Foam concrete based on acidic iron tailing sand and preparation method thereof
By constructing a multi-layered spatial network structure using a polymer-coated aluminosilicate fiber and carbon nanotube reinforced fiber composite system and S95 grade slag micro powder, the stability and strength issues of acidic iron tailings sand in roadbed materials were solved, realizing the safe resource utilization of acidic solid waste and the preparation of high-performance roadbed materials.
Patent Information
- Application Number
- CN202511916402.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-18
- Publication Date
- 2026-05-01
AI Technical Summary
Existing traditional fillers and lightweight materials have significant shortcomings in terms of resources, environment, mechanical properties and economy, making it difficult to meet the needs of modern transportation infrastructure for high-performance and low-environmental-impact roadbed materials. Furthermore, the acidic components of acidic iron tailings sand cause damage to the cementitious structure, limiting its resource utilization.
A composite reinforcement system consisting of polymer-coated aluminosilicate fibers and carbon nanotube-reinforced polypropylene fibers, combined with S95 grade slag powder and a composite acid-resistant foaming agent, was used to construct a multi-layered spatial network structure, forming a highly viscoelastic liquid film that neutralizes the acidic environment and generates CSH gel. A compressive strength prediction model was then established.
It significantly improves the long-term stability and acid resistance of foamed concrete, increases the strength retention rate, solves the problem of formwork collapse caused by acidic aggregates, and realizes the safe resource utilization of acidic solid waste.
Smart Images

Figure CN121948917A_ABST
Abstract
Description
A foamed concrete based on acidic iron tailings sand and its preparation method Technical Field
[0001] This invention relates to the field of solid waste material resource utilization technology, and in particular to a foamed concrete based on acidic iron tailings sand and its preparation method. Background Technology
[0002] In road engineering, foundation backfilling, and building construction, the selection of subgrade fillers and lightweight materials directly affects the stability, durability, and economic and environmental benefits of engineering structures. For a long time, the engineering industry has widely relied on natural sand and gravel as the primary filler. However, these materials face the dual pressures of resource depletion and ecological damage. Large-scale extraction not only consumes non-renewable natural resources but also causes irreversible damage to mountains, rivers, and the surrounding ecological environment. To improve strength, cement-stabilized crushed stone and other cementing materials have been used, but their inherent high weight significantly increases the foundation load, easily leading to uneven settlement on soft soil foundations. Simultaneously, the drying shrinkage and temperature shrinkage stresses generated during the hardening process of these materials can easily cause structural cracking, affecting the long-term integrity and performance of the subgrade. To overcome the weight problem, organic lightweight fillers such as polystyrene foam have been introduced, but their high material cost significantly increases the project budget, and their low compressive and shear strength makes them prone to plastic deformation and load-bearing failure under repeated heavy traffic, greatly limiting their application. In summary, existing traditional fillers and lightweight materials have significant shortcomings in terms of resources, environment, mechanical properties, and economy, making it difficult to meet the urgent needs of modern transportation infrastructure for high-performance, low-environmental-impact roadbed materials.
[0003] On the other hand, as a major steel producer, my country generates massive amounts of iron tailings solid waste during iron ore beneficiation, causing serious problems of stockpiling and environmental pollution. Among these, acidic iron tailings, containing sulfides such as pyrite, continuously generate sulfuric acid under open-air storage conditions through oxidation by air, rainwater, and microorganisms. This highly acidic environment not only activates heavy metals and pollutes surrounding soil and water bodies but also presents significant technical bottlenecks in its resource utilization. Although some studies have attempted to incorporate neutral or alkaline tailings as aggregates into concrete or roadbed materials, the acidic components and sulfate ions in acidic iron tailings severely erode the hydration products of ordinary silicate cement, leading to structural damage, strength degradation, and potential sulfate erosion and expansion, greatly limiting its large-scale, high-value-added utilization. Conventional pretreatment neutralization methods, while able to raise the pH value, are often costly, complex, and difficult to completely eliminate long-term stability risks. Therefore, how to safely, efficiently, and on a large scale dispose of acidic iron tailings solid waste, and how to develop a new type of building material that is compatible with its acidic properties and meets the requirements of engineering mechanical properties and durability, has become a technical problem that urgently needs to be solved in the fields of solid waste resource utilization and civil engineering materials. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a foamed concrete based on acidic iron tailings sand and its preparation method, which significantly improves the long-term stability and acid resistance of foamed concrete. At the same time, by utilizing the acid resistance and high-temperature resistance of polymer-coated aluminosilicate fibers, the overall performance of foamed concrete is significantly improved.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] A foamed concrete based on acidic iron tailings sand comprises the following components by weight: 200-500 parts cement, 100-400 parts acidic iron tailings sand, 50-150 parts slag powder, 15-25 parts composite acid-resistant foaming agent solution, 1-10 parts composite fiber, and 200-300 parts water; wherein the composite acid-resistant foaming agent solution is prepared by mixing a composite acid-resistant foaming agent with water, and the composite fiber comprises a combination of organic reinforcing fiber and inorganic modified fiber.
