Wear-resistant medium manganese steel with high product of strength and elongation and preparation method thereof
By optimizing the chemical composition and heat treatment process of medium manganese steel, a high-strength, high-ductility, wear-resistant medium manganese steel was prepared, solving the problem of low initial yield strength and achieving high initial hardness and excellent work hardening ability, making it suitable for manufacturing wear-resistant components with complex shapes.
Patent Information
- Application Number
- CN202511919317.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-18
- Publication Date
- 2026-04-17
AI Technical Summary
The existing medium manganese steel has a low initial yield strength, which makes it difficult to meet the application requirements of high wear-resistant parts. It is also difficult to balance high plasticity and high wear resistance, making it impossible to maintain stable service in high wear environments for a long time.
By optimizing the chemical composition of medium manganese steel, including the ratio of C, Mn, Si, Cr, Mo, Ni, Ti, Nb, and V, and combining it with specific heat treatment processes, high-strength, high-ductility, and wear-resistant medium manganese steel with fine-grained austenitic and martensitic structures is prepared. The process includes homogenization treatment, rolling, annealing, warm rolling, and tempering.
It significantly improves the initial hardness and work hardening ability of medium manganese steel, making it suitable for complex working conditions. It also has high elongation, making it suitable for manufacturing wear-resistant structural parts with complex shapes, thus expanding the application range of high-performance wear-resistant steel.
Smart Images

Figure CN121874636A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of iron and steel metallurgy technology, and in particular to a high-strength, high-ductility, wear-resistant medium-manganese steel and its preparation method. Background Technology
[0002] Medium-manganese steel is widely used as a wear-resistant material in mining machinery, engineering equipment, and other fields. However, traditional medium-manganese steel (carbon content 0.15%–0.25%) is limited by its low initial hardness, requiring significant work hardening to achieve ideal wear resistance in the early stages of service, leading to a risk of rapid material loss in the initial wear phase. Similarly, while high-manganese steel possesses excellent work hardening capabilities, its insufficient initial hardness also limits its adaptability to various working conditions. In contrast, traditional martensitic wear-resistant steels (such as NM400) suffer from insufficient strength-ductility balance, making it difficult to simultaneously achieve high strength and wear resistance with good formability, thus failing to meet the wear resistance requirements of complex steel structures. In existing technologies, traditional steel materials all suffer from insufficient balance between hardness and hardening ability, making it difficult to simultaneously meet the requirements of high initial wear resistance and sustained stable wear resistance.
[0003] CN112410681A discloses a high-strength, high-ductility medium-manganese steel and its preparation method. The method uses a cyclic warm rolling + critical annealing process to prepare an ultra-fine-grained medium-manganese steel with coarse-grained austenite and fine-grained austenite structures, which significantly improves the plasticity of the material. However, its yield strength is only 484-736 MPa, which can easily lead to excessive weight loss in the early stage of wear. It is only suitable for the field of automotive steel.
[0004] CN112159931A discloses a 1000MPa grade medium-manganese TRIP steel with continuous yield strength. By optimizing the C and Mn element ratio, the intermediate annealing process required for high-manganese medium-manganese steel is eliminated. The hot-rolled coil can be directly cold-rolled after uncoiling. The process reduces manufacturing costs and improves production efficiency. However, its yield strength level is still mainly concentrated in 700-750MPa, which cannot meet the requirements of wear environment.
[0005] CN110592491A describes a high-wear-resistant martensitic / austenitic duplex wear-resistant steel plate and its manufacturing method. By using TiC particles to block the wear track mechanism, the wear resistance is improved by more than 50%, and the welding preheating temperature is reduced by 80°C. It is suitable for high-wear scenarios such as mining and engineering machinery. However, its elongation is only 10.3% to 17.5%, which cannot meet the forming requirements of complex steel structures.
