Nickel-based catalyst as well as preparation method and application thereof
By using a magnesium-aluminum aerogel support and a nickel-based catalyst combined with a modifying agent, a highly active and low-cost ultra-low temperature methanation catalyst was prepared, which solved the problems of low activity and high cost of existing catalysts, and achieved a reduction in energy consumption and an improvement in hydrogen quality in the low-temperature methanation process.
Patent Information
- Application Number
- CN202411538638.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2026-05-01
AI Technical Summary
Existing ultra-low temperature methanation catalysts suffer from low activity, high reduction temperature, poor thermal stability, and high production costs, making it difficult to meet the energy consumption requirements of the low-temperature methanation process.
A catalyst was prepared by impregnation using a magnesium-aluminum aerogel support and a nickel-based catalyst, combined with modifying agents such as metals from Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB and Group VIII. This method improves the dispersion and specific surface area of the active metal and reduces the cost of the catalyst.
This technology enables methanation reactions with high activity and stability at low temperatures, reducing production costs and improving the environmental friendliness of the catalyst, while meeting the hydrogen quality requirements of downstream processes.
Smart Images

Figure CN121945080A_ABST
Abstract
Description
Nickel-based catalysts, their preparation methods and applications Technical Field
[0001] This invention relates to the field of preparation of ultra-low temperature methanation catalysts, specifically to a nickel-based catalyst, its preparation method, and its application. Background Technology
[0002] In the industrial plant producing ethylene from naphtha and light hydrocarbons through cracking, the hydrogen-rich gas separated from the hydrogen / methane separator inevitably contains CO and CO2. This portion of H2 is the feedstock for downstream hydrogenation processes. Failure to remove the CO will cause poisoning and deactivation of the hydrogenation catalyst. In ammonia synthesis plants, the feedstock gas after CO conversion and CO2 removal still contains small amounts of CO and CO2; the requirement for entering the reactor is below 10 ppm. In proton exchange membrane fuel cells (PEMFCs), considered the most likely replacement for internal combustion engines, the Pt electrode's tolerance to CO is below 10 ppm. Methanation is a common method for purifying crude hydrogen in methane steam reforming for hydrogen production, steam cracking for ethylene production, and ammonia synthesis, and it has significant research and application value. Although there are many suppliers of methanation catalysts both domestically and internationally, they all suffer from problems such as low activity, high reduction temperature, and poor thermal stability. Furthermore, conventional methanation processes typically require a reactor inlet temperature of 280℃, meaning that conventional methanation processes have high energy consumption. If the activity of the methanation catalyst can meet the requirement of trace amounts at the outlet when the reactor inlet temperature is between 150 and 200°C, the energy consumption of the process can be significantly reduced; this is known as cryogenic methanation. Therefore, developing cryogenic methanation catalysts with high activity and good thermal stability is an important research direction in this field.
[0003] Currently, ultra-low temperature methanation catalysts are mainly of two types: Ru-based and Ni-based. Foreign countries have primarily developed Ru-based catalysts and Ni-based catalysts with high Ni content produced via co-precipitation methods. For example, the C13-LT catalyst from Southern Chemical Industry is an ultra-low temperature methanation catalyst with Ru as the active metal, while the N111 catalyst from NIKKI Corporation of Japan is a high-Ni-content Ni-based catalyst produced via co-precipitation, with a NiO content exceeding 55%, significantly increasing catalyst costs. Domestically produced ultra-low temperature methanation catalysts are mainly the BC-H-10 developed by the Beijing Institute of Chemical Technology, produced via a multiple impregnation method, but the NiO content still exceeds 50%, resulting in high production costs and a complex process. Furthermore, due to outdated preparation processes, catalyst performance still has considerable room for improvement, primarily due to poor low-temperature activity, high reduction and activation temperatures, and poor thermal stability. Therefore, there remains a significant market demand for developing novel, highly active, highly stable, and low-cost ultra-low temperature methanation catalysts. Summary of the Invention
[0004] The purpose of this invention is to overcome the problems existing in the prior art and provide a nickel-based catalyst, its preparation method, and its application. When the catalyst provided by this invention is applied to the ultra-low temperature methanation reaction for crude hydrogen purification, it exhibits advantages such as high activity, high methane selectivity, and good stability.
[0005] To achieve the above objectives, the first aspect of the present invention provides a nickel-based catalyst, the catalyst comprising a magnesium-aluminum aerogel support, an active metal component, and a modifying agent; the active metal component is nickel; the modifying agent is selected from at least one of Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB, and Group VIII metal elements.
[0006] The dispersion of the active metal component is not less than 10%.
[0007] A second aspect of this invention provides a method for preparing a nickel-based catalyst, the method comprising the following steps:
[0008] (1) Aluminum salt, magnesium salt, swelling agent and solvent are gelled and then supercritically dried to obtain magnesium aluminum aerogel precursor;
[0009] (2) The magnesium-aluminum aerogel precursor and the extrusion aid are mixed and molded, and then subjected to a first drying and a first calcination to obtain a magnesium-aluminum aerogel carrier.