[0007] Preferably, the aforementioned cement is one or a mixture of two of ordinary silicate cement and sulfoaluminate cement; when the cement is a mixture of two, the mass ratio of ordinary silicate cement to sulfoaluminate cement is 7:3-6:4.
[0008] Preferably, the aforementioned acidic iron tailings sand has a pH value of 3-5, a fineness modulus of 0.5-1.2, and a particle size of less than 0.75 mm; the acidic iron tailings sand includes the following components: 30%-35% hematite, 5%-10% magnetite, 3%-8% pyrite, 30%-40% quartz, and 10%-15% kaolin.
[0009] Preferably, the aforementioned slag powder is S95 grade slag powder, comprising 35%-45% CaO and 28%-35% SiO2, and the mass ratio of slag powder to cement is 1:4-3:8.
[0010] Preferably, the aforementioned composite acid-resistant foaming agent comprises a polyvinyl alcohol modified surfactant, modified nano-silica, and an organosilicon modifier in a mass ratio of 60-80:10-20:5-15; the foam has a water bleeding rate of ≤15 mL / h at pH 3.
[0011] Preferably, the aforementioned polyvinyl alcohol modified surfactant is prepared from polyvinyl alcohol and sodium dodecyl sulfate in a mass ratio of 1:1 to 1:2; the modified nano silica is prepared from a silane coupling agent and nano silica, wherein the amount of silane coupling agent is 5%-10% of the mass of nano silica; and the organosilicon modifier is a polyether modified organosilicon.
[0012] Preferably, the mass ratio of the aforementioned carbon nanotube-reinforced polypropylene fiber and polymer-coated aluminosilicate fiber is 1:1 to 2:1; the carbon nanotube-reinforced polypropylene fiber is obtained by combining carbon nanotubes with polypropylene fiber through surface grafting or impregnation; the polymer-coated aluminosilicate fiber is prepared by coating the surface of aluminosilicate fiber with polyurea or polyurethane coating.
[0013] Preferably, the contact angle of the aforementioned carbon nanotube-reinforced polypropylene fiber is ≥120°.
[0014] The method for preparing foamed concrete based on acidic iron tailings sand includes the following steps:
[0015] S1. Add cement, acidic iron tailings sand, slag powder and composite fiber to a mixer and dry mix. Slowly add water and continue mixing to make a uniform cement slurry.
[0016] S2. Prepare a foaming liquid by mixing a composite acid-resistant foaming agent with water to obtain stable foam;
[0017] S3. Add the stabilized foam to the cement slurry and stir to obtain foamed concrete slurry;
[0018] S4. Pour the slurry into the mold, let it stand and then demold to obtain foamed concrete.
[0019] Preferably, in step S2, the mass ratio of the composite acid-resistant foaming agent to water is 1:30-40, the foaming pressure is 0.3-0.5 MPa, and the foaming ratio is 35-45 times.
[0020] The 28-day compressive strength of the prepared foamed concrete was predicted and calculated using the following formula:
[0021]
[0022] in, Predicted 28-day compressive strength of foamed concrete; : Reference strength; Dosage of acidic iron tailings sand; Dosage of slag powder; : Parameters to be fitted; : Parameters to be fitted.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0024] (1) The present invention constructs a ternary stable foam system composed of polyvinyl alcohol-surfactant complex, nano silica and organosilicon. By utilizing the Pickering effect of nanoparticles and the low surface energy characteristics of organosilicon, a highly viscoelastic and acid-resistant pseudo-solid liquid film is formed at the gas-liquid interface, which enables the foam to maintain an independent spherical structure in acidic slurry, significantly reducing the amount of bleeding and solving the problem of mold collapse caused by acidic aggregates.
