Cold rolling method for overcoming brittle fracture of non-oriented silicon steel for new energy automobile

By performing normalization, pickling, low-temperature heating, and cold rolling on non-oriented silicon steel in a laboratory environment, the brittle fracture problem in the cold rolling process of non-oriented silicon steel was solved, the stability and yield of the cold rolling process were improved, and the requirements for use in new energy vehicles were met.

CN121852666APending Publication Date: 2026-04-14INNER MONGOLIA UNIV OF SCI & TECH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202512021786.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-30
Publication Date
2026-04-14

AI Technical Summary

Technical Problem

In a laboratory environment, edge cracks and brittle fractures are prone to occur during the cold rolling process of non-oriented silicon steel for new energy vehicles, affecting production efficiency and yield. Moreover, existing research mainly focuses on the industrial production field and lacks solutions for the laboratory.

Method used

The process involves normalizing, pickling, low-temperature heating, and cold rolling. By testing the ductile-brittle transition temperature of the non-oriented silicon steel sheet, the sheet is heated in the range of 200-500℃ to avoid the ductile-brittle transition temperature. Cold rolling is then performed using a straight-pull four-roll reversible cold rolling mill, followed by continuous annealing to control stress distribution and plastic deformation.

Benefits of technology

It effectively avoids brittle fracture, improves the stability and yield of the cold rolling process, ensures the quality of the sheet shape and magnetic properties, reduces equipment costs and floor space, simplifies the structure of cold rolling equipment, and meets the requirements of non-oriented silicon steel for new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121852666A_ABST
    Figure CN121852666A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal material processing, and discloses a cold rolling method for overcoming brittle fracture of non-oriented silicon steel for a new energy automobile, which comprises the following steps: S1, normalizing treatment: heating at 920-1000 DEG C for 2.5-4 minutes; s2, pickling treatment: pickling in an acidic aqueous solution, then soaking in a clean water tank, neutralizing with an alkaline aqueous solution, blow-drying and coating oil to prevent rusting; s3, heating treatment is conducted, specifically, the workpiece is placed in a box-type resistance furnace, and heat preservation is conducted for 20-120 min under the condition of 200-500 DEG C; s4, cold rolling is conducted, specifically, hot rolling is rapidly conducted on a cold-rolling mill; and S5, continuous annealing is conducted, specifically, continuous annealing is conducted at the strip steel speed of 85 m / min to 95 m / min, and the annealing soaking temperature is 920 DEG C to 1000 DEG C. The technical problem that when silicon steel cold rolling is carried out in a laboratory environment, the edge of a cold-rolled plate is cracked or brittle fracture occurs is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal material processing technology, specifically to a cold rolling method for overcoming brittle fracture of non-oriented silicon steel used in new energy vehicles. Background Technology

[0002] In the field of metal processing, silicon steel, as an important electrical steel material, is widely used in industries such as power and electronics. The cold rolling process is a crucial step in the production of silicon steel. Laboratory conditions differ from industrial production environments, and traditional silicon steel cold rolling processes are difficult to fully adapt to a laboratory setting. Differences in equipment scale and process control precision lead to more complex stress distribution and deformation during cold rolling. The silicon content in the silicon steel also significantly affects its cold-rolling performance; higher silicon content increases the hardness and brittleness of the steel, thereby increasing the risk of edge cracking and brittle fracture. Therefore, when cold rolling silicon steel in a laboratory environment, edge cracking and even brittle fracture of the cold-rolled sheet are frequently encountered. This problem not only affects the production efficiency of silicon steel but also reduces the yield rate and increases production costs.