[0010] (3) Introduce active metal components and modifying agents onto the magnesium-aluminum aerogel carrier by impregnation method;
[0011] The active metal component is nickel; the modifying agent is selected from at least one of Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB and Group VIII metal elements.
[0012] The third aspect of this invention provides the application of the nickel-based catalyst described in the first aspect or the nickel-based catalyst prepared by the preparation method described in the second aspect in the methanation reaction for crude hydrogen purification.
[0013] The beneficial effects of the present invention through the above technical solution include:
[0014] When the catalyst provided by this invention is applied to the methanation reaction of crude hydrogen purification, it has the advantages of high activity, high methane selectivity and good stability, and can fully meet the requirements of downstream processes for hydrogen quality.
[0015] In a preferred embodiment, the catalyst provided by the present invention still exhibits high activity even with low amounts of active metal components, thereby significantly reducing production costs.
[0016] Compared with traditional hydrothermal and precipitation methods, the catalyst preparation method provided by this invention is simple to operate, has a short preparation cycle, and has the advantages of high efficiency and energy saving. It avoids the generation of a large amount of wastewater containing metal ions and nitrates during the precipitation or hydrothermal product washing process, thereby reducing production costs and enhancing the green and environmentally friendly advantages of the preparation method. Attached Figure Description
[0017] Figure 1 is the H2-TPR spectrum of the catalysts prepared in Example 1 and Comparative Example 1 of the present invention;
[0018] Figure 2 shows the evaluation results of the catalyst prepared in Example 1 after 1000 hours of long-term operation. Detailed Implementation
[0019] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0020] The first aspect of the present invention provides a nickel-based catalyst, the catalyst comprising a magnesium-aluminum aerogel support, an active metal component, and a modifying agent; the active metal component is nickel; the modifying agent is selected from at least one of Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB, and Group VIII metal elements.
[0021] The dispersion of the active metal component is not less than 10%.
[0022] According to the present invention, the dispersion of the active metal component is not less than 10%, specifically it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, and the range of any two of these values, preferably 11-20%. This preferred embodiment is beneficial for improving the low-temperature activity of the catalyst.
[0023] According to the present invention, preferably, the specific surface area of the active metal component is not less than 7 m². 2 / g cat Specifically, it can be 7m 2 / g cat 7.5m 2 / g cat 8m 2 / g cat 8.5m 2 / gcat 9m 2 / g cat 9.5m 2 / g cat 10m 2 / g cat 10.5m 2 / g cat 11m 2 / g cat 11.5m 2 / g cat 12m 2 / g cat 12.5m 2 / g cat 13m 2 / g cat 13.5m 2 / g cat 14m 2 / g cat 14.5m 2 / g cat 15m 2 / g cat And the range of any two of these point values, preferably 7-15m. 2 / g cat .
[0024] According to the present invention, preferably, the specific surface area of the active metal component is not less than 60 m². 2 / g Ni Specifically, it can be 60m 2 / g Ni 65m 2 / g Ni 70m 2 / g Ni 75m 2 / g Ni 80m 2 / g Ni 85m 2 / g Ni 90m 2 / g Ni 95m 2 / g Ni 100m 2 / g Ni 105m 2 / g Ni 110m 2 / g Ni 115m 2 / g Ni 120m 2 / g NiAnd the range of any two of these point values, preferably 65-100m. 2 / g Ni .
[0025] According to the present invention, preferably, the average particle size of the active metal component is not greater than 10 nm, and more preferably 1-9 nm.
[0026] The dispersion, specific surface area, and average particle size of the active metal component described in this invention were determined by chemisorption, specifically using an AutoChem2950 automated catalyst characterization and adsorption instrument manufactured by Micromeritics, USA. 200 mg of catalyst was reduced in situ at 400 °C in a hydrogen atmosphere for 2 h, followed by Ar purging at the same temperature for 30 min, and then cooled to 100 °C for hydrogen pulse chemisorption testing. The pulse gas was H2 / Ar with a volume fraction of 10% H2.
[0027] The dispersion degree D, specific surface area S1 (based on catalyst), specific surface area S2 (based on metal), and average particle size d of the active component are calculated using the following formulas:
[0028]
[0029]
[0030]
[0031]
[0032] In the formula, V H The total volume of H2 adsorbed by the sample is expressed in mL; Fs is the stoichiometric factor between the adsorbed substance (H2) and the active metal (nickel); N0 is Avogadro's constant, 6.019 × 10⁻⁶. 23 ;σ 金属 The cross-sectional area of the metal (see Chemical Handbook), unit m. 2 m is the sample mass in g; W is the mass fraction of metal oxide in the catalyst as determined by XRF, %; M is the relative atomic mass or relative molecular mass; ρ is the metal density in g / cm³. 3 A is the instrument calibration coefficient.
[0033] In the above formula, the number of H atoms is obtained by converting the volume of H2 obtained through chemical adsorption test, and then the number of active metal components on the catalyst surface is calculated from the number of H atoms; the mass of the active metal components in the catalyst is measured by XRF, and then the number of active metal components in the catalyst is calculated.