[0006] In summary, most medium-manganese steel processes achieve high strength-ductility product mechanical properties by introducing a large amount of metastable residual austenite and regulating the phase transformation-induced plasticity and twin-induced plasticity effects. However, the initial yield strength is insufficient and cannot meet the application requirements of high wear-resistant parts. Martensitic-based materials have insufficient plasticity and are not suitable for applications of structurally complex parts. Summary of the Invention
[0007] Based on the above analysis, the present invention aims to provide a high-strength, high-ductility, wear-resistant medium-manganese steel and its preparation method, in order to solve at least one of the following problems in the prior art: low initial yield strength of manganese steel makes it difficult to meet the application requirements of high wear-resistant parts; difficulty in achieving both high ductility and high wear resistance; and difficulty in long-term stable service under high wear environments.
[0008] In a first aspect, the present invention provides a high-strength, high-performance, wear-resistant medium-manganese steel, wherein the chemical composition of the medium-manganese steel, by mass percentage, is: C: 0.35% to 0.45%, Si: 0.75% to 1.25%, Mn: 8.5% to 11.5%, with the balance being Fe and unavoidable impurities.
[0009] Furthermore, the chemical composition of the medium manganese steel also includes one or more of the following components: Cr: 0%–1.5%, Ni: 0%–3%, Mo: 0%–0.5%, Ti: 0%–0.5%, Nb: 0%–0.5%, V: 0%–1.0%.
[0010] Secondly, the present invention provides a method for preparing the high-strength, high-performance, wear-resistant medium-manganese steel, comprising the following steps:
[0011] S1: According to the chemical composition of the medium manganese steel, the raw materials are batched, smelted, and cast to obtain a slab;
[0012] S2: The slab is subjected to homogenization treatment and rolling in sequence to obtain a hot-rolled plate;
[0013] S3: Anneal the hot-rolled plate and then cool it to room temperature to obtain a steel plate;
[0014] S4: The steel plate is subjected to warm rolling and then cooled to room temperature;
[0015] S5: The rolled steel plate is tempered and then cooled to room temperature to obtain the medium manganese steel.
[0016] Furthermore, in S1, the casting is carried out by die casting or continuous casting. When continuous casting is used, the stretching speed is ≤1.5m / min.
[0017] Furthermore, in S2, the homogenization treatment temperature is 1180–1250°C, and the homogenization time is 1–5 h.
[0018] Furthermore, in S2, the initial rolling temperature is 1080–1150°C, the final rolling temperature is 860–930°C, and the rolling reduction rate is ≥85%.
[0019] Furthermore, in S3, the annealing temperature is 550–630°C, and the holding time is 0.5–8 hours.
[0020] Furthermore, in S4, the warm rolling is carried out at 550-630°C for 0.5-8 hours, and the final rolling temperature is 530-610°C.
[0021] Furthermore, the warm rolling reduction rate is ≥60%.
[0022] Furthermore, in S5, the tempering temperature is 550–630°C, and the tempering time is 0.5–8 hours.
[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0024] 1. This invention overcomes the limitation of insufficient initial hardness of traditional medium manganese steel (C: 0.15%~0.25%) by optimizing the alloy design of medium manganese wear-resistant steel, enabling it to have high surface hardness before the work hardening stage. This results in excellent wear resistance in the early stages of structural components' service life, effectively avoiding the high wear rate problem caused by insufficient hardness in the early stages of wear of traditional high / medium manganese steel.
[0025] 2. This invention optimizes the ratio and morphology of martensite and retained austenite in the steel plate, resulting in a steel plate that combines high yield strength with excellent work hardening capability. By appropriately increasing the carbon content and precisely controlling the Mn element ratio and heat treatment process, it maintains high initial hardness while still possessing excellent work hardening capability, enabling it to adapt to complex working conditions such as impact and extrusion. This allows the material to maintain stable wear resistance during long-term wear, overcoming the shortcomings of insufficient hardening capability in traditional martensitic wear-resistant steels.
[0026] 3. This invention improves the balance between strength and plasticity, making it suitable for processing wear-resistant components with complex shapes. Through reasonable composition and heat treatment process design, it maintains high strength while still having a high elongation rate, making it suitable for manufacturing complex-shaped wear-resistant structural parts in mining machinery and engineering equipment, greatly expanding the application range of high-performance wear-resistant steel.
