to the isocyanate curing agent is 19:(1-4).
[0010] Optionally, the isocyanate curing agent is any one of hexamethylene diisocyanate, toluene diisocyanate, and diphenylmethane diisocyanate.
[0011] Optionally, the high-boiling-point lipid solvent is any one of diethylene glycol butyl ether acetate, diethylene glycol butyl ether, polyoxymethylene dimethyl ether, butyl carbohydrin, dodecyl alcohol ester, hexadecyl alcohol ester, dimethyl adipate, and dibutyl phthalate.
[0012] Optionally, a high-boiling-point lipid solvent is added to the PVB resin and heated and stirred at a temperature of 85-95℃ and a stirring speed of 750-850 r / min.
[0013] In another aspect of this disclosure, a conductive metal paste is provided, the conductive metal paste comprising: 80-92 parts by weight of silver powder; 1-3 parts by weight of glass powder; 6-12 parts by weight of organic carrier; 0.1-3 parts by weight of a polymeric adhesion promoter, wherein the polymeric adhesion promoter is the polymeric adhesion promoter described above.
[0014] Optionally, the conductive metal paste has a viscosity of 80-102 Pa·s and an adhesion pull force of 2.1-2.8 N / mm. 2 The viscosity increase rate over 24 hours is 4.5-6.5%.
[0015] This disclosure presents a polymeric adhesion promoter and its preparation method, as well as a conductive metal paste. The structural formula of the polymeric adhesion promoter is as follows: Wherein, n ranges from 60-85 mol%, x ranges from 3-10 mol%, y ranges from 10-20 mol%, and z ranges from 1-10 mol%. The polymeric adhesion promoter disclosed herein can simultaneously enhance the adhesion between the metal paste and the substrate, as well as the cross-linking density within the paste, thereby improving the overall adhesion of the paste. This results in an adhesion of conductive silver paste of 2.1 N / mm² after drying. 2 The above results. Attached Figure Description
[0016] Figure 1 A flowchart illustrating the preparation method of the polymeric adhesion promoter according to a specific embodiment of this disclosure; Figure 2 These are schematic diagrams illustrating the grid line adhesion test levels of Embodiments 1-5 and Comparative Examples 1-3 of this disclosure; wherein, Figure 2 (a) in the text refers to a tensile force greater than 2 N / mm. 2 ; Figure 2 (b) in the figure represents a tensile force of 1-2 N / mm. 2 ; Figure 2 (c) in the figure represents a tensile force of 0-1 N / mm. 2 . Detailed Implementation
[0017] To enable those skilled in the art to better understand the technical solutions of this disclosure, the disclosure will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain this disclosure and represent a part of the embodiments of this disclosure, not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without creative effort are within the protection scope of this disclosure.
[0018] In one aspect, this disclosure provides a polymeric adhesion promoter, which is:
[0019] Wherein, n ranges from 60 to 85 mol%, x ranges from 3 to 10 mol%, y ranges from 10 to 20 mol%, and z ranges from 1 to 10 mol%.
[0020] It should be noted that, in polymeric adhesion promoters, based on a total conversion of 100 mol%, different scales can be used to prepare materials with different molecular weights when the proportions of various monomers in the polymer material are the same.
[0021] In this embodiment, the main chain segment of the polymeric adhesion promoter is based on the acetal structure of PVB resin, providing good flexibility and coating ability for metal powders, ensuring compatibility with the silver paste system. Secondly, the promoter also has hydroxyl groups, crosslinking groups, and functional side chains. Among them, the hydroxyl groups (-OH) retained in the PVB chain segment can form hydrogen bonds with the hydroxyl groups on the surface of silver powder, enhancing the anchoring effect on the metal powder and improving the dispersion stability of the paste. Through the reaction of isocyanate with hydroxyl groups, a urea group (-NH-CO-NH-) crosslinking structure is formed between the molecular chains, constructing a three-dimensional network, improving the cohesive strength of the silver paste after curing, and preventing powder shedding. The amino group (-NH-) in the urea group can form strong hydrogen bonds with the hydroxyl groups on the surface of the substrate (such as silicon wafer). At the same time, the R1 group (methylene chain, ether bond, or benzene ring) balances adhesion and printability by adjusting the rigidity or flexibility of the chain segment.