[0025] (2) The present invention adopts a composite reinforcement system of carbon nanotube reinforced polypropylene fiber and polymer coated aluminosilicate fiber to construct a multi-layer spatial grid structure. The superhydrophobic effect of CNT blocks the permeation path of acidic pore water, while the polymer coating layer solves the problem of interface corrosion of inorganic fibers in acidic matrix. The two work together to increase the strength retention rate of concrete in long-term acidic erosion environment to more than 90%.
[0026] (3) This invention utilizes the activation characteristics of S95 grade slag powder in an acidic environment to enable it to undergo an in-situ neutralization reaction with residual acidic substances in the tailings. The generated CSH gel not only encapsulates the tailings particles but also chemically fixes free sulfate ions, effectively suppressing the risk of volume expansion and cracking caused by delayed formation of ettringite, and realizing the safe resource utilization of acidic solid waste.
[0027] (4) The present invention establishes a set of compressive strength prediction models that include the competitive mechanism of acid damage and alkaline repair. These models can be directly embedded into the automatic control system of the mixing plant. When the acidity of the raw materials fluctuates or the supply changes, the slag content can be dynamically adjusted according to this model to ensure the stability of the final product quality. Attached Figure Description
[0028] Figure 1 is a flowchart of the preparation process of foamed concrete from acidic iron tailings sand of the present invention.
[0029] Figure 2 is a flowability diagram of the foamed concrete of iron tailings sand of the present invention. Detailed Implementation
[0030] To clearly illustrate the technical features of this solution, the following detailed implementation method will be used to describe the solution.
[0031] A foamed concrete based on acidic iron tailings sand comprises the following components by weight: 200-500 parts cement, 100-400 parts acidic iron tailings sand, 50-150 parts slag powder, 15-25 parts foam, 1-10 parts composite fiber, and 200-300 parts water. The cement is one or a mixture of ordinary Portland cement and sulfoaluminate cement; when the cement is a mixture of two, the mass ratio of ordinary Portland cement to sulfoaluminate cement is 7:3-6:4. This invention utilizes its hydration reaction to increase the bond strength of the foamed concrete, and simultaneously utilizes its alkalinity to increase the acid resistance of the foamed concrete.
[0032] The pretreated acidic iron tailings sand has a pH of 3-5, a fineness modulus of 0.5-1.2, and a particle size of less than 0.75 mm. The acidic iron tailings sand comprises the following components: 30%-35% hematite, 5%-10% magnetite, 3%-8% pyrite, 30%-40% quartz, and 10%-15% kaolin. This invention allows for an iron tailings sand content of 35%-45% through pretreatment. The slag powder is S95 grade slag powder, comprising 35%-45% CaO and 28%-35% SiO2. The mass ratio of slag powder to cement is 1:4-3:8. The slag powder activity index is ≥75% at 7 days and ≥95% at 28 days, and hydration generates CSH gel to continuously neutralize residual acidic substances.
[0033] The foam is prepared by mixing a composite acid-resistant foaming agent and water at a mass ratio of 1:30-40. The composite acid-resistant foaming agent includes a polyvinyl alcohol modified surfactant, modified nano-silica, and an organosilicon modifier, with a mass ratio of 60-80:10-20:5-15. The specific preparation method is as follows: The polyvinyl alcohol modified surfactant powder, modified nano-silica powder, and organosilicon modifier are mixed and stirred in a mixer at 500-600 rpm for 30 minutes to ensure uniform dispersion, thus obtaining the composite acid-resistant foaming agent. In use, the composite acid-resistant foaming agent is mixed with water at a mass ratio of 1:30-40 to prepare the foaming liquid.
[0034] The specific substances used in the polyvinyl alcohol-modified surfactant are polyvinyl alcohol (PVA-1788, degree of hydrolysis 87%-89%) and the anionic surfactant sodium dodecyl sulfate (SDS). Polyvinyl alcohol is dissolved in hot water at 80-90 °C to prepare a 5-10 wt% polyvinyl alcohol solution. Then, sodium dodecyl sulfate is added, with a mass ratio of polyvinyl alcohol to sodium dodecyl sulfate of 1:1-1:2. The reaction is carried out with continuous stirring at 70-80 °C for 2-3 hours, allowing polyvinyl alcohol and the surfactant to form a complex through hydrogen bonding and hydrophobic interactions. After the reaction is complete, the mixture is cooled to room temperature and spray-dried to obtain a polyvinyl alcohol-modified surfactant powder.