[0003] Currently, research on edge cracking and brittle fracture during the cold rolling of silicon steel mainly focuses on industrial production, with relatively little research conducted in laboratory settings. However, laboratories serve as research platforms for new technologies and processes, making solutions to edge cracking and brittle fracture during silicon steel cold rolling crucial. They not only improve the efficiency and quality of laboratory research but also provide valuable references for industrial production. Therefore, developing a method suitable for laboratory environments to prevent brittle fracture during silicon steel cold rolling is urgently needed. Summary of the Invention

[0004] The present invention aims to provide a cold rolling method to overcome the brittle fracture of non-oriented silicon steel used in new energy vehicles, and solves the technical problem of edge cracking or brittle fracture of cold-rolled plates when silicon steel is cold rolled in a laboratory environment.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] A cold rolling method for overcoming brittle fracture of non-oriented silicon steel used in new energy vehicles includes the following steps:

[0007] S1. Normalizing treatment: The non-oriented silicon steel sheet is normalized at a heating temperature of 920-1000℃ and a holding time of 2.5-4min.

[0008] S2. Pickling treatment: Pickle the non-oriented silicon steel sheet after step S1 in an acidic aqueous solution at a temperature of 50-60℃; then soak it in a clean water tank, brush off the surface oxide scale and rust, neutralize it with an alkaline aqueous solution, blow it dry and apply oil to prevent rust.

[0009] S3. Heat treatment: Place the silicon steel treated with S2 in a box-type resistance furnace and hold it at 200-500℃ for 20-120 minutes.

[0010] S4. Cold rolling: The heat-treated silicon steel is quickly rolled on a cold rolling mill at a temperature higher than its ductile-brittle transition temperature, which can prevent it from brittle fracture.

[0011] S5. Continuous annealing: Continuous annealing is carried out at a strip speed of 85m / min to 95m / min, and the annealing temperature is 920-1000℃.

[0012] Furthermore, in S2, the acidic aqueous solution is a 10% HCl aqueous solution, and the acid washing time is 25~35 min; the alkaline aqueous solution is a 6% Na2CO3 alkaline aqueous solution.

[0013] Furthermore, in S3, the box-type resistance furnace is first heated to 200-500℃, and then the silicon steel plate is placed inside the box-type resistance furnace.

[0014] Furthermore, in S4, the total reduction of silicon steel undergoing multi-pass cold rolling is 80-90%.

[0015] Furthermore, in S4, the cold rolling mill is a straight-pull four-high reversible cold rolling mill, with the following technical specifications: finished product thickness: hmin = 0.2 mm, width: bmax = 350 mm, length: Imax = 3000 mm; support roll dimensions: 550×450mm, work roll dimensions: 200×470mm, 150×470mm 110×470mm.

[0016] Furthermore, the chemical composition of silicon steel by mass percentage is as follows: silicon content is 1.5%~3.0%, aluminum content is about 0.8%~1.5%, carbon content is ≤0.03%, manganese content is about 0.3%~0.8%, the sum of phosphorus, sulfur and nitrogen content is ≤0.03%, and the remainder is Fe and unavoidable impurities.

[0017] Furthermore, the grain size of the finished plate after continuous annealing following cold rolling is 90-120μm.

[0018] The beneficial effects of the technical solution are:

[0019] This invention addresses the brittle fracture that occurs during the cold rolling of 30AV1500 high-efficiency non-oriented silicon steel for new energy vehicles by improving related processes. Through in-depth analysis of the characteristics of silicon steel cold rolling under laboratory conditions, combined with the chemical composition and performance characteristics of 30AV1500 silicon steel, a targeted process control scheme is formulated. Specifically, by testing the ductile-brittle transition temperature of the 30AV1500 non-oriented silicon steel sheet, the sheet is heated to a temperature range of 200-500℃ before cold rolling. This effectively avoids the ductile-brittle transition temperature, generating sufficient plastic deformation during rolling and improving the efficiency of the entire rolling process. Simultaneously, it avoids high stress concentration, eliminating work hardening and preventing brittle fracture. Furthermore, this low-temperature, short-time heating method avoids problems such as surface oxidation and performance changes in the strip caused by heating, while ensuring good sheet shape quality after cold rolling, effectively controlling the flatness of the sheet, and achieving ideal magnetic properties, thus meeting the requirements of new energy vehicles for high-efficiency non-oriented silicon steel.

