Large-size polytetrafluoroethylene filled hydraulic product and preparation method thereof
By controlling the mixing ratio of polytetrafluoroethylene resin and copper powder and the pressure application method, large-size, high-strength polytetrafluoroethylene-filled hydraulic products were prepared, solving the problem of insufficient product strength in the existing technology and achieving higher compressive strength, making them suitable for strict insulation environments.
Patent Information
- Application Number
- CN202511792258.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-01
- Publication Date
- 2026-04-21
AI Technical Summary
Existing technologies make it difficult to manufacture large, irregularly shaped PTFE hydraulic products, and the strength of these hydraulic products is insufficient to meet the stringent requirements of insulation and sealing environments.
By controlling the mixing ratio of polytetrafluoroethylene resin and copper powder, and using specific pressure and pressure application methods, combined with vacuum treatment and sintering processes, large-size, high-strength polytetrafluoroethylene-filled hydraulic products are prepared.
The compressive strength of PTFE hydraulic products has been significantly improved, giving them better application prospects in strictly insulating environments. The compressive strength has been increased from 30MPa to over 45MPa.
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer material processing, specifically to a method for preparing large-format polytetrafluoroethylene-filled hydraulic products. Background Technology
[0002] Polytetrafluoroethylene (PTFE) stands out due to its superior overall performance. It possesses excellent corrosion resistance and chemical stability, resisting the erosion of most acidic and alkaline media. It also exhibits good aging resistance, electrical insulation, and a wide temperature range, while remaining purely inert. These advantages make it a vital material in numerous fields such as aerospace, chemical machinery, and electronics, especially in demanding insulation and sealing applications, where it is a highly competitive and ideal material.
[0003] Patent application CN100365025C discloses a method for manufacturing high-strength polytetrafluoroethylene (PTFE), which involves polymerizing PTFE in an aqueous medium in the presence of a water-soluble polymerization initiator to produce PTFE resin. Patent application CN106009429A proposes improving the mechanical strength of PTFE plastics by adding toughening agents, impact modifiers, heat stabilizers, and fillers. Patent application CN104817796A proposes adding modified corundum ultrafine powder with a particle size of 1000-325 mesh as a reinforcing agent and wear-resistant agent during the preparation of PTFE, thereby improving the strength and hardness of the PTFE plastic. These patents improve the strength of PTFE by modifying the resin and raw material formulations, but do not describe the molding method of the product. Patent application CN105666889A discloses a method for preparing high-strength PTFE films by improving calendering and stretching processes. However, traditional molding methods for PTFE products, such as compression molding and calendering, are limited by the molds or molding methods and cannot produce large or irregularly shaped PTFE products. Furthermore, current patent literature on PTFE hydroforming does not provide a detailed description of how to improve the strength of hydroformed products. The compressive strength of the high-strength PTFE hydroformed product preparation method proposed in patent application CN108284554A is relatively low.
[0004] There is an urgent need to provide large-format PTFE hydraulic products with improved strength for better application in fields with more demanding insulation and sealing environments. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a large-size polytetrafluoroethylene (PTFE) filled hydraulic product and its preparation method. The large-size, high-strength PTFE hydraulic product provided by this invention can effectively improve the compressive strength of large-size PTFE hydraulic products and can be well used in environments with more stringent insulation requirements.
[0006] In a first aspect, the present invention provides a method for preparing large-size, high-strength polytetrafluoroethylene-filled hydraulic products, comprising the following steps: 1) After mixing polytetrafluoroethylene resin and copper powder, the mixture is placed into a mold to form an inner bag; the inner bag is then packaged with a rubber bag to form an outer bag; the mass percentage of the polytetrafluoroethylene resin is 10% to 90% of the total mass of the polytetrafluoroethylene resin and copper powder.
[0007] 2) The outer bag is vacuumed and then pressure-treated to obtain a hydraulic blank; the pressure-treatment includes treatment under a first pressure and then treatment under a second pressure, wherein the second pressure is greater than the first pressure.
[0008] 3) The hydraulic blank is left to stand and then sintered. This invention, by controlling the mixing ratio of PTFE resin and copper powder, as well as the pressure and application method during the preparation of PTFE-filled hydraulic products, can effectively improve the strength of PTFE hydraulic products and has excellent application prospects.