[0035] The specific materials of the nano-silica are nano-silica (particle size 10-20 nm) and a silane coupling agent (KH-550, γ-aminopropyltriethoxysilane). The nano-silica is dispersed in anhydrous ethanol (solid-liquid ratio 1:10) and ultrasonically treated for 30 minutes to ensure uniform dispersion. Then, the silane coupling agent is added, with the amount of silane coupling agent being 5%-10% of the mass of the nano-silica. The reaction is stirred at 60 °C for 4 hours to allow the silane coupling agent to hydrolyze and graft onto the surface of the nano-silica. After the reaction is complete, the modified nano-silica powder is obtained by centrifugation, washing three times with ethanol, and vacuum drying at 80 °C for 6 hours.
[0036] The specific substance of the organosilicon modifier is polyether-modified organosilicon, which has the functions of reducing surface tension and enhancing water resistance.
[0037] Polyvinyl alcohol-modified surfactants improve foam stability, especially its durability in acidic environments; nano-silica enhances the mechanical strength and durability of the foam film; and organosilicon modifiers strengthen the water resistance and aging resistance of the foam film. This composite foaming agent system, through the reinforcing effect of polyvinyl alcohol, the strengthening effect of nano-silica, and the surface treatment with organosilicon modifiers, achieves a water loss of ≤15 mL per hour at pH=3, significantly improving the acid resistance and long-term stability of foamed concrete.
[0038] The composite fiber comprises carbon nanotube-reinforced polypropylene fibers and polymer-coated aluminosilicate fibers in a mass ratio of 1:1 to 2:1. The carbon nanotube-reinforced polypropylene fibers are obtained by combining carbon nanotubes with polypropylene fibers through surface grafting or impregnation; the polymer-coated aluminosilicate fibers are prepared by coating the surface of aluminosilicate fibers with polyurea or polyurethane. The combined effect of the carbon nanotube-reinforced polypropylene fibers and the polymer-coated aluminosilicate fibers enhances the corrosion resistance of foamed concrete in acidic environments, maintaining high strength even in environments with low pH values. The contact angle of the carbon nanotube-reinforced polypropylene fibers is ≥120°, and the strength loss after immersion in concentrated sulfuric acid for 7 days is ≤5%.
[0039] The preparation method of carbon nanotube-reinforced polypropylene fiber adopts an impregnation method. Specifically, carboxylated carbon nanotubes are first modified with a silane coupling agent KH-550, and then dispersed in water to prepare a 3 wt% dispersion. Polypropylene fiber bundles are impregnated in this dispersion, followed by drying at 100-130 °C and heat treatment at 130-140 °C for 1-5 minutes to ensure that the CNTs firmly adhere to the fiber surface. The resulting properties are: fiber contact angle ≥120°, and strength loss ≤5% after immersion in concentrated sulfuric acid for 7 days.
[0040] The polymer-coated aluminosilicate fibers were prepared using a dip-coating-curing method. Specifically, the aluminosilicate fibers were first pretreated with KH-550 for surface amination. Then, they were immersed in a polyurethane coating solution with a solid content of 20 wt%, pulled at a speed of 1-5 m / min, and finally cured at 100-120 °C for 1-1.5 h to form a dense coating layer. The resulting properties included a coating layer thickness of 1.5-2.5 μm and significantly improved acid resistance.
[0041] Example 1
[0042] The foamed concrete based on acidic iron tailings sand in this embodiment uses the following components by weight: 350 parts ordinary silicate cement, 100 parts slag powder, 200 parts acidic iron tailings sand, 4 parts carbon nanotube reinforced polypropylene fiber, 4 parts polymer-coated aluminosilicate fiber, 250 parts water, and 20 parts foam.
[0043] Weigh each component according to the above raw material ratio, and prepare it according to the following method:
[0044] S1. Weigh out 350 parts of ordinary silicate cement, 150 parts of slag powder, 200 parts of acidic iron tailings sand, 4 parts of carbon nanotube reinforced polypropylene fiber and 4 parts of polymer-coated aluminosilicate fiber by weight. Mix them thoroughly with a mixer. After 1 minute, add 250 parts of water and continue mixing for 3 minutes to make cement mortar.
[0045] S2. Mix the composite acid-resistant foaming agent and water at a ratio of 1:35 to prepare a foaming liquid. Use a foaming machine to foam the foam and weigh out 20 parts of the foam.