[0020] Furthermore, the method of this invention avoids heating the strip steel through heat conduction from the heating rollers and eliminates the need for heating the rolled plate with hot water, steam, or heated rolling emulsion. This reduces the requirements for cold rolling equipment and avoids strip steel quality fluctuations caused by heating roller malfunctions or inaccurate temperature control, effectively improving the stability of the cold rolling process. Moreover, the elimination of heating rollers and related auxiliary devices simplifies the structure of the cold rolling equipment, reduces manufacturing and maintenance costs, and minimizes the equipment's footprint, providing a more rational layout solution for limited laboratory space.

[0021] Therefore, this invention improves the stability and yield of cold rolling of 30AV1500 non-oriented silicon steel. It can maintain good ductility during cold rolling, promote the formation of favorable texture during cold rolling, and make it easier to obtain a uniform recrystallized structure after annealing. This not only reduces the risk of brittle fracture, but also improves the magnetic properties and surface quality of the finished product. Attached Figure Description

[0022] Figure 1 This is a macroscopic photograph of a 30AV1500 non-oriented silicon steel sheet after hot-rolling in Embodiment 1 of the present invention.

[0023] Figure 2 This is a micrograph of the finished 30AV1500 non-oriented silicon steel plate in Embodiment 1 of the present invention.

[0024] Figure 3 This is a macroscopic photograph of a 30AV1500 non-oriented silicon steel sheet after hot-rolling in Embodiment 2 of the present invention.

[0025] Figure 4This is a micrograph of the unheated finished plate of 30AV1500 non-oriented silicon steel in Embodiment 2 of the present invention.

[0026] Figure 5 This is a macroscopic photograph of the edge cracking of a 30AV1500 non-oriented silicon steel sheet after cold rolling, as shown in Comparative Example 1. Detailed Implementation

[0027] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments:

[0028] Example 1

[0029] The silicon steel is a hot-rolled non-oriented silicon steel sheet with the grade 30AV1500. Its chemical composition by mass percentage is as follows: silicon content is 2.8%, aluminum content is about 0.95%, carbon content is 0.002%, manganese content is about 0.62%, phosphorus, sulfur and nitrogen content combined is ≤0.16%, and the remainder is Fe and unavoidable impurities.

[0030] The specific cold rolling method to overcome the brittle fracture of non-oriented silicon steel used in new energy vehicles is as follows:

[0031] S1. Normalizing treatment: The non-oriented silicon steel sheet is normalized at a heating temperature of 980℃ and a holding time of 3min.

[0032] S2. Pickling treatment: Pickle the non-oriented silicon steel sheet after S1 treatment in a 10% HCl aqueous solution at a temperature of 50-60℃ for 30 minutes; then soak it in a clean water tank, brush off the surface oxide scale and rust, then neutralize it with an alkaline aqueous solution of about 6% Na2CO3, and finally blow it dry and apply oil to prevent rust.

[0033] S3. Heat treatment: First, heat the box-type resistance furnace to 300℃, and then place the silicon steel pickled in step S2 into the box-type resistance furnace for heat treatment at 300℃ for 60 minutes.

[0034] S4. Cold Rolling: The heat-treated silicon steel is rapidly rolled on a cold rolling mill at a temperature higher than its ductile-brittle transition temperature to prevent brittle fracture. The cold rolling mill is a direct-draw four-roll reversible cold rolling mill. Technical specifications include: finished product thickness: hmin = 0.2mm, width: bmax = 350mm, length: Imax = 3000mm; support roll dimensions: 550×450mm, work roll dimensions: 200×470mm, 150×470mm 110×470mm.

[0035] No brittle fracture occurred during the cold rolling process. The total cold rolling reduction was 88%. The sheet shape quality after cold rolling was good, with no obvious edge waviness, center waviness, or other defects. Figure 1 As shown.

[0036] S5. Continuous Annealing: Continuous annealing is performed at a strip speed of 90 m / min, with a soaking temperature of 940℃. The flatness of the strip is controlled within a reasonable range. After annealing, the grain size of the finished strip reaches 98.37 μm, exhibiting good grain size uniformity. Figure 2 As shown, it meets the requirements for the use of non-oriented silicon steel in new energy vehicles.

