Ultrahigh-strength Al-Mg-Si-Cu alloy and thermomechanical treatment method thereof

By using a deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloys to control the precipitation of alloying elements and the distribution of dislocations, the problem of insufficient strength and plasticity of existing 6xxx series aluminum alloys has been solved, realizing aluminum alloy sheets with high strength and good plasticity, which are suitable for lightweight design in the transportation field.

CN121951334APending Publication Date: 2026-05-01BAOSHAN IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411535944.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2026-05-01

AI Technical Summary

Technical Problem

The existing 6xxx series aluminum alloys have low yield strength and tensile strength in the peak-aged state, and the peak-aging treatment time is long, which makes it difficult to meet the lightweight design requirements of the future transportation sector.

Method used

Ultra-high strength Al-Mg-Si-Cu alloy and its deformation heat treatment method are adopted, including solution quenching, under-aging treatment, pre-deformation and aging treatment. By controlling the precipitation and dislocation distribution of alloying elements, the peak aging treatment time is shortened, thereby improving the strength and plasticity of the alloy.

Benefits of technology

The alloy has a yield strength ≥378MPa, tensile strength ≥415MPa, elongation ≥8.7%, and peak aging treatment time is shortened to 0.5-4h, which significantly improves production efficiency and alloy performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121951334A_ABST
    Figure CN121951334A_ABST
Patent Text Reader

Abstract

The invention discloses an ultrahigh-strength Al-Mg-Si-Cu alloy and a thermomechanical treatment method thereof. The alloy comprises the following components in percentage by mass: 1.2 to 2.0 percent of Mg, 1.0 to 1.5 percent of Si, 0.5 to 1.5 percent of Cu, 0.15 to 0.5 percent of Zn, 0.2 to 0.4 percent of Mn, 0.05 to 0.1 percent of Ti, 0 to 0.5 percent of Fe and the balance of Al and inevitable impurities. The density of a strengthening phase in the structure of the alloy is greater than or equal to 7.18 * 10 < 22 > / m < 3 >; the specific heat treatment comprises the following steps of (1) solid solution quenching, (2) under-aging treatment, (3) pre-deformation and (4) aging treatment, and based on the composite strengthening effect of precipitation strengthening and dislocation strengthening, the aluminum alloy plate obtains higher strength on the premise that good shaping is guaranteed; meanwhile, the time of peak aging heat treatment is shortened, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy technology, specifically relating to an ultra-high strength Al-Mg-Si-Cu alloy and its deformation heat treatment method. Background Technology

[0002] 6xxx series aluminum alloys are widely used in automotive body panels due to their excellent formability, good surface quality, corrosion resistance, and age-hardening properties. By increasing the alloy strength, the overall vehicle weight can be reduced while ensuring body strength and safety performance, thereby improving its power, handling performance, fuel consumption, and emissions of harmful gases.

[0003] Currently, typical commercial 6xxx series aluminum alloys are mainly AA6111, AA6016 and AA6022 alloys, whose yield strength at peak aging is only 290-300 MPa.

[0004] Enoch Advanz TM Taking 6HS s650 alloy (commercialized) as an example, by increasing the content of Mg and Si elements and adding some Cu elements, the yield strength of existing 6xxx series aluminum alloy plates under peak aging state was increased to 340MPa, the yield strength was increased to 400MPa, and the total elongation was 14%.

[0005] Chinese Patent Publication No. CN117535601A discloses a composite deformation heat treatment method for suppressing natural aging of automotive aluminum alloys and improving the response of artificial aging. This method suppresses the formation of room-temperature atomic clusters during natural aging and promotes the precipitation of strengthening phases during artificial aging, fully utilizing the dispersion strengthening effect to achieve a significant artificial aging response. The artificial aging response maintains a high level even after natural aging, especially with a significant increase in tensile strength, and exhibits excellent plasticity. Two pre-deformation processes are required to achieve the desired performance.

[0006] Chinese Patent Publication No. CN104060201A discloses a deformation heat treatment method that simultaneously improves the strength and intergranular corrosion resistance of 6000 series aluminum alloys. The aluminum alloy is subjected to solution treatment, quenching, direct or under-aging treatment, and then subjected to room temperature cold rolling deformation with a large reduction. The degree of hardening of the alloy after under-aging treatment is controlled to not exceed 95% of the peak aged hardness. The reduction (reduction rate) of room temperature cold rolling deformation is not less than 80%. No further treatment is required, and excellent alloy strength and intergranular corrosion resistance can be obtained at the same time.