[0034] According to the present invention, preferably, the crushing strength of the catalyst is above 400 N / cm, and more preferably 400-600 N / cm.
[0035] The crushing strength of the catalyst described in this invention is measured by a strength tester. Twenty test ball samples are measured, and one maximum and one minimum value are removed. The average value of the other data is taken to obtain the crushing strength of the test ball samples.
[0036] The catalyst provided by this invention has stable texture properties (strength above 400 N / cm), small particle size of active metal components (below 10 nm), and large specific surface area of active metal components, exhibiting excellent reaction characteristics in the methanation reaction of crude hydrogen purification.
[0037] The catalyst provided by this invention has a low reduction and activation temperature, and the reduction and activation operation is simple and has a short cycle before the reaction starts, which greatly saves start-up time.
[0038] According to the present invention, preferably, the temperature corresponding to the highest peak in the H2-TPR spectrum of the catalyst is 200-450℃, more preferably 250-350℃, as characterized by H2-TPR.
[0039] The H2-TPR process described in this invention specifically includes: The process is performed on an Autochem 2950 automated catalyst characterization and adsorption instrument manufactured by Micromeritics, USA, with a sample loading of approximately 0.20 g. First, the sample is heated to 120°C under an Ar gas flow for dehydration. Then, after the temperature drops to 50°C, the TPR experiment is conducted. The experimental conditions and procedure are as follows: heating rate 10°C / min, final temperature 900°C, reducing gas is a 10% H2 / N2 mixture at a flow rate of 50 mL / min, using a thermal conductivity detector, to obtain the H2-TPR reduction curve. The temperature corresponding to the highest reduction peak represents the suitable reduction and activation temperature of the catalyst.
[0040] The catalyst provided by this invention maintains high activity even with low amounts of active metal component, significantly reducing production costs. Preferably, the mass content of the active metal component, calculated as oxide, is 5-25%, more preferably 10-20%.
[0041] According to the present invention, preferably, based on the total mass of the catalyst, the mass content of the magnesium-aluminum aerogel support is 70-94%, more preferably 79-89%; the mass content of the active metal component, calculated as oxides, is 5-25%, more preferably 10-20%; and the mass content of the modifying agent, calculated as oxides, is 0.5-5%, more preferably 1-5%.
[0042] The components in the catalyst described in this invention were measured by XRF.
[0043] The present invention has a wide range of choices for the types of modifying agents. Preferably, the modifying agent is selected from at least one of yttrium, lanthanum, cerium, zirconium, titanium and vanadium, and more preferably from at least one of yttrium, lanthanum and cerium.
[0044] In existing catalysts, a large specific surface area of the support is beneficial for increasing the number of active sites and thus improving reaction activity, but it often reduces the catalyst strength, which is detrimental to the long-term reaction. The catalyst provided by this invention, however, can simultaneously possess both high strength and a large specific surface area of the support. Preferably, the specific surface area of the magnesium-aluminum aerogel support is 200-400 m². 2 / g, preferably 200-300m 2 / g.
[0045] According to the present invention, preferably, in the magnesium-aluminum aerogel carrier, the mass ratio of magnesium to aluminum, calculated as oxides, is 2-10:90-98.
[0046] A second aspect of this invention provides a method for preparing a nickel-based catalyst, the method comprising the following steps:
[0047] (1) Aluminum salt, magnesium salt, swelling agent and solvent are gelled and then supercritically dried to obtain magnesium aluminum aerogel precursor;
[0048] (2) The magnesium-aluminum aerogel precursor and the extrusion aid are mixed and molded, and then subjected to a first drying and a first calcination to obtain a magnesium-aluminum aerogel carrier.
[0049] (3) Introduce active metal components and modifying agents onto the magnesium-aluminum aerogel carrier by impregnation method;
[0050] The active metal component is nickel; the modifying agent is selected from at least one of Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB and Group VIII metal elements.
[0051] The catalyst preparation method provided by this invention can simply and efficiently prepare the catalyst described in the first aspect. The preparation method of this invention is simple to operate, has a short preparation cycle, and has the advantages of high efficiency and energy saving; it avoids the generation of large amounts of wastewater containing metal ions and nitrates during precipitation methods or hydrothermal product washing processes, thereby reducing production costs and enhancing the green and environmentally friendly advantages of the preparation method.
[0052] According to the present invention, preferably, the mass ratio of magnesium salt to aluminum salt, based on metal oxides, is 2-10:90-98.
[0053] This invention does not specifically limit the types of magnesium and aluminum salts mentioned, and they can be various magnesium and aluminum salts commonly found in the art. For example, they can be magnesium nitrate, magnesium chloride, magnesium sulfate, aluminum nitrate, aluminum chloride, aluminum sulfate, etc.
[0054] The present invention allows for a wide range of choices regarding the type of expanding agent. Preferably, the expanding agent is propylene oxide and formamide. This preferred embodiment is beneficial for increasing the specific surface area of the carrier.