[0022] In some preferred embodiments, the polymeric adhesion promoter has the structural formula of any of the following: z = 1 mol% (Equation 1); z = 1 mol% (Equation 2); z = 1 mol% (Equation 3); z = 2 mol% (Equation 4); z = 4mol% (Equation 5).
[0023] It should be noted that the ranges of n, x, and y in the above structural formula (1-5) are consistent with the general structural formula given above, that is, the range of n is 60-85 mol%, the range of x is 3-10 mol%, and the range of y is 10-20 mol%.
[0024] like Figure 1 As shown, another aspect of this disclosure provides a method S100 for preparing a polymeric adhesion promoter, specifically including the following steps S110~S120: S110. Add a high-boiling-point lipid solvent to PVB resin, and heat and stir until completely dissolved to obtain a PVB resin solution. S120. Add isocyanate curing agent to PVB resin solution, continue stirring for 1-3 hours, and then cool to room temperature to obtain polymeric adhesion promoter.
[0025] In some preferred embodiments, the content ratio of PVB resin, isocyanate curing agent and the high-boiling-point lipid solvent is (16-19):(1-4):80. For example, the PVB resin can preferably be 16 parts by mass, 17 parts by mass, 18 parts by mass, 19 parts by mass, etc., the high-boiling-point lipid solvent and isocyanate curing agent can preferably be 1 part by mass, 2 parts by mass, 3 parts by mass, 4 parts by mass, etc., the high-boiling-point lipid solvent can preferably be 80 parts by mass, and the total content is 100 parts by mass.
[0026] As a further preferred embodiment, the ratio of PVB resin to the isocyanate curing agent is 19:(1-4).
[0027] In some other preferred embodiments, the structural formula of the polyvinyl butyral (PVB) resin is as follows: .
[0028] This type of PVB resin is a commonly used resin in photovoltaic silver paste. It has good compatibility and strong flexibility. The hydroxyl groups in this resin can dissolve in high-boiling-point lipid solvents, which has a strong coating effect on metal powder. In addition, after curing with isocyanate, the network crosslinking density of this resin increases, and the dispersion stability of the silver paste system increases. At the same time, the hydrogen bonding ability of the urea group is stronger than that of the hydroxyl group in adsorbing the substrate. Therefore, while increasing the adhesion, it also improves the storage stability of the silver paste and the smoothness of the printing line.
[0029] It should be noted that PVB resins can be selected from B16H or B20H types, etc.
[0030] In other preferred embodiments, the isocyanate curing agent is hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), etc., including prepolymer curing agents of polyisocyanates.
[0031] In some other preferred embodiments, the high-boiling-point lipid solvent is any one of diethylene glycol butyl ether acetate, diethylene glycol butyl ether, polyoxymethylene dimethyl ether, butyl carbohydrol, dodecyl alcohol ester, hexadecyl alcohol ester, dimethyl adipate, and dibutyl phthalate.
[0032] In some other preferred embodiments, the temperature at which a high-boiling-point lipid solvent is added to the PVB resin and heated and stirred is 85-95°C, for example, preferably 90°C, and the stirring speed is 750-850 r / min, for example, preferably 800 r / min.
[0033] The polymeric adhesion promoters synthesized in this embodiment all contain a PVB backbone and a urea crosslinking network. Their hydroxyl groups can be adjusted by the completeness of the reaction, and the crosslinking density, molecular chain flexibility / rigidity, and compatibility with the slurry system can be adjusted by adjusting the content of PVB resin and curing agent, thereby directly affecting the adhesion of conductive metal slurry.
[0034] In another aspect of this disclosure, a conductive metal paste is provided, comprising: 80-92 parts by weight of silver powder; 1-3 parts by weight of glass powder; 6-12 parts by weight of an organic carrier; and 0.1-3 parts by weight of a polymeric adhesion promoter, wherein the polymeric adhesion promoter is the polymeric adhesion promoter described above, and the specific structural formula is described above and will not be repeated here.