[0046] S3. Add the prepared foam to the cement slurry and stir for 5 minutes to obtain foamed concrete slurry.
[0047] S4. Pour the foamed concrete slurry into pre-oiled 100 mm × 100 mm × 100 mm triple molds, and cover the molds with a layer of plastic wrap to prevent moisture loss and collapse. Let stand for 24 hours before demolding. Acidic iron tailings sand foamed concrete modules are obtained.
[0048] Comparative Example 1
[0049] The specific difference between this comparative example and Example 1 is that no slag powder was added.
[0050] Comparative Example 2
[0051] The specific difference between this comparative example and Example 1 is that: no polymer-coated aluminum silicate fiber was added, and 8 parts of carbon nanotube-reinforced polypropylene fiber were added.
[0052] Comparative Example 3
[0053] The specific difference between this comparative example and Example 1 is that: no carbon nanotube-reinforced polypropylene fiber was added, and 8 parts of polymer-coated aluminum silicate fiber were added.
[0054] Comparative Example 4
[0055] The specific difference between this comparative example and Example 1 is that no slag powder and composite fiber were added.
[0056] Comparative Example 5
[0057] The specific difference between this comparative example and Example 1 is that a common animal protein foaming agent is used.
[0058] Performance testing
[0059] The fluidity, compressive strength, flexural strength, water absorption, splitting tensile strength, and number of freeze-thaw cycles of the concrete prepared in Example 1 and Comparative Examples 1-5 were tested according to the following national standards: fluidity (GB / T 2419), compressive and flexural strength (GB / T 17671, 100 mm³ specimen, loading rates of 2.4 kN / s and 50 N / s respectively), water absorption (JG / T266, soaked after drying to constant weight), splitting tensile strength (GB / T 50081), and number of freeze-thaw cycles (GB / T 50082 rapid freezing method, durability evaluated by mass loss rate and relative dynamic modulus of elasticity). The test results are shown in Table 1.
[0060] Table 1. Properties of the concrete prepared in Example 1 and Comparative Examples 1-5
[0061]
[0062] As can be seen from the data in Table 1, Example 1, while meeting the requirements for compressive strength, fluidity, and water absorption, exhibits higher splitting tensile strength compared to Comparative Examples 1-5. Furthermore, it demonstrates good experimental data in freeze-thaw cycle tests, showcasing certain advantages. It can utilize a large amount of different tailings solid waste materials, satisfying both strength and foundation bearing capacity requirements. This effectively solves the problems of large-scale utilization of solid waste tailings and the tendency of foamed lightweight concrete to crack, thus improving the performance of foamed lightweight concrete and facilitating its large-scale application.
[0063] Comparative Example 5 used the same components as Example 1, except that the composite acid-resistant foaming agent was replaced with a common foaming agent. The results showed that Comparative Example 5 experienced severe foam collapse due to foam instability in acidic slurry, making accurate flowability measurement impossible. Furthermore, its 28-day compressive strength, flexural strength, and water absorption were all at the same level as the baseline group (Comparative Example 4) without any reinforcement or slag treatment, with strength far lower than Example 1, and it exhibited the worst freeze-thaw performance. These data indicate that common foaming agents rapidly fail in acidic slurry, leading to complete destruction of the foam structure, increased slurry density, and thus the loss of the lightweight and porous characteristics expected of foamed concrete. The composite acid-resistant foaming agent of this invention successfully solves this problem by constructing a ternary foam-stabilizing system composed of polyvinyl alcohol-modified surfactant, nano-silica, and organosilicon modifier. The mechanism is as follows: First, nanoparticles form a physical barrier at the gas-liquid interface through the Pickering effect, significantly improving the mechanical strength of the foam film. Second, the synergistic effect of the polyvinyl alcohol-surfactant complex and organosilicon endows the gas-liquid interface with highly viscoelastic and acid-resistant pseudo-solid liquid film properties. This liquid film structure can resist the erosion of acidic mineral slurry, ensuring the independent spherical structure and volume stability of the foam during stirring and settling.