[0055] According to the present invention, preferably, the mass ratio of the expanding agent to the aluminum salt is 0.5-5:1, more preferably 1-2:1.
[0056] According to the present invention, preferably, the mass ratio of propylene oxide to formamide is 5-30:1, more preferably 10-20:1.
[0057] The present invention allows for a wide range of solvent choices, which can be conventional choices in the field. Ethanol and water are preferably used as solvents in the embodiments of the present invention.
[0058] The present invention does not have a particular limitation on the amount of solvent used, as long as the other substances are mixed evenly.
[0059] According to one specific embodiment of the present invention, aluminum salt, magnesium salt, and water are mixed, then a swelling agent and ethanol are added, and the mixture is gelled to obtain a gel. Conventional methods such as stirring or ultrasound can be used during the mixing process of the substances described in this invention to achieve uniform mixing.
[0060] According to the present invention, preferably, the gelation conditions in step (1) include: a temperature of 40-70°C and a time of 0.5-3h.
[0061] The present invention does not have any particular limitation on the supercritical drying in step (1), and conventional supercritical drying methods in the art can be used. Preferably, the supercritical drying in step (1) is supercritical carbon dioxide drying.
[0062] The present invention allows for a wide range of specific conditions for supercritical carbon dioxide drying. In order to increase the specific surface area of the carrier, the conditions for supercritical carbon dioxide drying preferably include: pressure of 6-22 MPa, preferably 8-12 MPa; temperature of 240-450℃, preferably 250-300℃; and drying time of 0.5-8 h, preferably 1-4 h.
[0063] Preferably, the method further includes washing the gel obtained by gelling in step (1) with ethanol before supercritical drying to exchange out the solvent water.
[0064] The present invention does not impose any particular limitation on the ethanol exchange process, and it can be carried out with reference to conventional methods in the art.
[0065] According to the present invention, preferably, the specific surface area of the magnesium-aluminum aerogel carrier obtained in step (2) is 200-400 m². 2 / g, preferably 200-300m 2 / g.
[0066] The present invention allows for a wide range of choices for the extrusion additives, including conventional options in the field, such as hydroxymethyl cellulose, guar gum powder, and soluble starch.
[0067] The present invention does not impose a particular limitation on the amount of the extrusion aid, as long as the subsequent molding is successful, and conventional methods in the art can be referred to. Preferably, the amount of the extrusion aid is 0.1-10 parts by weight relative to 100 parts by weight of magnesium-aluminum aerogel precursor.
[0068] Preferably, a peptizing solvent is also added during the mixing in step (2). The present invention allows for a wide range of choices for the type of peptizing solvent, including conventional choices in the art, such as nitric acid.
[0069] The present invention does not impose a particular limitation on the amount of the adhesive solvent used, as long as the subsequent molding process is successful, and conventional methods in the art can be referred to. Preferably, the amount of the adhesive solvent is 0.02-6 parts by weight relative to 100 parts by weight of magnesium-aluminum aerogel precursor.
[0070] Preferably, water is also added to the mixture in step (2).
[0071] The present invention does not impose a particular limitation on the amount of water used, as long as the subsequent molding process is successful, and conventional methods in the art can be followed. Preferably, the weight ratio of water to magnesium-aluminum aerogel precursor is 0.3-1.8:1.
[0072] The present invention does not impose any particular limitation on the molding process described in step (2), and appropriate methods can be selected from conventional molding methods in the field according to actual needs. An exemplary embodiment of the present invention uses extrusion molding for molding.
[0073] The present invention does not have any particular limitation on the first drying in step (2), and can be carried out with reference to conventional methods in the art.
[0074] Preferably, the conditions for the first roasting in step (2) include: a temperature of 500-1000℃ and a time of 2-10h.
[0075] According to the present invention, preferably, the amount of active metal component and modifying agent introduced in step (3) is such that, based on the total mass of the catalyst, the mass content of the magnesium-aluminum aerogel support is 70-94%, preferably 79-89%; the mass content of the active metal component, calculated as oxide, is 5-25%, preferably 10-20%; and the mass content of the modifying agent, calculated as oxide, is 0.5-5%, preferably 1-5%.
[0076] According to the present invention, preferably, the impregnation method in step (3) includes: contacting an impregnation solution containing an active metal component compound and a modified auxiliary compound with a magnesium-aluminum aerogel carrier, and then performing a second drying and a second calcination.
[0077] The present invention does not specifically limit the method of impregnation. The method of impregnation can be impregnation with excess liquid or impregnation with equal volume, depending on the amount of impregnation liquid used.
[0078] The present invention does not have a particular limitation on the number of impregnations; impregnation can be performed once or multiple times, as long as the mass content of the active metal component and the modifying agent in the catalyst is within the above-mentioned range.