[0009] Preferably, in step 1), the polytetrafluoroethylene (PTFE) resin accounts for 50% to 70% of the total mass of PTFE resin and copper powder; more preferably, the PTFE resin accounts for 55% to 65% of the total mass of PTFE resin and copper powder. Using the above-mentioned specific PTFE resin and copper powder mixture can further improve the strength of large-size PTFE-filled hydraulic products, and the preferred ratio can improve the overall performance of the filled products.
[0010] Preferably, in step 2), the pressure treatment method includes: holding at a pressure of 5-15 MPa, then increasing the pressure to 16-30 MPa and holding at that pressure; preferably, the pressure treatment method includes: holding at a pressure of 10-15 MPa for 15-25 minutes, then increasing the pressure to 20-25 MPa and holding at that pressure for 20-60 minutes. The preferred pressure treatment method and conditions, combined with the polytetrafluoroethylene resin and copper powder mixture, can better achieve synergistic effects, further improving the compressive strength of the product and resulting in better overall performance.
[0011] Further preferably, in step 1), the copper powder is 300-500 mesh. The use of copper powder of a preferred specification in this invention results in better preparation.
[0012] Preferably, the mold includes a PVC film mold.
[0013] Preferably, the mold size is 30% to 40% larger than the final required product size in all directions.
[0014] Further preferred, in step 2), the pressurization rate is 0.5~1MPa / min and the depressurization rate is 0.2~0.8MPa / min.
[0015] Further preferred, in step 1), the polytetrafluoroethylene resin is a suspension resin.
[0016] Further preferred, in step 3), the settling time is 12~24h.
[0017] Preferably, in step 3), the sintering temperature is 365~380℃ and the sintering time is 72~100h; Further optimization includes step 4), which involves machining the shaped blank obtained in step 3).
[0018] Secondly, the present invention provides a large-size polytetrafluoroethylene-filled hydraulic product, which is prepared by the above-described preparation method. The compressive strength of the product (large-size polytetrafluoroethylene-filled hydraulic product Φ280×650mm) obtained by the method of the present invention preferably reaches 33~45MPa.
[0019] The beneficial effects of this invention are at least as follows: By controlling the proportion of copper powder added, as well as the pressure and application method during the preparation of PTFE-filled hydraulic products, this invention can effectively improve the strength of large-size PTFE hydraulic products. The products prepared by this invention have significant application prospects and can be used in environments with more stringent insulation requirements. The compressive strength is increased from 30 MPa to over 45 MPa, which well meets the requirements of users. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0021] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.
[0022] Unless otherwise specified, the techniques or conditions described in the literature of this invention shall apply, or the product instructions shall be followed. Devices, instruments, reagents, etc., whose manufacturers are not specified, are all conventional products that can be purchased from legitimate channels. All experimental reagents and raw materials involved are commercially available, and all reagents are analytical grade products.
[0023] The polytetrafluoroethylene suspension resin used in the following examples is CGM16F, provided by Zhonghao Chenguang Chemical Research Institute Co., Ltd.; the copper powder is 400 mesh and is commercially available.
[0024] Example 1 This embodiment provides a large-size polytetrafluoroethylene-filled hydraulic product and its preparation method, the steps of which are as follows: 1) Prepare a PVC film mold of the appropriate size, with a diameter of 350mm and a height of 1000mm; 2) Mix polytetrafluoroethylene resin and copper powder in a certain proportion (PTFE resin accounts for 65% of the total mass) and then fill the mold to form an inner bag.
[0025] 3) Pack the inner bag with a rubber bag to form an outer bag.
[0026] 4) After vacuuming the outer bag using a vacuum pump, place it in an autoclave for pressurization: hold the pressure at 10 MPa for 15 minutes, then increase the pressure to 15 MPa (pressure increase rate 0.8 MPa / min), hold the pressure for 30 minutes, and then slowly depressurize (pressure depressurization rate 0.5 MPa / min), and remove it to obtain a hydraulic blank.
[0027] 5) After the above hydraulic blank is left to stand for 24 hours, it is sintered at 370°C for 80 hours to obtain the shaped blank.
[0028] 6) The above-mentioned molded blank is machined to obtain a polytetrafluoroethylene filled hydraulic product with a diameter of Φ280×650mm.
[0029] The compressive strength of the polytetrafluoroethylene-filled hydraulic product is 34 MPa.