[0064] A comparison of data from Comparative Example 1 and Example 1 shows that the introduction of slag powder increased the 28-day compressive strength by approximately 19.5%. This strength increase is mainly attributed to the in-situ neutralization effect and secondary hydration effect of the slag. S95 grade slag powder itself contains active components such as CaO and SiO2. During slurry mixing, the slag undergoes an in-situ neutralization reaction with residual acidic substances in the tailings. This not only helps to increase the local pH value of the slurry and promote the hydration of ordinary Portland cement, but also activates the latent hydraulic properties of the slag itself. More importantly, the CSH gel generated by slag hydration encapsulates the acidic tailings sand particles and achieves the chemical fixation of free sulfate ions. Sulfate ions can trigger delayed ettringite formation, leading to volume expansion and structural cracking. By stabilizing and fixing sulfate ions in the early stages, the slag system fundamentally eliminates the potential threat to the long-term stability of materials posed by acidic iron tailings sand. In addition, the secondary hydration effect of slag fills the micropores in the cement stone, making the matrix structure of Example 1 more compact, thereby indirectly reducing the water absorption rate and ensuring its long-term stability and safety as a roadbed material.
[0065] (2) Acid resistance: To evaluate the long-term durability of foamed concrete under extreme acidic conditions, an accelerated acid etching test was conducted. The test method is as follows: 100 mm × 100 mm × 100 mm test blocks (Example 1, Comparative Examples 2-4) after standard curing for 28 days were immersed in a sulfuric acid solution with pH=2 (the ratio of solution volume to test block surface area was fixed at 10 mL / cm²). 2 (The solution was changed every 14 days to maintain a constant acidity). After soaking for 28 days, the specimens were removed, and their compressive and flexural strengths were measured. The strength retention rate relative to the water-soaked specimens of the same age was calculated. The specific results are shown in Table 2.
[0066] Table 2. Acid resistance of concrete prepared in Example 1 and Comparative Examples 1-4
[0067]
[0068] Table 2 shows that after immersion in a strong acid environment at pH=2 for 28 days, the compressive and flexural strength retention rates of Example 1 of the present invention (using the complete composite fiber system) both exceeded 90%, and the flexural strength was increased by about 60% compared with the baseline group (Comparative Example 4), far exceeding the expected 40%. In contrast, Comparative Examples 2 and 3, which lacked either component, showed a significant decrease in acid resistance, demonstrating that carbon nanotube-reinforced polypropylene fibers and polymer-coated aluminosilicate fibers play an indispensable synergistic reinforcing role in resisting acid corrosion and maintaining structural integrity.
[0069] This invention provides an in-depth analysis of the oxidation and acid production mechanism of acidic iron tailings and the acid-activated neutralization mechanism of slag powder, and also offers a predictive model for the compressive strength of foamed concrete after 28 days. In the porous structure of foamed concrete, air and pore water coexist, providing an ideal environment for the oxidation of pyrite. A unit mass of sulfur-containing tailings possesses enormous acid production potential throughout its entire life cycle. Acidic iron tailings sand dosage... The degree of chemical damage within the material is positively correlated. Since acid etching is a diffusion-reaction process, and the porosity of foamed concrete ensures sufficient oxidant, the effective damage can be approximated as being related to the degree of chemical damage within the material. It exhibits a linear or near-linear monotonically increasing relationship. The main components of slag powder (S95 grade) are CaO, SiO2, and Al2O3, possessing potential hydraulic properties. In ordinary concrete, strong alkali activation is required. However, in the acidic system of this invention, it exhibits a unique in-situ neutralization-repair mechanism.
[0070] Assuming the macroscopic pore distribution of foamed concrete is uniform, acid damage is statistically uniformly distributed. Assuming strength loss is primarily determined by long-term chemical corrosion accumulation, and that the 28-day strength already reflects the competition between early acid corrosion and neutralization. Based on composite mechanics and the Ryshkewitch-Duckworth theory, the strength of porous materials... Depends on its matrix strength and effective solid volume fraction (or porosity) ,in ).
[0071] For the foamed concrete of the present invention, its total porosity It consists of two parts: physical porosity ( ) and chemical evolution pores ( Physical porosity is the capillary porosity determined by the volume of bubbles introduced by the foaming agent and the water-cement ratio. Under the condition of a fixed water-cement ratio and foaming agent dosage, this part can be regarded as an initial constant or a baseline quantity that is finely adjusted with the total amount of dry material. Chemical evolution porosity is the increase in porosity caused by acid erosion and dissolution of the matrix, and the decrease in porosity caused by the filling of slag hydration products.