[0007] Chinese patent publication number CN116623111A discloses a deformation heat treatment process for continuous cold rolling of ultra-high strength Al-Zn-Mg-Cu alloy. The process employs a deformation heat treatment method that combines high-temperature pre-aging, cold rolling deformation, and short-time high-temperature solution treatment. This method achieves room temperature cold rolling of the alloy while significantly refining the grain size, resulting in a good balance between strength and plasticity. It also features energy efficiency, high cost, and low efficiency.

[0008] Currently, the most mature 6-series aluminum alloys can achieve a maximum yield strength of 350 MPa and a tensile strength of 400 MPa under peak aging heat treatment. Moreover, the holding time for peak aging heat treatment is usually 10-12 hours or even longer. Summary of the Invention

[0009] The purpose of this invention is to provide an ultra-high strength Al-Mg-Si-Cu alloy and its deformation heat treatment method, which improves the alloy strength, shortens the peak aging treatment time, and provides 6xxx series aluminum alloy plates with better comprehensive performance for lightweight design in the future transportation field.

[0010] To achieve the above objectives, the technical solution of the present invention is as follows:

[0011] An ultra-high strength Al-Mg-Si-Cu alloy, characterized in that the alloy composition, by mass percentage, comprises: Mg: 1.2–2.0 wt.%, Si: 1.0–1.5 wt.%, Cu: 0.5–1.5 wt.%, Zn: 0.15–0.5 wt.%, Mn: 0.2–0.4 wt.%, Ti: 0.05–0.1 wt.%, Fe: 0–0.5 wt.%, with the remainder being Al and unavoidable impurities; the density of the strengthening phase in the microstructure of the alloy is ≥7.18 × 10⁻⁶. 22 / m 3 .

[0012] The alloy described in this invention has a yield strength ≥378MPa, a tensile strength ≥415MPa, and an elongation ≥8.7%.

[0013] The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy of the present invention includes the following steps:

[0014] 1) Solution quenching

[0015] The cold-rolled alloy was solution treated by holding it at 550–580℃ for 1.0–2.0 h, and then water-quenched to room temperature after the holding period.

[0016] 2) Handling of overdue payments

[0017] The alloy is subjected to under-aging treatment by holding it at 140–180°C for 1–3 hours.

[0018] 3) Pre-deformation

[0019] After under-aging treatment, the sample was air-cooled to room temperature, and then the under-aged alloy was pre-deformed by cold rolling with a deformation amount of 5-15%.

[0020] 4) Timeliness processing

[0021] The pre-deformed alloy is aged at 160–200℃ for 0.5–4 hours.

[0022] Preferably, in step 1), the solution treatment is carried out in a salt bath furnace.

[0023] Preferably, in step 1), the cooling rate during water quenching is ≥60℃ / s.

[0024] Preferably, the time from water quenching of the alloy to under-aging treatment does not exceed 1 minute.

[0025] Preferably, in step 3), the pre-deformation is a single-pass deformation.

[0026] Preferably, in step 3), the time from the pre-deformation of the alloy to the aging treatment does not exceed 30 minutes.

[0027] Solution hardening of cold-rolled alloy sheets is performed using a salt bath furnace. Once the furnace reaches 550–580°C, the sheet is immersed to rapidly heat to the target temperature. After the furnace temperature stabilizes, a timed holding period of 1.0–2.0 hours begins, followed by rapid water quenching to room temperature. Solution hardening allows the three effective elements—Mg, Si, and Cu—into the alloy sheet to fully dissolve into the matrix.

[0028] The time for transferring the solution-quenched alloy to the constant-temperature drying oven for under-aging treatment should not exceed 1 minute. The reason for strictly limiting the transfer time is that the solution-quenched alloy is in an unstable state of supersaturation of alloying elements. If the placement time is too long, alloying elements will desolve and precipitate during the placement process, affecting the precipitation kinetics of the precipitate phase during the under-aging heat treatment. The under-aging treatment temperature is 140-180℃, and the treatment time is 1-3 hours. The purpose is to precipitate high-density GP zones inside the alloy matrix, increase the dislocation density introduced by subsequent cold rolling pre-deformation, and improve its distribution uniformity.

[0029] After under-aging treatment, the sheet metal undergoes single-pass cold rolling pre-deformation. During the pre-deformation stage, the metastable strengthening phases—β and Q—preferably nucleate along dislocations, increasing the nucleation rate of the strengthening phases along the dislocation direction. The introduction of high-density, uniformly distributed dislocations into the matrix inhibits the coarsening effect of the strengthening phases to some extent, ultimately improving the aging response rate and strength of the alloy, thereby shortening the peak aging heat treatment time. Controlling the pre-deformation reduction to 5–15% further enhances the alloy's mechanical properties based on the combined strengthening effect of precipitation strengthening and dislocation strengthening.