[0037] Example 2

[0038] The silicon steel is a hot-rolled non-oriented silicon steel sheet with the grade 30AV1500. Its chemical composition by mass percentage is as follows: silicon content is 2.8%, aluminum content is about 0.95%, carbon content is 0.002%, manganese content is about 0.62%, phosphorus, sulfur and nitrogen content combined is ≤0.16%, and the remainder is Fe and unavoidable impurities.

[0039] The specific cold rolling method to overcome the brittle fracture of non-oriented silicon steel used in new energy vehicles is as follows:

[0040] S1. Normalizing treatment: The non-oriented silicon steel sheet is normalized at a heating temperature of 980℃ and a holding time of 3min.

[0041] S2. Pickling treatment: Pickle the non-oriented silicon steel sheet after S1 treatment in a 10% HCl aqueous solution at a temperature of 50-60℃ for 30 minutes; then soak it in a clean water tank, brush off the surface oxide scale and rust, then neutralize it with an alkaline aqueous solution of about 6% Na2CO3, and finally blow it dry and apply oil to prevent rust.

[0042] S3. Heat treatment: First, heat the box-type resistance furnace to 270℃, and then place the silicon steel pickled in step S2 into the box-type resistance furnace for heat treatment at 270℃ for 30 minutes.

[0043] S4. Cold Rolling: The heat-treated silicon steel is rapidly rolled on a cold rolling mill at a temperature higher than its ductile-brittle transition temperature to prevent brittle fracture. The cold rolling mill is a direct-draw four-roll reversible cold rolling mill. Technical specifications include: finished product thickness: hmin = 0.2mm, width: bmax = 350mm, length: Imax = 3000mm; support roll dimensions: 550×450mm, work roll dimensions: 200×470mm, 150×470mm 110×470mm.

[0044] No brittle fracture occurred during the cold rolling process. The total cold rolling reduction was 86%, and the sheet shape quality after cold rolling was good. Figure 3 As shown.

[0045] S5. Continuous Annealing: Continuous annealing is performed at a strip speed of 90 m / min, with a soaking temperature of 940℃. The flatness of the strip is controlled within a reasonable range, and the grain size of the finished strip after annealing reaches 96.58 μm. Figure 4 As shown, it meets the requirements for the use of non-oriented silicon steel in new energy vehicles.

[0046] Comparative Example 1

[0047] The silicon steel used was a hot-rolled non-oriented silicon steel sheet of grade 30AV1500. Its chemical composition by mass percentage was: silicon content 2.8%, aluminum content approximately 0.95%, carbon content 0.002%, manganese content approximately 0.62%, and the sum of phosphorus, sulfur, and nitrogen content ≤0.16%, with the remainder being Fe and unavoidable impurities. After normalizing and pickling as in Example 1, no heating was performed; instead, it was directly cold-rolled on a straight-pull four-roll reversible cold rolling mill. Significant edge cracking occurred during the cold rolling process. Figure 5 As shown in the image. At this point, the steel strip undergoes brittle fracture, making subsequent continuous annealing impossible.

[0048] In summary, this invention addresses the brittle fracture that occurs during the cold rolling of 30AV1500 high-efficiency non-oriented silicon steel for new energy vehicles by improving related processes. Through in-depth analysis of the characteristics of silicon steel cold rolling under laboratory conditions, combined with the chemical composition and performance characteristics of 30AV1500 silicon steel, a targeted process control scheme was developed. Specifically, by testing the ductile-brittle transition temperature of the 30AV1500 non-oriented silicon steel sheet, the sheet is heated to a temperature range of 200-500℃ before cold rolling. This effectively avoids the ductile-brittle transition temperature, generating sufficient plastic deformation during rolling and improving the efficiency of the entire rolling process. Simultaneously, it avoids high stress concentration, eliminating work hardening and preventing brittle fracture. Furthermore, this low-temperature, short-time heating method avoids problems such as surface oxidation and performance changes in the strip caused by heating, while ensuring good sheet shape quality after cold rolling, effectively controlling the flatness of the sheet, and achieving ideal magnetic properties, thus meeting the requirements of new energy vehicles for high-efficiency non-oriented silicon steel.