[0035] In some preferred embodiments, the silver powder content may preferably be 80 parts by weight, 83 parts by weight, 86 parts by weight, 90 parts by weight, 92 parts by weight, etc.
[0036] In other preferred embodiments, the content of glass powder may preferably be 1 part by weight, 2 parts by weight, 3 parts by weight, etc.
[0037] In other preferred embodiments, the content of the organic carrier may preferably be 6 parts by mass, 8 parts by mass, 10 parts by mass, 12 parts by mass, etc.
[0038] In other preferred embodiments, the content of the polymeric adhesion promoter may preferably be 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 3 parts by weight, etc.
[0039] In some other preferred embodiments, the viscosity of the conductive metal paste is 80-102 Pa·s, and the adhesion pull is 2.1-2.8 N / mm. 2 The viscosity increase rate over 24 hours is 4.5-6.5%.
[0040] The polymeric adhesion promoter of this embodiment can simultaneously enhance the adhesion between the metal paste and the substrate, as well as the cross-linking density within the paste, thereby improving the overall adhesion of the paste. This results in the conductive silver paste achieving an adhesion of 2.1 N / mm after drying. 2 The above results, for example, 2.5 N / mm 2 The above achieves the effect of improving the overall adhesion of the metal grid lines.
[0041] The preparation method and specific applications of polymeric adhesion promoters will be further explained below with reference to specific embodiments: Example 1 The preparation method of the polymeric adhesion promoter in this example includes the following steps: As shown in Table 1, 19g of PVB resin (B16H) was weighed into a beaker, 80g of diethylene glycol butyl ether acetate solvent was added, the mixture was heated to 90℃ and stirred at 800r / min until completely dissolved, 1g of curing agent HDI was added, and stirring was continued for 2h. After cooling and returning to room temperature, adhesion promoter (DPV1) was obtained.
[0042] The adhesion promoter (DPV1) obtained in Example 1 has the following structural formula: (Equation 1) In Equation 1, z = 1 mol%.
[0043] Further, as shown in Tables 2 and 3, in this Example 1, 1 part by weight of adhesion promoter (DPV1) was mixed with 8 parts by weight of organic carrier, 2 parts by weight of glass powder, and 89 parts by weight of silver powder under vacuum conditions. The mixture was then ground using a three-roll mill to obtain a conductive metal paste. The viscosity of this conductive metal paste was 80 Pa·s (Bolefeld rotational viscometer, No. 14 rotor, 50 r). After drying, the printed grid lines did not peel off, the powder shedding was good, and the tensile strength of the 3M tape was 2.5 N / mm. 2 . Furthermore, as shown in Table 3, the viscosity of the conductive metal slurry in Example 1 was 82.5 Pa·s at 12h, 84.3 Pa·s at 24h, with a viscosity increase rate of 5.3% at 24h, and 84.9 Pa·s at 36h. The viscosity remained basically unchanged. The stable viscosity also reflects that the cross-linking adhesion promoter has the effect of increasing the stability of the slurry. No precipitation occurred in the slurry.
[0044] In this example 1, HDI (hexamethylene diisocyanate) was used as a flexible curing agent. Its chain segments exhibited good flexibility, resulting in tight adhesion to the substrate. The urea-based hydrogen bonding effect was significant, achieving an adhesion strength reaching the benchmark value (2.5 N / mm). 2 It has moderate crosslinking density, the lowest viscosity (80 Pa·s), and excellent printability, making it suitable for fine grid line printing applications.
[0045] Example 2 As shown in Table 1, 19g of PVB resin (B16H) was weighed into a beaker, 80g of diethylene glycol butyl ether acetate solvent was added, the mixture was heated to 90℃ and stirred at 800r / min until completely dissolved, 1g of curing agent TDI was added, and stirring was continued for 2h. After cooling and returning to room temperature, adhesion promoter (DPV2) was obtained.
[0046] (Equation 2) In Equation 2, z = 1 mol%.