[0027] 4. The process of this invention is highly feasible and suitable for industrial production. Warm rolling and heat preservation can be achieved using conventional continuous annealing furnaces or bell-type furnaces; the warm rolling temperature and reduction are moderate, and the rolling load is acceptable to existing hot continuous rolling or narrow strip rolling lines, without the need for additional equipment, and it has the potential for large-scale promotion and application.
[0028] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0029] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0030] Figure 1 This is an Omniform microstructure photograph of the medium-manganese steel prepared in Example 1 of the present invention. Detailed Implementation
[0031] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0032] A specific embodiment of the present invention discloses a high-strength, high-performance, wear-resistant medium-manganese steel, wherein the chemical composition of the medium-manganese steel, by mass percentage, is: C: 0.35% to 0.45%, Si: 0.75% to 1.25%, Mn: 8.5% to 11.5%, with the balance being Fe and unavoidable impurities.
[0033] Specifically, the chemical composition of the medium manganese steel also includes one or more of the following components: Cr: 0%–1.5%, Ni: 0%–3%, Mo: 0%–0.5%, Ti: 0%–0.5%, Nb: 0%–0.5%, V: 0%–1.0%.
[0034] The reasons for limiting the composition of manganese steel in the high-strength, high-performance, wear-resistant steel of this invention will be explained. Hereinafter, only the percentage of mass in the composition will be expressed as %.
[0035] C is the most important strengthening element in steel, playing a decisive role in hardness, strength, and wear resistance. This invention increases the C content to 0.35%–0.45% (e.g., 0.35%, 0.36%, 0.37%, 0.38%, 0.39%, 0.40%, 0.41%, 0.42%, 0.43%, 0.44%, 0.45%). Compared to traditional medium manganese steel (C: 0.15%–0.25%), this significantly improves the initial hardness of the martensitic / bainitic matrix, reducing wear in the early stages of service. Furthermore, during the austenitic reversal transformation, C promotes austenite carbonization, enhancing its stability and facilitating the induction of the TRIP effect during deformation, thereby enhancing work hardening capacity and maintaining high wear resistance throughout the wear process.
[0036] Mn: As a core alloying element, this invention significantly increases the Mn content to 8.5%–11.5% (e.g., 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%). Its effects are: strongly expanding the austenite phase region, reducing the critical cooling rate for phase transformation, and ensuring a fine-grained austenite / martensite multiphase microstructure after hot rolling or heat treatment; Mn and C synergistically stabilize austenite, allowing the reverse-transformed austenite to be retained even at room temperature and during deformation, thereby achieving high work hardening capacity through the TRIP effect; solid solution strengthens the matrix and improves hardenability, but excessively high content can easily lead to deterioration of steel toughness. This invention optimizes the Mn to C ratio, balancing high yield strength and plasticity reserve.
[0037] Si (Si) is a strong substitutional solid solution strengthening element that also significantly inhibits cementite precipitation. This invention sets the Si content to 0.75%–1.25% (e.g., 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1.0%, 1.05%, 1.1%, 1.15%, 1.2%, 1.25%), which has three main effects: inhibiting carbide precipitation during two-phase annealing and promoting C enrichment in austenite, thereby improving austenite stability and enhancing its work hardening capacity through the TRIP effect during subsequent deformation; strengthening the matrix through solid solution and synergistically increasing initial hardness with C; and improving the fluidity of molten steel. However, a content exceeding 1.25% can easily lead to increased inclusions and decreased plasticity. This invention balances the strengthening effect of Si with process adaptability, ensuring that wear-resistant steel possesses both high hardness and good formability (elongation ≥15%).
[0038] Cr: Primarily enhances matrix strength through solid solution strengthening and significantly improves the hardenability of steel. It can also combine with carbon to form fine, dispersed carbides, increasing material hardness by 10%–20% through hard precipitates, thereby significantly improving wear resistance. However, excessively high Cr content increases the austenite content in the final microstructure, leading to excessively low initial hardness and compromising initial wear resistance. Therefore, the Cr content in this invention is controlled within the range of 0%–1.5% (e.g., 0%, 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%).