[0030] Example 2 This embodiment provides a large-size polytetrafluoroethylene-filled hydraulic product and its preparation method, the steps of which are as follows: 1) Prepare a PVC film mold of the appropriate size, with a diameter of 350mm and a height of 1000mm; 2) Mix polytetrafluoroethylene resin and copper powder in a certain proportion (PTFE resin accounts for 65% of the total mass) and then fill the mold to form an inner bag.
[0031] 3) Pack the inner bag with a rubber bag to form an outer bag.
[0032] 4) After vacuuming the outer bag using a vacuum pump, place it in an autoclave for pressurization: hold the pressure at 10 MPa for 15 minutes, then increase the pressure to 20 MPa (pressure increase rate 0.8 MPa / min), hold the pressure for 30 minutes, and then slowly depressurize (pressure depressurization rate 0.5 MPa / min), and remove it to obtain a hydraulic blank.
[0033] 5) After the above hydraulic blank is left to stand for 24 hours, it is sintered at 370°C for 80 hours to obtain the shaped blank.
[0034] 6) The above-mentioned molded blank is machined to obtain a polytetrafluoroethylene filled hydraulic product with a diameter of Φ280×650mm.
[0035] The compressive strength of the polytetrafluoroethylene-filled hydraulic product was 39 MPa.
[0036] Example 3 This embodiment provides a large-size polytetrafluoroethylene-filled hydraulic product and its preparation method, the steps of which are as follows: 1) Prepare a PVC film mold of the appropriate size, with a diameter of 350mm and a height of 1000mm.
[0037] 2) Mix polytetrafluoroethylene resin and copper powder in a certain proportion (PTFE resin accounts for 55% of the total mass) and then fill the mold to form an inner bag.
[0038] 3) Pack the inner bag with a rubber bag to form an outer bag.
[0039] 4) After vacuuming the outer bag using a vacuum pump, place it in an autoclave for pressurization: hold the pressure at 15MPa for 15 minutes, then increase the pressure to 25MPa (pressure increase rate 0.8MPa / min), hold the pressure for 30 minutes, and then slowly depressurize (pressure depressurization rate 0.5MPa / min), and remove it to obtain a hydraulic blank.
[0040] 5) After the above hydraulic blank is left to stand for 24 hours, it is sintered at 370°C for 80 hours to obtain the shaped blank.
[0041] 6) The above-mentioned molded blank is machined to obtain a polytetrafluoroethylene filled hydraulic product with a diameter of Φ280×650mm.
[0042] The compressive strength of the polytetrafluoroethylene-filled hydraulic product is 45 MPa.
[0043] Example 4 This embodiment provides a large-size polytetrafluoroethylene-filled hydraulic product and its preparation method, the steps of which are as follows: 1) Prepare a PVC film mold of the appropriate size, with a diameter of 350mm and a height of 1000mm; 2) Mix polytetrafluoroethylene resin and copper powder in a certain proportion (PTFE resin accounts for 75% of the total mass) and then fill the mold to form an inner bag.
[0044] 3) Pack the inner bag with a rubber bag to form an outer bag.
[0045] 4) After vacuuming the outer bag using a vacuum pump, place it in an autoclave for pressurization: hold the pressure at 10 MPa for 15 minutes, then increase the pressure to 15 MPa (pressure increase rate 0.8 MPa / min), hold the pressure for 30 minutes, and then slowly depressurize (pressure depressurization rate 0.5 MPa / min), and remove it to obtain a hydraulic blank.
[0046] 5) After the above hydraulic blank is left to stand for 24 hours, it is sintered at 370°C for 80 hours to obtain the shaped blank.
[0047] 6) The above-mentioned molded blank is machined to obtain a polytetrafluoroethylene filled hydraulic product with a diameter of Φ280×650mm.
[0048] The compressive strength of the polytetrafluoroethylene-filled hydraulic product is 33 MPa.
[0049] Comparative Example 1 1) Prepare a PVC film mold of the appropriate size, with a diameter of 350mm and a height of 1000mm.
[0050] 2) Mix polytetrafluoroethylene resin and copper powder in a certain proportion (PTFE resin accounts for 75% of the total mass) and then fill the mold to form an inner bag.
[0051] 3) Pack the inner bag with a rubber bag to form an outer bag.