[0047] Further, as shown in Tables 2 and 3, in this Example 2, 1 part by weight of adhesion promoter (DPV2) was mixed with 8 parts by weight of organic carrier, 2 parts by weight of glass powder, and 89 parts by weight of silver powder under vacuum conditions. After grinding with a three-roll mill, a conductive metal paste was obtained. The viscosity of the conductive metal paste was 85 Pa·s, the degree of powder shedding from the printed grid lines after drying was medium, and the tensile strength of the 3M tape was 2.1 N / mm. 2 The viscosity increased by 6.2% over 24 hours.
[0048] The TDI (toluene diisocyanate) in this embodiment contains rigid benzene ring segments. After crosslinking, the system hardness increases, and the interfacial adhesion with the substrate (silicon wafer) decreases, resulting in slightly lower adhesion (16% lower than in Example 1). The rigid segments also cause slightly poorer silver powder dispersion, with a powder shedding degree of "medium", but it is still better than the following comparative examples.
[0049] Example 3 As shown in Table 1, 19g of PVB resin (B16H) was weighed into a beaker, 80g of diethylene glycol butyl ether acetate solvent was added, the mixture was heated to 90℃ and stirred at 800r / min until completely dissolved, 1g of curing agent MDI was added, and stirring was continued for 2h. After cooling and returning to room temperature, adhesion promoter (DPV3) was obtained.
[0050] (Equation 3) In Equation 3, z = 1 mol%.
[0051] Further, as shown in Tables 2 and 3, in this Example 3, 1 part by weight of adhesion promoter (DPV3) was mixed with 8 parts by weight of organic carrier, 2 parts by weight of glass powder, and 89 parts by weight of silver powder under vacuum conditions. After grinding with a three-roll mill, a conductive metal paste was obtained. The viscosity of the conductive metal paste was 90 Pa·s. After drying, the printed grid lines did not fall off, the powder shedding was good, and the tensile strength of the 3M tape was 2.4 N / mm. 2 The viscosity increased by 4.5% over 24 hours.
[0052] The MDI (diphenylmethane diisocyanate) chain segment used in Example 3 is in a soft-hard balance (containing benzene ring + methylene), and the system has the best stability after crosslinking (viscosity increase rate of only 4.5%), which is suitable for slurry scenarios that require long-term storage.
[0053] Example 4 As shown in Table 1, 18g of PVB resin (B16H) was weighed into a beaker, 80g of diethylene glycol butyl ether acetate solvent was added, the mixture was heated to 90℃ and stirred at 800r / min until completely dissolved, 2g of curing agent HDI was added, and stirring was continued for 2h. After cooling down and returning to room temperature, adhesion promoter (DPV4) was obtained.
[0054] (Equation 4) In Equation 4, z = 2 mol%.
[0055] Further, as shown in Tables 2 and 3, in this Example 4, 1 part by weight of adhesion promoter (DPV4) was mixed with 8 parts by weight of organic carrier, 2 parts by weight of glass powder, and 89 parts by weight of silver powder under vacuum conditions. After grinding with a three-roll mill, a conductive metal paste was obtained. The viscosity of the conductive metal paste was 89 Pa·s. After drying, the printed grid lines did not fall off, the powder shedding was good, and the tensile strength of the 3M tape was 2.8 N / mm. 2 The viscosity increased by 5.2% over 24 hours.
[0056] In this embodiment, the proportion of curing agent was increased to 2 parts, which increased the crosslinking density and the number of urea groups. The interfacial hydrogen bonding and the internal network cohesive strength were both enhanced, and the adhesion reached its peak. The viscosity of 89 Pa·s was still within the process range, and there was no gelation caused by excessive crosslinking. This is the best cost-effective formulation.
[0057] Example 5 As shown in Table 1, 16g of PVB resin (B16H) was weighed into a beaker, 80g of diethylene glycol butyl ether acetate solvent was added, the mixture was heated to 90℃ and stirred at 800r / min until completely dissolved, 4g of curing agent HDI was added, and stirring was continued for 2h. After cooling and returning to room temperature, adhesion promoter (DPV5) was obtained.
[0058] (Equation 5) In Equation 5, z = 4 mol%.