[0030] The pre-deformed samples / sheets were transferred to a constant-temperature drying oven for aging treatment. The transfer time should not exceed 30 minutes, as 6-series sheets undergo natural aging during placement. Shortening the transfer time reduces the occurrence of natural aging and is more conducive to obtaining high strength and rapid aging response during artificial aging. The aging treatment temperature is 160–200℃, and the aging treatment time is 0.5–4 hours. Aging treatment enables secondary precipitation of strengthening phases in the matrix, controls the dislocation configuration, avoids coarsening, improves dislocation distribution, and avoids excessive loss of plasticity.

[0031] This invention involves applying a sub-aging treatment to an Al-Mg-Si-Cu alloy after solution treatment, followed by pre-deformation through cold rolling, and then matching this with subsequent aging treatment. This significantly improves the alloy's strength while greatly shortening the peak aging time. The design principle is as follows:

[0032] Under-aging treatment can induce the precipitation of high-density GP zones in the supersaturated solid solution state of the alloy matrix, increasing the dislocation density introduced by subsequent cold rolling pre-deformation and improving its distribution uniformity. After cold rolling pre-deformation of the under-aged sheet, the introduction of numerous dislocations allows the metastable strengthening phases (β and Q phases) to preferentially nucleate along dislocations during the subsequent aging stage. This increases the nucleation rate of the strengthening phase along the dislocation direction, introducing a high density of uniformly distributed dislocations into the matrix. This, in turn, suppresses the coarsening effect of the strengthening phase to some extent, ultimately improving the aging response rate and strength of the alloy, thus shortening the peak aging heat treatment time. Furthermore, as the aging time increases, dislocations in the matrix exhibit recovery phenomena, which can also improve plasticity to some extent. The synergistic effect of "under-aging-pre-deformation-aging" results in high strength and good plasticity in the sheet.

[0033] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0034] The Al-Mg-Si-Cu alloy of this invention has a higher density of strengthening phases in its microstructure compared to conventional 6-series alloys, wherein the density of strengthening phases is ≥7.18 × 10⁻⁶. 22 / m 3 This improves the alloy's strength while ensuring good plasticity.

[0035] The alloy obtained by this invention undergoes a "slight aging - pre-deformation - aging" heat treatment process after solution treatment to maximize the dispersed precipitation of strengthening phases and maximize the contribution of precipitation strengthening. Simultaneously, based on the combined strengthening effect of precipitation strengthening and dislocation strengthening, the mechanical properties of the alloy are further improved. Subsequent aging treatment controls the dislocation configuration, avoiding excessive loss of plasticity, allowing the aluminum alloy sheet to achieve higher strength while ensuring good ductility. The 6-series aluminum alloy obtained using the method described in this invention has a strengthening phase density ≥ 7.18 × 10⁻⁶. 22 / m 3 The alloy has a yield strength ≥378MPa, a tensile strength ≥415MPa, and an elongation ≥8.7%.

[0036] The method described in this invention introduces high-density, uniformly distributed dislocations during the pre-deformation stage, thereby suppressing the coarsening effect of the strengthening phase, ultimately improving the aging response rate and strength of the alloy, and shortening the peak aging heat treatment time to 0.5–4 hours. In contrast, the peak aging treatment time in conventional processes is typically 10–12 hours. This invention significantly reduces the peak aging treatment time compared to conventional processes, thus improving production efficiency. Attached Figure Description

[0037] Figure 1 This is the hardness change curve of the alloy in Example 3 of the present invention during the aging process.

[0038] Figure 2 The tensile property curve of the alloy in Example 3 of this invention is shown.

[0039] Figure 3 This is a TEM image of the alloy sample from Example 3 of the present invention.

[0040] Figure 4 This is a TEM image of the alloy sample from Comparative Example 1. Detailed Implementation

[0041] The present invention will be further described below with reference to the embodiments and accompanying drawings.

[0042] The alloy compositions used in the embodiments and comparative examples of this invention are shown in Table 1. The alloys with the compositions described in Table 1 were subjected to hot rolling, annealing, and cold rolling to obtain cold-rolled sheets. These sheets were then processed according to the heat treatment process described in this invention.

[0043] The heat treatment process parameters for the embodiments and comparative examples of this invention are detailed in Table 2.

[0044] Alloy samples obtained in the embodiments and comparative examples of this invention were sampled from the center and subjected to mechanical property tests. The experimental results are shown in Table 3.

[0045] As shown in Examples 1 to 7, this invention utilizes a combination of under-aging, pre-deformation, and aging treatments to achieve an ultra-high strength Al-Mg-Si-Cu alloy with a yield strength of 378–437 MPa, a tensile strength of 415–476 MPa, and an elongation of 8.7–14.3%.