[0072] The baseline strength model can be written in exponential form:
[0073]
[0074] Breaking down porosity:
[0075]
[0076] make To determine the design strength without considering chemical damage (determined solely by the amount of foam), the model simplifies to:
[0077]
[0078] here, This represents cleanroom damage. If This indicates that acid etching leads to increased porosity and decreased strength; if (i.e., pore filling) will increase the strength.
[0079] According to kinetic analysis, the total amount of acid released is directly proportional to the sulfide content in the tailings. When the tailings source is consistent, the total amount of sulfides is directly proportional to the amount of tailings used. Acidic corrosion leading to matrix dissolution (CSH decalcification) increases porosity. According to stoichiometry, the volume of dissolved material is proportional to the amount of acid consumed. Therefore, potential chemical damage... and A linear relationship exists:
[0080]
[0081] in, This is the erosion sensitivity coefficient, which depends on the sulfur content of the tailings, particle size (specific surface area), and the acid resistance of the cement matrix. However, this only represents potential damage. The actual damage also depends on the presence of a neutralizing agent. In the absence of slag, .
[0082] Slag and cement hydration products are competing There is competition among ions. The introduction of slag significantly reduces the effective acid concentration. According to the Langmuir adsorption isotherm or the saturation attack model in multiphase reaction kinetics, the effect of the neutralizing agent is not infinitely linear. When the amount of slag... In small quantities, each additional bit of slag can efficiently neutralize free acid, resulting in extremely high marginal benefits. When the amount of slag... When the acidic substances are large enough, they are completely neutralized, and adding slag only serves as a physical filler, with its marginal contribution to resisting acid damage approaching zero. Therefore, a hyperbolic neutralization attenuation factor is used to describe this effect:
[0083]
[0084] in: This is a parameter for neutralization efficiency. When... hour, This indicates that the acid damage has completely acted on the matrix. When hour, This indicates that acid damage has been completely suppressed.
[0085] Combining the above two steps, the chemical damage is purified. It is the product of potential acidic damage and the neutralization attenuation factor. This reflects... and It is a strong coupling between them, rather than a simple linear superposition.
[0086]
[0087] Substitute this net damage into the exponential intensity model established in the first step:
[0088]
[0089]
[0090] Will Rename , as the first fitting parameter. It is considered as the baseline design strength under this mix proportion system, which can be obtained experimentally or treated as a known constant.
[0091] The final theoretical prediction model formula:
[0092]
[0093] in, : Predicted 28-day compressive strength of foamed concrete (MPa); Reference strength (MPa); : Amount of acidic iron tailings sand used (unit: parts or kg / m³). Dosage of slag powder (unit: parts or kg / m³) 3 ); (Parameter to be fitted 1): Acid etching sensitivity coefficient, The higher the value, the higher the sulfur content of the tailings, or the more easily the matrix is corroded by acid, and the faster the strength decreases with increasing tailings content. Unit: The reciprocal of the unit; (Parameter 2 to be fitted): Slag buffer efficiency factor, which characterizes the ability of a unit mass of slag to inhibit acid damage and the efficiency of microstructure repair. A higher value indicates higher activity and finer particle size of the slag, meaning a better acid resistance can be achieved with a smaller quantity. Unit: The reciprocal of the unit.
[0094] After fitting the running data, regression was performed. , The model predictions and experimental values were compared, and the results are shown in Table 3.
[0095] Table 3. Actual and model-predicted values of 28-day compressive strength of foamed concrete.
[0096]
[0097] As shown in Table 3, the model proposed in this invention can effectively determine the compressive strength of foamed concrete at 28 days, with a coefficient of determination R. 2 The value of 0.9995 indicates that the model has a high goodness of fit, good predictive consistency, and excellent capture of the strength evolution law in the acidic iron tailings foamed concrete system.
[0098] Based on the regression model This allows for deeper engineering analysis, which can then be used to guide actual production. At that point, the denominator is 1, and the acidic damage is completely released. hour( The denominator is approximately 2, and the damage index is halved. When... At that time, the denominator is approximately 3, and the damage index decreases to 1 / 3. When the concentration of slag increased from 85 to 170, although the amount of slag doubled, the effect of inhibiting damage only increased from 50% to 66.7%.
[0099] Therefore, in practical engineering, more slag is not necessarily better. According to the analysis of this model, the strength improvement efficiency per unit of slag is highest when the slag content is controlled between 80 and 120 parts. Beyond 150 parts, the strength gain slows down, and the demolding time may be affected due to the slow early hydration of the slag.