[0059] Further, as shown in Tables 2 and 3, in this Example 5, 1 part by weight of adhesion promoter (DPV5) was mixed with 8 parts by weight of organic carrier, 2 parts by weight of glass powder, and 89 parts by weight of silver powder under vacuum conditions. After grinding with a three-roll mill, a conductive metal paste was obtained. The viscosity of the conductive metal paste was 102 Pa·s. After drying, the degree of powder shedding from the printed grid lines was medium, and the tensile strength of the 3M tape was 2.6 N / mm. 2 The viscosity increased by 6.5% over 24 hours.
[0060] In this embodiment, the curing agent was increased to 4 parts. Excessive cross-linking led to a significant increase in the system viscosity (102 Pa·s), which may affect printing smoothness. However, the adhesion remained high (2.6 N / mm). 2 However, the viscosity stability decreased, indicating that the proportion of curing agent should not exceed 4 parts.
[0061] Comparative Example 1 As shown in Tables 2 and 3, in Comparative Example 1, 9 parts by weight of organic carrier, 2 parts by weight of glass powder, and 89 parts by weight of silver powder were stirred together under vacuum conditions and then ground using a three-roll mill to obtain a conductive metal paste. The viscosity of this conductive metal paste was 78 Pa·s. After drying, the powder shedding degree of the printed grid lines was poor, and the grid lines showed some detachment. The tensile strength of the 3M tape was 1.2 N / mm. 2 The viscosity increased by 10.1% over 24 hours.
[0062] The comparative example uses a solution without an accelerator, and its adhesion is only 1.2 N / mm. 2 The degree of powder shedding was poor, confirming the necessity of the accelerator.
[0063] Comparative Example 2 As shown in Tables 2 and 3, in Comparative Example 2, 1 part by mass of silane coupling agent (KH550 or KH560) was mixed with 8 parts by mass of organic carrier, 2 parts by mass of glass powder, and 89 parts by mass of silver powder under vacuum conditions. After grinding with a three-roll mill, a conductive metal paste was obtained. The viscosity of the conductive metal paste was 74 Pa·s. After drying, the powder shedding degree of the printed grid lines was poor, and the grid lines showed some detachment. The tensile strength of the 3M tape was 1.8 N / mm. 2 The viscosity increased by 9.8% over 24 hours.
[0064] This comparative example uses a small molecule silane coupling agent with an adhesion strength of 1.8 N / mm. 2 The strength was reduced by 28% compared to the previous example due to insufficient cohesive strength caused by the lack of a cross-linked network.
[0065] Comparative Example 3 As shown in Tables 2 and 3, in Comparative Example 3, 1 part by mass of polyester-type accelerator, 8 parts by mass of organic carrier, 2 parts by mass of glass powder, and 89 parts by mass of silver powder were stirred together under vacuum conditions. After grinding with a three-roll mill, a conductive metal paste was obtained. The viscosity of the conductive metal paste was 82 Pa·s. After drying, the powder shedding degree of the printed grid lines was medium, and the tensile strength of the 3M tape was 2.0 N / mm. 2 The viscosity increased by 8.6% over 24 hours.
[0066] This comparative example uses a polyester-based accelerator with an adhesion strength of 2.0 N / mm. 2 Compared to the previous example, the hydrogen bond of the ester group is weaker than that of the urea group, and the crystallinity leads to poor compatibility.
[0067] It should be noted that the organic carrier, glass powder, and silver powder used in Examples 1-5 and Comparative Examples 1-3 are all conventional. For example, the organic carrier contains a mixture of thickener (ethyl cellulose), dispersant (BYK111), leveling agent (polysiloxane), thixotropic agent (polyamide wax), and solvent (butyl carbitol). The silver powder is a spherical powder with a D50 of 1.2 μm. All examples and comparative examples use the same organic carrier, the same glass powder, and the same silver powder to illustrate the difference in slurry performance caused by the difference in polymeric adhesion promoters.
[0068] Table 1. Synthesis formulations of adhesion promoters in Examples 1-5
[0069] Table 2. Conductive paste formulations for Examples 1-5 and Comparative Examples 1-3
[0070] Table 3 Test results of Examples 1-5 and Comparative Examples 1-3
[0071] In summary, adding the accelerator DPV to the conductive paste improved overall adhesion. Viscosity stability was also significantly improved. Because DPV2 uses TDI for crosslinking, its hardness increases after curing, limiting its adhesion to the substrate, resulting in a slightly smaller improvement in adhesion. Increasing the curing agent dosage increases the crosslinking density and improves adhesion. However, excessive curing agent leads to a rapid increase in viscosity. Therefore, a PVB / curing agent ratio of 19 / 1 to 19 / 4 is recommended.