[0049] Furthermore, the method of this invention avoids heating the strip steel through heat conduction from the heating rollers and eliminates the need for heating the rolled plate with hot water, steam, or heated rolling emulsion. This reduces the requirements for cold rolling equipment and avoids strip steel quality fluctuations caused by heating roller malfunctions or inaccurate temperature control, effectively improving the stability of the cold rolling process. Moreover, the elimination of heating rollers and related auxiliary devices simplifies the structure of the cold rolling equipment, reduces manufacturing and maintenance costs, and minimizes the equipment's footprint, providing a more rational layout solution for limited laboratory space.

[0050] Therefore, this invention improves the stability and yield of cold rolling of 30AV1500 non-oriented silicon steel. It can maintain good ductility during cold rolling, promote the formation of favorable texture during cold rolling, and make it easier to obtain a uniform recrystallized structure after annealing. This not only reduces the risk of brittle fracture, but also improves the magnetic properties and surface quality of the finished product.

[0051] The above descriptions are merely embodiments of the present invention, and common knowledge regarding specific technical solutions or characteristics is not elaborated upon here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the technical solutions of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.

Claims

1. A cold rolling method for overcoming brittle fracture of non-oriented silicon steel used in new energy vehicles, characterized in that, Includes the following steps: S1. Normalizing treatment: The non-oriented silicon steel sheet is normalized at a heating temperature of 920-1000℃ and a holding time of 2.5-4min. S2. Pickling treatment: Pickle the non-oriented silicon steel sheet after step S1 in an acidic aqueous solution at a temperature of 50-60℃; then soak it in a clean water tank, brush off the surface oxide scale and rust, neutralize it with an alkaline aqueous solution, blow it dry and apply oil to prevent rust. S3. Heat treatment: Place the silicon steel treated with S2 in a box-type resistance furnace and keep it at 200-500℃ for 20-120 minutes. S4. Cold rolling: The heat-treated silicon steel is quickly rolled on a cold rolling mill at a temperature higher than its ductile-brittle transition temperature, which can prevent it from brittle fracture. S5. Continuous annealing: Continuous annealing is carried out at a strip speed of 85m / min to 95m / min, and the annealing temperature is 920-1000℃.

2. The cold rolling method for overcoming brittle fracture of non-oriented silicon steel for new energy vehicles according to claim 1, characterized in that: In S2, the acidic aqueous solution is a 10% HCl aqueous solution, and the acid washing time is 25~35 min; the alkaline aqueous solution is a 6% Na2CO3 alkaline aqueous solution.

3. The cold rolling method for overcoming brittle fracture of non-oriented silicon steel for new energy vehicles according to claim 1, characterized in that: In S3, the box-type resistance furnace is first heated to 200-500℃, and then the silicon steel plate is placed inside the box-type resistance furnace.

4. The cold rolling method for overcoming brittle fracture of non-oriented silicon steel for new energy vehicles according to claim 1, characterized in that: In S4, the total reduction of silicon steel undergoing multi-pass cold rolling is 80-90%.

5. The cold rolling method for overcoming brittle fracture of non-oriented silicon steel for new energy vehicles according to claim 1, characterized in that: In S4, the cold rolling mill is a straight-pull four-high reversible cold rolling mill. The technical specifications include: finished product thickness: hmin = 0.2 mm, width: bmax = 350 mm, length: Imax = 3000 mm; support roll dimensions: 550×450mm, work roll dimensions: 200×470mm, 150×470mm, 110×470mm.

6. The cold rolling method for overcoming brittle fracture of non-oriented silicon steel for new energy vehicles according to claim 1, characterized in that: The chemical composition of silicon steel by mass percentage is as follows: silicon content is 1.5%~3.0%, aluminum content is about 0.8%~1.5%, carbon content is ≤0.03%, manganese content is about 0.3%~0.8%, the sum of phosphorus, sulfur and nitrogen content is ≤0.03%, and the remainder is Fe and unavoidable impurities.