[0039] Mo, as a strong carbide-forming element, can combine with C in steel to form fine nanoscale carbides, which not only improves the hardness and wear resistance of the material, but also has the effect of pinning grain boundaries, helping to inhibit grain growth. It can also improve the secondary hardening effect of steel, enhance its resistance to tempering softening, and enable it to maintain high hardness and strength during subsequent heat treatment or use. However, the Mo content should not be too high, as this will not only increase costs but may also promote the formation of brittle phases, thereby impairing the toughness of the steel. Therefore, the Mo content in this invention is controlled within the range of 0% to 0.5% (e.g., 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%).
[0040] Ni, as a strong austenite stabilizing element, can significantly increase the content and stability of reverse-transformed austenite, achieving high strength and high plasticity through the TRIP effect; it can also lower the ductile-brittle transition temperature of steel and improve low-temperature impact toughness. However, excessive Ni can lead to excessively low initial hardness and increased costs. Based on this, the Ni content in this invention is controlled within the range of 0% to 3.0% (e.g., 0%, 0.5%, 1.0%, 1.5%, 2%, 2.5%, 3%).
[0041] V: By precipitating nano-sized VC carbides, dislocations and grain boundaries are pinned, resulting in a significant precipitation strengthening effect. It also inhibits abnormal growth of austenite grains during warm rolling or critical annealing, ensuring microstructure uniformity. Simultaneously, VC can induce a secondary hardening effect, maintaining stable high hardness even at higher service temperatures. However, excessively high V content may lead to carbide coarsening and decreased processing plasticity. Therefore, the V content in this invention is controlled within the range of 0% to 1.0% (e.g., 0%, 0.2%, 0.4%, 0.6%, 0.8%, 1%).
[0042] Nb can form nanoscale NbC / Nb(CN) precipitates, effectively pinning grain boundaries and inhibiting austenite grain growth, thereby improving strength and toughness through grain refinement. It can also lower the ductile-brittle transition temperature and improve low-temperature toughness. Furthermore, the Nb-containing nanoprecipitates produce a significant precipitation strengthening effect, significantly increasing yield strength. Simultaneously, the addition of Nb significantly improves the high-temperature stability of the material, enabling the wear-resistant steel to maintain excellent wear resistance under high-temperature service conditions. However, excessive Nb can lead to carbide coarsening and affect weldability. Therefore, the V content in this invention is controlled within the range of 0% to 0.5% (e.g., 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%).
[0043] Ti can form ultrafine Ti(C,N) precipitates, significantly refining austenite grains and improving the balance between strength and toughness. Secondly, Ti can effectively fix free nitrogen in molten steel, reducing the tendency for aging embrittlement and improving weldability. Simultaneously, Ti can react with residual sulfur in steel to form TiS compounds, improving the transverse impact toughness of the steel. However, a Ti content exceeding 0.5% leads to the formation of coarse TiN, reducing the mechanical properties of the material. Therefore, the Ti content in this invention is controlled within the range of 0% to 0.5% (e.g., 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%).
[0044] This invention significantly improves the initial hardness of steel plates and reduces material loss in the early stages of wear. By optimizing the alloy design of medium-manganese wear-resistant steel, it overcomes the limitation of insufficient initial hardness in traditional medium-manganese steel (C: 0.15%~0.25%), enabling it to possess high surface hardness even before work hardening. This results in excellent wear resistance in the early stages of structural component service, effectively avoiding the high wear rate problem caused by insufficient hardness in the early stages of wear of traditional high / medium-manganese steel.
[0045] Another specific embodiment of the present invention discloses a method for preparing high-strength, high-performance, wear-resistant medium-manganese steel, comprising the following steps:
[0046] S1: According to the chemical composition of the medium manganese steel, the raw materials are batched, smelted, and cast to obtain a slab;
[0047] S2: The slab is subjected to homogenization treatment and rolling in sequence to obtain a hot-rolled plate;
[0048] S3: Anneal the hot-rolled plate and then cool it to room temperature to obtain a steel plate;
[0049] S4: The steel plate is subjected to warm rolling and then cooled to room temperature;
[0050] S5: The rolled steel plate is tempered and then cooled to room temperature to obtain the medium manganese steel.