[0079] This invention does not impose a particular limitation on the impregnation temperature; it can be carried out using conventional methods, such as at room temperature. Similarly, this invention does not impose a particular limitation on the impregnation time, as long as the required amount of active metal component and modifying agent is loaded onto the carrier. Once the required impregnation amount and conditions are determined, a suitable impregnation time can be easily selected. This invention does not impose a particular limitation on the impregnation environment; it can be carried out under sealed conditions or in an open environment using conventional methods in the art.
[0080] According to the present invention, preferably, the impregnation solution further contains additives, the additives including a first additive and a second additive, wherein the first additive is P123, and the second additive is selected from at least one of glycine, ethylene glycol, citric acid, and urea. This preferred embodiment is beneficial for improving the dispersion of the active metal component in the catalyst.
[0081] According to the present invention, preferably, the mass ratio of the second additive to the carrier is 0.1-1:1, more preferably 0.1-0.8:1.
[0082] According to the present invention, preferably, the mass ratio of the first additive to the second additive is 1:200-1000, more preferably 1:300-800.
[0083] The present invention has a wide range of choices for the types of modifying agents. Preferably, the modifying agent is selected from at least one of yttrium, lanthanum, cerium, zirconium, titanium and vanadium, and more preferably from at least one of yttrium, lanthanum and cerium.
[0084] The present invention does not have any particular limitation on the types of active metal component compounds and modifying agent compounds, as long as they contain active metals and modifying agents.
[0085] The present invention does not particularly limit the solvent in the impregnation solution, and any conventional choice in the art can be used. In an exemplary embodiment of the present invention, water is used as the solvent.
[0086] The present invention does not have any particular limitation on the second drying step (3), and it can be carried out with reference to conventional methods in the art. Preferably, the second drying step (3) is vacuum drying.
[0087] Preferably, the conditions for the second calcination in step (3) include: a temperature of 500-1000℃ and a time of 2-10h.
[0088] In this invention, the terms "first" and "second" do not limit the substances and operations, but are only used to distinguish the substances introduced in different steps and the operations performed in different stages.
[0089] The third aspect of this invention provides the application of the nickel-based catalyst described in the first aspect or the nickel-based catalyst prepared by the preparation method described in the second aspect in the methanation reaction of crude hydrogen purification, preferably in the application of the methanation reaction of crude hydrogen purification at ultra-low temperature.
[0090] When the catalyst provided by this invention is applied to the ultra-low temperature methanation reaction for crude hydrogen purification, it has the advantages of high activity, high methane selectivity, and good thermal stability, and can fully meet the requirements of downstream processes for hydrogen quality.
[0091] Preferably, the crude hydrogen contains 2000-10000 ppm of carbon monoxide.
[0092] The catalyst provided by this invention can significantly reduce the temperature of the methanation reaction, thereby greatly saving the amount of high-pressure steam used, improving the safety factor of operation, reducing equipment requirements, and achieving significant energy saving and emission reduction effects. Preferably, the temperature of the ultra-low temperature methanation reaction is below 200℃, and more preferably 150-180℃.
[0093] Preferably, the conditions for the ultra-low temperature methanation reaction include: a reaction temperature of 150-180℃; a pressure of 0-6 MPa; and a volume hourly space velocity (VHSV) of 1000-12000 h⁻¹. -1 .
[0094] The present invention will be described in detail below through embodiments.
[0095] In the following examples, the components of the catalyst were measured by XRF;
[0096] P123 is a commercially available product from Beijing Innocare Technology Co., Ltd., under the brand name A13917.
[0097] Example 1
[0098] (1) Preparation of catalyst support
[0099] 699 g of aluminum nitrate nonahydrate and 31.8 g of magnesium nitrate hexahydrate were dissolved in 1000 ml of deionized water and heated to 70 °C. 3000 ml of ethanol was added and stirring continued for 5 min. A mixture of 52.7 g of formamide and 831.1 g of propylene oxide was added, and the mixture was stirred at 70 °C for another 30 min to obtain a gel. The resulting gel was washed with ethanol and then placed in a supercritical fluid reactor. CO2 gas was introduced for purging, followed by pressurization to 4.5 MPa. The temperature was then increased to 260 °C and maintained at 8 MPa for 2 h to obtain the magnesium-aluminum aerogel precursor.
[0100] 100g of magnesium-aluminum aerogel precursor, 3g of guar gum powder, and 2g of methylcellulose were uniformly mixed. Then, 1.2g of nitric acid (commercially available, 65wt%) and 60g of deionized water were added sequentially, and the mixture was stirred to obtain a final mixture. This mixture was then kneaded on a kneader and extruded into 1.4mm butterfly strips on a screw extruder at an extrusion temperature of 65℃ and an extrusion pressure of 350Kgf (strength). The butterfly strips were dried in an oven at 120℃ for 2 hours and calcined at 500℃ for 4 hours to obtain a carrier with a specific surface area of 204m². 2 / g.