[0072] In summary, as Figure 2 As shown in (ac), and in conjunction with the above embodiments and comparative examples, it can be seen that when using 3M tape to test tensile strength, the adhesion is significantly improved, the grid lines are intact, without breakage or powdering, the edges are smooth, the grid lines do not fall off, the surface is smooth, and there are no defects visible to the naked eye. The tensile strength reaches 2N / mm. 2 The above applies. When adhesion is insufficient, slight powdering occurs on the grid lines, and some edges are blurred. After tape testing, a small amount of powder residue remains on the grid line edges, or short cracks appear in some areas, but the main structure remains intact. The tensile strength is 1-2 N / mm. 2 At the lowest adhesion, the grid lines severely detached and broke, resulting in large-area powder shedding. After tape testing, the grid lines showed continuous breaks or complete detachment, increasing the exposed area on the substrate surface, with a tensile strength of 0-1 N / mm. 2 between.
[0073] It is understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of this disclosure, and this disclosure is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and substance of this disclosure, and these modifications and improvements are also considered to be within the scope of protection of this disclosure.
Claims
1. A polymeric adhesion promoter, characterized in that, The structural formula of the polymeric adhesion promoter is as follows: ; Wherein, n ranges from 60 to 85 mol%, x ranges from 3 to 10 mol%, y ranges from 10 to 20 mol%, and z ranges from 1 to 10 mol%.
2. The polymeric adhesion promoter according to claim 1, characterized in that, The polymeric adhesion promoter has the structural formula of any one of the following: z = 1 mol% (Equation 1); z = 1 mol% (Equation 2); z = 1 mol% (Equation 3); z = 2 mol% (Equation 4); z = 4mol% (Equation 5).
3. A method for preparing a polymeric adhesion promoter as described in claim 1 or 2, characterized in that, The preparation method includes: A high-boiling-point lipid solvent is added to PVB resin, and the mixture is heated and stirred until completely dissolved to obtain a PVB resin solution. An isocyanate curing agent was added to the PVB resin solution, and after stirring, the solution was cooled to room temperature to obtain a polymeric adhesion promoter.
4. The preparation method according to claim 3, characterized in that, The content ratio of the PVB resin, the isocyanate curing agent, and the high-boiling-point lipid solvent is (16-19):(1-4):
80.
5. The preparation method according to claim 4, characterized in that, The ratio of the PVB resin to the isocyanate curing agent is 19:(1-4).
6. The preparation method according to claim 3, characterized in that, The isocyanate curing agent is any one of hexamethylene diisocyanate, toluene diisocyanate, and diphenylmethane diisocyanate.
7. The preparation method according to claim 3, characterized in that, The high-boiling-point lipid solvent is any one of diethylene glycol butyl ether acetate, diethylene glycol butyl ether, polyoxymethylene dimethyl ether, butyl carbohydrol, decyl alcohol ester, hexadecyl alcohol ester, dimethyl adipate, and dibutyl phthalate.
8. The preparation method according to claim 3, characterized in that, The temperature for adding a high-boiling-point lipid solvent to the PVB resin and heating and stirring is 85-95℃, and the stirring speed is 750-850r / min.
9. A conductive metal paste, characterized in that, The conductive metal paste includes: 80-92 parts by weight of silver powder; 1-3 parts by weight of glass powder; 6-12 parts by weight of organic carrier; 0.1-3 parts by weight of a polymeric adhesion promoter, wherein the polymeric adhesion promoter is the polymeric adhesion promoter described in claim 1 or 2.
10. The conductive metal paste according to claim 9, characterized in that, The conductive metal paste has a viscosity of 80-102 Pa·s and an adhesion tensile strength of 2.1-2.8 N / mm. 2 The viscosity increase rate over 24 hours is 4.5-6.5%.