[0051] Specifically, in S1, the casting is carried out by ingot casting or continuous casting. When continuous casting is used, the stretching speed is ≤1.5m / min to avoid defects such as cracks in the casting billet.
[0052] Specifically, in S2, the homogenization temperature is 1180–1250℃, for example, 1180℃, 1190℃, 1200℃, 1210℃, 1220℃, 1230℃, 1240℃, 1250℃, and the homogenization time is 1–5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h.
[0053] To reduce elemental segregation in steel and to consider austenite grain coarsening, the homogenization temperature is controlled at 1180–1250℃. Meanwhile, the high Si content in the steel leads to poor thermal conductivity, which can easily cause cracking and incomplete burning. Therefore, the billet should be in the furnace for 1–5 hours before continuous rolling.
[0054] Specifically, in S2, the initial rolling temperature is 1080–1150℃, for example, 1080℃, 1090℃, 1100℃, 1110℃, 1120℃, 1130℃, 1140℃, or 1150℃; the final rolling temperature is 860–930℃, for example, 860℃, 870℃, 880℃, 890℃, 900℃, 910℃, 920℃, or 930℃; and the rolling reduction rate is ≥85%, for example, 85%, 87%, 89%, 91%, 93%, or 95%.
[0055] If the final rolling temperature is too high, the hot-rolled austenite grains will be coarser; if the final rolling temperature is too low, the mill load will increase significantly.
[0056] Specifically, in S3, the annealing temperature is 550-630℃, for example, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, 610℃, 620℃, 623℃, and the holding time is 0.5-8h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h.
[0057] It should be noted that the annealing temperature is within the austenite-ferrite two-phase region. If the annealing temperature is too low, the driving force for austenite reversal transformation is insufficient, resulting in an inadequate volume fraction of reversed austenite, making it difficult to fully utilize the TRIP effect. Furthermore, incomplete martensite tempering makes it difficult to fully eliminate residual stress, affecting plasticity and toughness. If the annealing temperature is too high, the stability of austenite decreases, and it is prone to transforming into fresh martensite during cooling, reducing the effective content of reversed austenite, exacerbating the tendency for grain coarsening, and impairing the material's strength and wear resistance. The holding time is set to simultaneously consider the full diffusion of carbon and manganese elements into austenite to improve austenite stability, while avoiding austenite grain coarsening or carbide precipitation due to excessively long holding times.
[0058] Specifically, in S4, the warm rolling is carried out at 550–630℃ (e.g., 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, 610℃, 620℃, 630℃) for 0.5–8 hours, e.g., 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h), the final warm rolling temperature is 530–610℃, e.g., 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, 610℃), and the warm rolling reduction rate is ≥60%, e.g., 60%, 65%, 70%, 75%, 80%, 85%.
[0059] It should be noted that excessively low temperatures result in excessive material deformation resistance, which is detrimental to subsequent rolling; excessively high temperatures may lead to a decrease in the stability of retained austenite. Controlling the final rolling temperature in warm rolling ensures that the material has sufficiently high plasticity during rolling while avoiding a sharp increase in mill load. A higher reduction rate can promote grain refinement and increase dislocation density, effectively enhancing the material's work hardening ability and overall strength; however, an excessive reduction rate can cause rolling defects or residual stress accumulation.
[0060] Specifically, in S5, the tempering temperature is 550–630℃, for example, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, 610℃, 620℃, or 630℃, and the tempering time is 0.5–8 hours, for example, 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours, or 8 hours. The selection of tempering temperature and time is mainly to take into account both the strength and ductility of medium manganese steel.
[0061] The high-strength, high-performance, wear-resistant medium-manganese steel prepared by the method of this invention has a grain size refined to several micrometers, with martensite / austenite distributed in lamellar form, and the retained austenite is mostly distributed in narrow strips or thin films at the lamellar interface, and locally in blocky form.