[0101] (2) Preparation of catalyst
[0102] Take 20g of the above-mentioned support, weigh out 13g of nickel nitrate hexahydrate, 1.62g of yttrium nitrate hexahydrate, 7.6g of ethylene glycol, and 0.015g of P123, dissolve them in 16mL of deionized water, soak them for 20min using the excess impregnation method, then dry them at 45℃ and 0.1MPa vacuum for 2h, and calcine them at 500℃ for 4h to obtain the nickel-based catalyst. The composition and characteristics of the catalyst are shown in Table 1.
[0103] The H2-TPR spectra of the catalysts prepared in Example 1 and Comparative Example 1 of the present invention are shown in Figure 1. As can be seen from Figure 1, the reduction peak in the spectrum of the catalyst prepared in Example 1 is high, with the highest peak corresponding to a temperature of approximately 350°C. In contrast, the reduction peak in the spectrum of the catalyst prepared in Comparative Example 1 is wide, with the highest peak corresponding to a temperature of approximately 530°C. This indicates that the active phase of the catalysts in the examples has a high degree of low-temperature reduction, and compared to Comparative Example 1, the interaction between the active phase and the support is more uniform and the dispersion is better.
[0104] Example 2
[0105] (1) Preparation of catalyst support
[0106] 699 g of aluminum nitrate nonahydrate and 80.6 g of magnesium nitrate hexahydrate were dissolved in 1000 ml of deionized water by stirring. The solution was heated to 70 °C, and 3000 ml of ethanol was added. The mixture was stirred for 5 min. Then, a mixture of 89.3 g of formamide and 831.1 g of propylene oxide was added, and the solution was stirred for 30 min while maintaining the temperature at 70 °C to obtain a gel. The resulting gel was washed with ethanol and then placed in a supercritical fluid reactor. CO2 gas was introduced for purging, and the pressure was increased to 4.5 MPa. The solution was stirred and heated to 280 °C, and the pressure was maintained at 9 MPa for 2 h to obtain the magnesium-aluminum aerogel precursor.
[0107] 100g of magnesium-aluminum aerogel precursor, 3g of guar gum powder, and 2g of methylcellulose were uniformly mixed. Then, 1.2g of nitric acid (commercially available, 65wt%) and 60g of deionized water were added sequentially, and the mixture was stirred to obtain a final mixture. This mixture was then kneaded on a kneader and extruded into 1.4mm butterfly strips on a screw extruder at an extrusion temperature of 65℃ and an extrusion pressure of 350Kgf (strength). The butterfly strips were dried in an oven at 120℃ for 2 hours and calcined at 500℃ for 4 hours to obtain a carrier with a specific surface area of 223m². 2 / g.
[0108] (2) Preparation of catalyst
[0109] Take 20g of the above-mentioned support, weigh out 13g of nickel nitrate hexahydrate, 1.21g of yttrium nitrate hexahydrate, 11g of glycine, and 0.015g of P123, dissolve them in 16mL of deionized water, soak them for 20min using the excess impregnation method, then dry them at 45℃ and 0.1MPa vacuum for 2h, and calcine them at 500℃ for 4h to obtain the nickel-based catalyst. The composition and characteristics of the catalyst are shown in Table 1.
[0110] Example 3
[0111] 699 g of aluminum nitrate nonahydrate and 31.8 g of magnesium nitrate hexahydrate were dissolved in 1000 ml of deionized water and heated to 70 °C. 3000 ml of ethanol was added and stirring continued for 5 min. A mixture of 52.7 g of formamide and 831.1 g of propylene oxide was added, and the mixture was stirred at 70 °C for another 30 min to obtain a gel. The resulting gel was washed with ethanol and then placed in a supercritical fluid reactor. CO2 gas was introduced for purging, followed by pressurization to 4.5 MPa. The temperature was then increased to 260 °C and maintained at 8 MPa for 2 h to obtain the magnesium-aluminum aerogel precursor.
[0112] 100g of magnesium-aluminum aerogel precursor, 3g of guar gum powder, and 2g of methylcellulose were uniformly mixed. Then, 1.2g of nitric acid (commercially available, 65wt%) and 60g of deionized water were added sequentially, and the mixture was stirred to obtain a final mixture. This mixture was then kneaded on a kneader and extruded into 1.4mm butterfly strips on a screw extruder at an extrusion temperature of 65℃ and an extrusion pressure of 350Kgf (strength). The butterfly strips were dried in an oven at 120℃ for 2 hours and calcined at 500℃ for 4 hours to obtain a carrier with a specific surface area of 204m². 2 / g.
[0113] (2) Preparation of catalyst
[0114] Take 20g of the above-mentioned support, weigh out 16.7g of nickel nitrate hexahydrate, 1.31g of lanthanum nitrate hexahydrate, 5.8g of urea, and 0.015g of P123, dissolve them in 16mL of deionized water, soak them for 20min using the excess impregnation method, then dry them at 45℃ and 0.1MPa vacuum for 2h, and calcine them at 500℃ for 4h to obtain the nickel-based catalyst. The composition and characteristics of the catalyst are shown in Table 1.
[0115] Example 4
[0116] The method described in Example 3 was followed, except that urea was not added during catalyst preparation. The catalyst composition and characteristics are shown in Table 1.