[0046] Compared with the traditional T6 process used in Comparative Examples 1-3, the yield strength and tensile strength of the final product were significantly improved, while ensuring that the plasticity was not reduced.

[0047] Figure 1 This is the hardness change curve of the alloy in Example 3 of the present invention during the aging process. Figure 2 The tensile property curve of the alloy in Example 3 of this invention is shown below. Figure 1 and Figure 2 As can be seen from the aging hardness change curve and tensile curve, the mechanical properties of the alloy are rapidly improved by using the deformation heat treatment described in this invention. The time required to reach the peak aging strength is shortened by about 10 hours compared with the traditional peak aging treatment, which greatly improves production efficiency.

[0048] Figure 3 These are TEM images of the alloy obtained in Example 3 of this invention. Figure 4 The TEM image of the alloy obtained in Comparative Example 1 shows that the density of the precipitates in the alloy obtained in this invention is significantly improved compared to that in the comparative example alloy. In the final product obtained by this invention, the aged precipitates are fine and uniformly distributed in the matrix, which plays a significant strengthening role, making the yield strength of the plate reach 427 MPa and the tensile strength reach 463 MPa, while maintaining good plasticity (elongation 10.6%).

[0049] In summary, the method described in this invention maximizes the contribution of precipitation strengthening while introducing a composite strengthening effect of dislocation strengthening, significantly improving the mechanical properties of the alloy. By controlling the aging regime, the dislocation configuration and distribution can be regulated, resulting in sheet metal with good plasticity. This invention provides guidance for the development, processing, and application of ultra-high strength 6xxx series aluminum alloy automotive sheet metal.

[0050] Those skilled in the art should recognize that the above embodiments are merely illustrative of the present invention and are not intended to limit the present invention. Any variations or modifications to the above embodiments that are within the spirit and essence of the present invention will fall within the scope of the claims of the present invention.

[0051]

[0052]

[0053]

Claims

1. An ultra-high strength Al-Mg-Si-Cu alloy, characterized in that, The alloy composition, by mass percentage, comprises: Mg: 1.2–2.0 wt.%, Si: 1.0–1.5 wt.%, Cu: 0.5–1.5 wt.%, Zn: 0.15–0.5 wt.%, Mn: 0.2–0.4 wt.%, Ti: 0.05–0.1 wt.%, Fe: 0–0.5 wt.%, with the remainder being Al and unavoidable impurities; the density of the strengthening phase in the microstructure of the alloy is ≥7.18 × 10⁻⁶. 22 / m 3 .

2. The ultra-high strength Al-Mg-Si-Cu alloy as described in claim 1, characterized in that, The alloy has a yield strength ≥378MPa, a tensile strength ≥415MPa, and an elongation ≥8.7%.

3. The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy as described in claim 1 or 2, characterized in that, Includes the following steps: 1) Solution quenching The cold-rolled alloy was solution treated by holding it at 550–580℃ for 1.0–2.0 h, and then water-quenched to room temperature after the holding period. 2) Handling of overdue payments The alloy is subjected to under-aging treatment by holding it at 140–180°C for 1–3 hours. 3) Pre-deformation After under-aging treatment, the sample was air-cooled to room temperature, and then the under-aged alloy was pre-deformed by cold rolling with a deformation amount of 5-15%. 4) Timeliness processing The pre-deformed alloy is aged at 160–200℃ for 0.5–4 hours.

4. The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy as described in claim 3, characterized in that, In step 1), the solution treatment is carried out in a salt bath furnace.

5. The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy as described in claim 3, characterized in that, The cooling rate during water quenching is ≥60℃ / s.

6. The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy as described in claim 3, characterized in that, The time from water quenching to under-aging treatment of the alloy should not exceed 1 minute.

7. The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy as described in claim 3, characterized in that, In step 3), the pre-deformation is a single-pass deformation.

8. The deformation heat treatment method for ultra-high strength Al-Mg-Si-Cu alloy as described in claim 3 or 7, characterized in that, In step 3), the time from the pre-deformation of the alloy to the aging treatment shall not exceed 30 minutes.

Citation Information

Patent Citations

  • Thermomechanical treatment method capable of simultaneously improving strength and intercrystalline corrosion resistance of 6000 series aluminum alloy

    CN104060201A

  • Thermomechanical treatment process for realizing continuous cold rolling of ultrahigh-strength Al-Zn-Mg-Cu alloy

    CN116623111A

  • Composite thermomechanical treatment method for inhibiting natural aging of aluminum alloy for automobile and improving artificial aging response

    CN117535601A