[0062] This invention optimizes the ratio and morphology of martensite and retained austenite in steel plates, resulting in steel plates that possess both high yield strength and excellent work hardening ability. By appropriately increasing the carbon content and precisely controlling the Mn element ratio and heat treatment process, it maintains high initial hardness while still possessing excellent work hardening ability, enabling it to adapt to complex working conditions such as impact and extrusion. This allows the material to maintain stable wear resistance during long-term wear, overcoming the shortcomings of insufficient hardening ability in traditional martensitic wear-resistant steels.
[0063] This invention improves the balance between strength and plasticity, making it suitable for machining wear-resistant components with complex shapes. Through a rational design of composition and heat treatment processes, it maintains high strength while also possessing high elongation, making it suitable for manufacturing complex-shaped wear-resistant structural parts in mining machinery and engineering equipment, thus significantly expanding the application range of high-performance wear-resistant steel.
[0064] The process of this invention is highly feasible and suitable for industrial production. Warm rolling and heat preservation can be achieved using conventional continuous annealing furnaces or bell-type furnaces; the warm rolling temperature and reduction are moderate, and the rolling load is acceptable to existing hot continuous rolling or narrow strip rolling lines, without the need for additional equipment, thus possessing the potential for large-scale promotion and application.
[0065] The advantages of precise control over the composition and process parameters of the high-strength, high-performance, wear-resistant manganese steel of the present invention are demonstrated below through specific embodiments and comparative examples. The chemical composition of the steel wires in the embodiments and comparative examples is shown in Table 1, the specific process parameters are shown in Table 2, and the mechanical properties of the high-strength, high-performance, wear-resistant manganese steel obtained during the preparation process are shown in Table 3.
[0066] Example
[0067] The embodiment employs converter smelting, followed by LF refining, RH degassing, electromagnetic stirring, and continuous casting to form slabs with a thickness of 40–200 mm. During continuous casting, the stretching speed is ≤1.5 m / min. The slabs are then cut into 5000 mm long billets and heated to 1180–1250 °C, held for 1–5 hours for homogenization. After exiting the furnace, the slabs are hot-rolled into hot-rolled plates with a diameter of 2–25 mm and a thickness. The initial rolling temperature is 1080–1150 °C, the final rolling temperature is 860–930 °C, the rolling reduction is ≥85%, and the plates are air-cooled after hot rolling.
[0068] The prepared hot-rolled plate is subjected to critical annealing treatment at a critical annealing temperature of 550–630℃ for 0.5–8h; then it is subjected to multiple warm rolling passes at 550–630℃ for 0.5–8h, with a final warm rolling temperature of 530–610℃ and a warm rolling reduction of ≥60%.
[0069] Finally, tempering is performed at a temperature of 550–630℃ for 0.5–8.0 h, followed by air cooling to room temperature to obtain medium manganese steel.
[0070] The preparation method of the comparative medium manganese steel is similar to that of the examples. The composition and process parameters in the preparation method are shown in Tables 1 and 2.
[0071] Table 1. Chemical composition (%) of manganese steel in the examples and comparative examples, balance being iron and unavoidable impurities.
[0072] Group C Si Mn Cr Ni Mo Ti Nb V Example 1 0.40 0.96 10.12 0 0.25 0.02 0.0025 0.0021 0.0025 Example 2 0.45 0.76 8.58 0.13 0.02 0.01 0.0018 0.0025 0.0013 Example 3 0.36 1.24 11.43 0 0 0.01 0.0012 0.0012 0.0017 Example 4 0.38 1.01 9.28 1.32 0.19 0.27 0.0021 0.0024 0.076 Example 5 0.35 1.16 9.35 0.12 2.17 0.47 0.49 0.36 0.98 Example 6 0.39 1.10 10.60 0 0 0 0 0 0 Comparative Example 1 0.20 0.56 9.96 0.56 0.63 0.12 0.0033 0.0017 0.23 Comparative Example 2 0.42 1.03 2.11 0.12 0.55 0.14 0.0019 0.025 0.82 Comparative Example 3 0.29 1.00 2.56 0.35 0.01 0.02 0.0018 0.0025 0.0013 Comparative Example 4 0.67 0.81 9.02 0.74 0.12 0.01 0.0028 0.0015 0.0033 Comparative Example 5 0.39 1.08 5.05 0.01 0.48 0.25 0.0013 0.032 0.74 Comparative Example 6 0.38 1.01 9.28 1.32 0.19 0.27 0.0021 0.0024 0.076 Comparative Example 7 0.38 1.01 9.28 1.32 0.19 0.27 0.0021 0.0024 0.076
[0073] Table 2. Process parameters during the preparation of the examples and comparative examples.