[0117] Comparative Example 1
[0118] Al2O3 spheres (specific surface area 120m²) 2 / g, pore volume 0.3cm 3 The support was obtained by drying (g). Then, 20g of the support was taken, and 13g of nickel nitrate hexahydrate was weighed and dissolved in 16mL of deionized water. The solution was soaked for 20min using the excess impregnation method, and then dried at 45℃ and 0.1MPa vacuum for 2h. Finally, it was calcined at 500℃ for 4h to obtain the nickel-based catalyst. The composition and characteristics of the catalyst are shown in Table 1.
[0119] Comparative Example 2
[0120] The preparation of the catalyst support was the same as in Example 1.
[0121] Take 20g of the above-mentioned support, weigh 13g of nickel nitrate hexahydrate and dissolve it in 16mL of deionized water. Soak the solution for 20min using the excess impregnation method, then dry it at 45℃ and 0.1MPa vacuum for 2h, and calcine it at 500℃ for 4h to obtain the nickel-based catalyst. The composition and characteristics of the catalyst are shown in Table 1.
[0122] Comparative Example 3
[0123] The Al2O3-MgO complex (specific surface area 135m²) 2 / g, pore volume 0.29cm 3 The nickel-based catalyst was prepared by drying a mixture of nickel nitrate (g / g) and magnesium oxide (5wt%). Then, 20g of the above support was taken, and 13g of nickel nitrate hexahydrate, 1.62g of yttrium nitrate hexahydrate, 11g of glycine, and 0.015g of P123 were weighed and dissolved in 16mL of deionized water. The solution was then impregnated for 20min using an excess impregnation method, dried at 45℃ and 0.1MPa vacuum for 2h, and calcined at 500℃ for 4h. The composition and characteristics of the catalyst are shown in Table 1.
[0124] Table 1
[0125]
[0126]
[0127] Note: A refers to the temperature corresponding to the highest peak in the H2-TPR spectrum of the catalyst, as characterized by H2-TPR.
[0128] As can be seen from the results in Table 1, the active metal component in the catalyst of the present invention has better dispersibility, larger specific surface area and higher crushing strength, indicating that the catalyst of the present invention has higher catalytic activity and longer service life.
[0129] Test Example 1
[0130] 1g of the catalyst prepared in the examples and comparative examples was weighed and packed into a fixed-bed reactor. The catalyst prepared in Example 2 was reduced at 300°C for 3 hours under normal pressure in a pure hydrogen atmosphere. The catalyst prepared in Comparative Example 1 was reduced at 350°C for 4 hours in a pure hydrogen atmosphere, and the catalyst prepared in Comparative Example 3 was reduced at 450°C for 4 hours in a pure hydrogen atmosphere.
[0131] After reduction, the temperature was lowered to 150°C under a hydrogen atmosphere, and the crude hydrogen feed gas (H2 with a CO concentration of 5000 ppm) was switched to react at 150°C with a reaction volume hourly space velocity of 10000 h⁻¹. -1 The reaction pressure was 2 MPa. After 8 hours of reaction, the tail gas composition was analyzed by online gas chromatography. The CO concentration in the tail gas is shown in Table 2.
[0132] Table 2
[0133] Example No. CO concentration in exhaust gas, ppm Example 1: Below 1 ppm, not detected Example 2 3 Example 3 2 Example 4 3 8 Comparative Example 1 1 3 5 6 Comparative Example 2 3 2 2 Comparative Example 3 1 2 3 1 surface
[0134] As can be seen from the results in Table 2, the catalyst provided by this invention exhibits significantly better reaction activity when applied to the ultra-low temperature methanation reaction for crude hydrogen purification.
[0135] The test examples described in this invention are used to illustrate the stability of the catalyst of this invention.
[0136] Test Example 2
[0137] 1 g of the catalyst prepared in Example 1 was weighed and packed into a fixed-bed reactor. Activation was performed by reduction at 300°C for 3 hours under a pure hydrogen atmosphere at atmospheric pressure. After reduction, the temperature was lowered to 150°C under a hydrogen atmosphere, and the crude hydrogen feed gas (H2 with a CO concentration of 5000 ppm) was switched to react at 150°C with a reaction space velocity of 10000 h⁻¹. -1 The reaction pressure was 2 MPa. After 1000 h of reaction, the tail gas composition was analyzed by online gas chromatography, and the results are shown in Figure 2.
[0138] As shown in Figure 2, the CO conversion rate was 99.9% and the methane selectivity was 99.2% after 100 h of reaction; the CO conversion rate was 99.0% and the methane selectivity was 98.8% after 500 h of reaction; and the CO conversion rate was 96.4% and the methane selectivity was 99.2% after 1000 h of reaction. The CO conversion rate and methane selectivity did not decrease significantly, indicating that the catalyst provided by this invention has high stability.