[0052] 4) After vacuuming the outer bag using a vacuum pump, place it in an autoclave for pressurization: hold the pressure at 10MPa for 45 minutes and slowly release the pressure (release rate 0.5MPa / min), then remove it to obtain a hydraulic blank.
[0053] 5) After the above hydraulic blank is left to stand for 24 hours, it is sintered at 370°C for 80 hours to obtain the shaped blank.
[0054] 6) The above-mentioned molded blank is machined to obtain a polytetrafluoroethylene filled hydraulic product with a diameter of Φ280×650mm.
[0055] The compressive strength of the polytetrafluoroethylene-filled hydraulic product is 31 MPa.
[0056] Comparative Example 2 The only difference from Example 1 is that step 4) does not involve applying pressure.
[0057] The resulting polytetrafluoroethylene-filled hydraulic products are not dense enough, have many pores, or cannot be formed.
[0058] Comparative Example 3 The only difference from Example 2 is that in step 2), the percentage of PTFE resin by mass is changed from 65% to 8% of the total mass of PTFE resin and copper powder.
[0059] The compressive strength of the polytetrafluoroethylene-filled hydraulic products is only 30 MPa.
[0060] Comparative Example 4 The only difference from Example 3 is that copper powder is not added in step 2).
[0061] The compressive strength of the polytetrafluoroethylene-filled hydraulic product is only 29 MPa.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a large-size, high-strength polytetrafluoroethylene-filled hydraulic product, characterized in that, Includes the following steps: 1) After mixing polytetrafluoroethylene resin and copper powder, the mixture is placed into a mold to form an inner bag; the inner bag is then packaged with a rubber bag to form an outer bag; the mass percentage of the polytetrafluoroethylene resin is 10% to 90% of the total mass of the polytetrafluoroethylene resin and copper powder; 2) The outer bag is vacuumed and then subjected to pressure treatment to obtain a hydraulic blank; the pressure treatment includes treatment under a first pressure and then treatment under a second pressure, wherein the second pressure is greater than the first pressure; 3) The hydraulic blank is left to stand and then sintered.
2. The preparation method according to claim 1, characterized in that, In step 1), the polytetrafluoroethylene resin accounts for 50% to 70% of the total mass of the polytetrafluoroethylene resin and copper powder; Preferably, the polytetrafluoroethylene resin accounts for 55% to 65% of the total mass of the polytetrafluoroethylene resin and copper powder.
3. The preparation method according to claim 1 or 2, characterized in that, In step 2), the pressure treatment method includes: maintaining pressure at 5~15MPa, then increasing the pressure to 16~30MPa and maintaining pressure.
4. The preparation method according to claim 3, characterized in that, The pressure treatment method includes: maintaining the pressure at 10~15MPa for 15~25min, then increasing the pressure to 20~25MPa and maintaining the pressure for 20~60min.
5. The preparation method according to any one of claims 1-4, characterized in that, In step 1), the copper powder is 300-500 mesh; and / or, the mold includes a PVC film mold; and / or, the mold size is 30% to 40% larger than the final required product size in all directions.
6. The preparation method according to any one of claims 1-5, characterized in that, In step 2), the pressurization rate is 0.5~1MPa / min and the depressurization rate is 0.2~0.8MPa / min.
7. The preparation method according to any one of claims 1-6, characterized in that, In step 1), the polytetrafluoroethylene resin is a suspension resin.
8. The preparation method according to any one of claims 1-7, characterized in that, In step 3), the settling time is 12-24 hours; and / or the sintering temperature is 365-380°C and the sintering time is 72-100 hours.
9. The preparation method according to any one of claims 1-8, characterized in that, It also includes step 4), which involves machining the shaped blank obtained in step 3).
10. A large-format polytetrafluoroethylene-filled hydraulic product, characterized in that, It is prepared by the preparation method according to any one of claims 1-9.
Citation Information
Patent Citations
Process for producing high-strength tetrafluoroethylene polymer
CN100365025C
Method for improving strength and wear resistance of polytetrafluoroethylene
CN104817796A
Preparation method of high-intensity teflon film
CN105666889A
High-strength durable polytetrafluoroethylene plastic
CN106009429A
Preparation method of high-strength polytetrafluoroethylene hydraulic product
CN108284554A