[0074]
[0075]
[0076] Table 3 Mechanical properties of manganese steel in the examples and comparative examples
[0077]
[0078] According to Table 3, the medium manganese steel prepared by the method of the present invention has a yield strength ≥1053 MPa, tensile strength ≥1390 MPa, total elongation after fracture ≥33.6%, strength-ductility product ≥46.7%, and a weight loss rate relative to NM400 steel plate in the sliding wear test under 30N load ≤70%.
[0079] Figure 1 The image shows the microstructure of the medium manganese steel prepared in Example 1 of this invention. It can be seen that the high strength, high ductility, and wear-resistant medium manganese steel prepared by the method of this invention has a grain size refined to several micrometers. The martensite / austenite is distributed in a lamellar manner, and the retained austenite is mostly distributed in narrow strips or thin films at the lamellar interface, and locally in a blocky manner.
[0080] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-strength, high-performance, wear-resistant medium-manganese steel, characterized in that, The chemical composition of the medium manganese steel, by mass percentage, is: C: 0.35%–0.45%, Si: 0.75%–1.25%, Mn: 8.5%–11.5%, with the balance being Fe and unavoidable impurities.
2. The high-strength, high-performance, wear-resistant medium-manganese steel according to claim 1, characterized in that, The chemical composition of the medium manganese steel also includes one or more of the following components: Cr: 0%–1.5%, Ni: 0%–3%, Mo: 0%–0.5%, Ti: 0%–0.5%, Nb: 0%–0.5%, V: 0%–1.0%.
3. A method for preparing high-strength, high-performance, wear-resistant medium-manganese steel as described in claim 1 or 2, characterized in that, Includes the following steps: S1: According to the chemical composition of the medium manganese steel, the raw materials are batched, smelted, and cast to obtain a slab; S2: The slab is subjected to homogenization treatment and rolling in sequence to obtain a hot-rolled plate; S3: Anneal the hot-rolled plate and then cool it to room temperature to obtain a steel plate; S4: The steel plate is subjected to warm rolling and then cooled to room temperature; S5: The rolled steel plate is tempered and then cooled to room temperature to obtain the medium manganese steel.
4. The preparation method according to claim 3, characterized in that, In S1, the casting is carried out by die casting or continuous casting. When continuous casting is used, the stretching speed is ≤1.5m / min.
5. The preparation method according to claim 3, characterized in that, In S2, the homogenization treatment temperature is 1180–1250°C, and the homogenization time is 1–5 h.
6. The preparation method according to claim 3, characterized in that, In S2, the initial rolling temperature is 1080–1150°C, the final rolling temperature is 860–930°C, and the rolling reduction rate is ≥85%.
7. The preparation method according to claim 3, characterized in that, In S3, the annealing temperature is 550–630°C, and the holding time is 0.5–8 hours.
8. The preparation method according to claim 3, characterized in that, In S4, the warm rolling is carried out at 550-630℃ for 0.5-8 hours, and the final rolling temperature is 530-610℃.
9. The preparation method according to claim 8, characterized in that, Warm rolling reduction rate ≥ 60%.
10. The preparation method according to claim 3, characterized in that, In S5, the tempering temperature is 550–630°C, and the tempering time is 0.5–8 hours.
Citation Information
Patent Citations
High-wear-resistance martensite / austenite biphasic wear-resistant steel plate and manufacturing method thereof
CN110592491A
1000MPa-grade medium manganese TRIP steel with continuous yield and preparation method of 1000MPa-grade medium manganese TRIP steel
CN112159931A
Medium manganese steel with high product of strength and elongation and preparation method thereof
CN112410681A