[0139] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A nickel-based catalyst, characterized in that, The catalyst comprises a magnesium-aluminum aerogel support, an active metal component, and a modifying agent; the active metal component is nickel; the modifying agent is selected from at least one of Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB, and Group VIII metal elements; wherein the dispersion of the active metal component is not less than 10%.
2. The catalyst according to claim 1, wherein, The dispersion of the active metal component is 11-20%; preferably, the average particle size of the active metal component is not greater than 10 nm, more preferably 1-9 nm; preferably, the specific surface area of the active metal component is not less than 7 m². 2 / g cat Preferably 7-15m 2 / g cat ; and / or, the specific surface area of the active metal component is not less than 60 m². 2 / g Ni Preferably 65-100m 2 / g Ni .
3. The catalyst according to claim 1 or 2, wherein, H2-TPR characterization shows that the temperature corresponding to the highest peak in the H2-TPR spectrum of the catalyst is between 200-450℃, preferably between 250-350℃; preferably, the catalyst has a breakage strength of 400 N / cm or higher, preferably 400-600 N / cm; preferably, based on the total mass of the catalyst, the mass content of the magnesium-aluminum aerogel support is 70-94%, preferably 79-89%; the mass content of the active metal component, calculated as oxides, is 5-25%, preferably 10-20%; the mass content of the modifying agent, calculated as oxides, is 0.5-5%, preferably 1-5%; preferably, the modifying agent is selected from at least one of yttrium, lanthanum, cerium, zirconium, titanium, and vanadium.
4. The catalyst according to any one of claims 1-3, wherein, In the magnesium-aluminum aerogel carrier, the mass ratio of magnesium to aluminum, calculated as oxides, is 2-10:90-98; preferably, the specific surface area of the magnesium-aluminum aerogel carrier is 200-400 m². 2 / g, preferably 200-300m 2 / g.
5. A method for preparing a nickel-based catalyst, characterized in that, The preparation method includes the following steps: (1) gelling aluminum salt, magnesium salt, expanding agent and solvent, and then supercritical drying to obtain magnesium-aluminum aerogel precursor; (2) mixing the magnesium-aluminum aerogel precursor and extrusion aid to form a mold, and then performing a first drying and a first calcination to obtain magnesium-aluminum aerogel carrier; (3) introducing an active metal component and a modifying agent onto the magnesium-aluminum aerogel carrier by impregnation; wherein the active metal component is nickel; and the modifying agent is selected from at least one of Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB and Group VIII metal elements.
6. The method according to claim 5, wherein, The mass ratio of magnesium salt to aluminum salt, calculated as oxides, is 2-10:90-98; preferably, the expanding agent is propylene oxide and formamide; preferably, the mass ratio of the expanding agent to aluminum salt is 0.5-5:1, more preferably 1-2:1; preferably, the mass ratio of propylene oxide to formamide is 5-30:1, more preferably 10-20:
1.
7. The method according to claim 5 or 6, wherein, The gelation conditions in step (1) include: a temperature of 40-70℃ and a time of 0.5-3h; preferably, the supercritical drying in step (1) is supercritical carbon dioxide drying; preferably, the conditions for supercritical carbon dioxide drying include: a pressure of 6-22MPa, preferably 8-12MPa; a temperature of 240-450℃, preferably 250-300℃; and a drying time of 0.5-8h, preferably 1-4h.
8. The method according to any one of claims 5-7, wherein, The specific surface area of the magnesium-aluminum aerogel carrier obtained in step (2) is 200-400 m². 2 / g, preferably 200-300m 2 / g; Preferably, the amount of active metal component and modified additive introduced in step (3) is such that, based on the total mass of the catalyst, the mass content of the magnesium aluminum aerogel support is 70-94%, preferably 79-89%; The active metal component, calculated as oxide, has a mass content of 5-25%, preferably 10-20%; the modifying agent, calculated as oxide, has a mass content of 0.5-5%, preferably 1-5%.
9. The method according to any one of claims 5-8, wherein, Step (3) of the impregnation method includes: contacting an impregnation solution containing an active metal component compound and a modifying agent compound with a magnesium-aluminum aerogel carrier, followed by a second drying and a second calcination; preferably, the impregnation solution also contains additives, the additives including a first additive and a second additive, the first additive being P123, and the second additive being selected from at least one of glycine, ethylene glycol, citric acid, and urea; preferably, the mass ratio of the second additive to the carrier is 0.1-1:1, more preferably 0.1-0.8:1; preferably, the mass ratio of the first additive to the second additive is 1:200-1000, more preferably 1:300-800; preferably, the modifying agent is selected from at least one of yttrium, lanthanum, cerium, zirconium, titanium, and vanadium.
10. The application of a nickel-based catalyst according to any one of claims 1-4 or a nickel-based catalyst prepared by any one of claims 5-9 in a crude hydrogen purification methanation reaction, preferably in a crude hydrogen purification ultra-low temperature methanation reaction; preferably, the crude hydrogen contains 2000-10000 ppm of carbon monoxide; preferably, the ultra-low temperature methanation reaction temperature is below 200°C, preferably 150-180°C.