[0100] Assuming the engineering design requires a minimum 28-day compressive strength of 2.5 MPa for foamed concrete, we can deduce the maximum amount of tailings that can be absorbed under a specific slag dosage. .
[0101] Based on model transformation:
[0102]
[0103] set up ,slag :
[0104] Buffer factor: .
[0105] Intensity logarithmic decay: .
[0106] calculate :
[0107] .
[0108] This means that, with the addition of 100 parts of slag for protection, the system can theoretically accommodate up to 458 parts of acidic iron tailings sand while still meeting the strength requirement of 2.5 MPa.
[0109] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any way, and all technical solutions obtained by equivalent substitution or equivalent transformation fall within the protection scope of the present invention.
Claims
1. A foamed concrete based on acidic iron tailings sand, characterized in that, It comprises the following components by weight: 200-500 parts cement, 100-400 parts acidic iron tailings sand, 50-150 parts slag powder, 15-25 parts composite acid-resistant foaming agent solution, 1-10 parts composite fiber, and 200-300 parts water; wherein the composite acid-resistant foaming agent solution is prepared by mixing a composite acid-resistant foaming agent with water, and the composite fiber comprises a combination of organic reinforcing fiber and inorganic modified fiber.
2. The foamed concrete based on acidic iron tailings sand according to claim 1, characterized in that, The cement is one or a mixture of ordinary Portland cement and sulfoaluminate cement; when the cement is a mixture of two, the mass ratio of ordinary Portland cement to sulfoaluminate cement is 7:3-6:
4.
3. The foamed concrete based on acidic iron tailings sand according to claim 1, characterized in that, The pH value of the acidic iron tailings sand is 3-5.
4. The foamed concrete based on acidic iron tailings sand according to claim 1, characterized in that, The slag powder is S95 grade slag powder, comprising 35%-45% CaO and 28%-35% SiO2, and the mass ratio of slag powder to cement is 1:4-3:
8.
5. The foamed concrete based on acidic iron tailings sand according to claim 1, characterized in that, The composite acid-resistant foaming agent comprises polyvinyl alcohol modified surfactant, modified nano-silica, and organosilicon modifier in a mass ratio of 60-80:10-20:5-15.
6. The foamed concrete based on acidic iron tailings sand according to claim 5, characterized in that, The polyvinyl alcohol modified surfactant is prepared by polyvinyl alcohol and sodium dodecyl sulfate in a mass ratio of 1:1 to 1:2; the modified nano silica is prepared by silane coupling agent and nano silica, and the amount of silane coupling agent is 5%-10% of the mass of nano silica; the organosilicon modifier is polyether modified organosilicon.
7. The foamed concrete based on acidic iron tailings sand according to claim 1, characterized in that, The mass ratio of carbon nanotube-reinforced polypropylene fiber to polymer-coated aluminosilicate fiber is 1:1-2:1; the carbon nanotube-reinforced polypropylene fiber is obtained by combining carbon nanotubes with polypropylene fiber through surface grafting or impregnation; the polymer-coated aluminosilicate fiber is prepared by coating the surface of aluminosilicate fiber with polyurea or polyurethane coating.
8. The method for preparing foamed concrete based on acidic iron tailings sand according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Add cement, acidic iron tailings sand, slag powder and composite fiber to a mixer and dry mix. Slowly add water and continue mixing to make a uniform cement slurry. S2. Mix composite acid-resistant foaming agent and water to prepare foaming liquid to obtain stable foam. S3. Add stable foam to cement slurry and stir to obtain foamed concrete slurry. S4. Pour the slurry into a mold, let it stand and demold to obtain foamed concrete.
9. The preparation method according to claim 8, characterized in that, In step S2, the mass ratio of the composite acid-resistant foaming agent to water is 1:30-40, the foaming pressure is 0.3-0.5 MPa, and the foaming ratio is 35-45 times.
10. The preparation method according to claim 8, characterized in that, The 28-day compressive strength of the prepared foamed concrete was predicted and calculated using the following model: ;in, Predicted 28-day compressive strength of foamed concrete; : Reference strength; Dosage of acidic iron tailings sand; Dosage of slag powder; : Parameters to be fitted; : Parameters to be fitted.
Citation Information
Cited By
A lightweight concrete for mine filling and its preparation method
CN122127117A