Tin-based thin film and preparation method and application thereof

By employing a multi-pass gradient deposition method, the problems of poor uniformity, low crystallinity, and weak stability of tin-based thin films in traditional single-pass processes were solved, resulting in tin-based thin films with high uniformity, high crystallinity, and strong stability, exhibiting excellent electrical properties.

CN121951456APending Publication Date: 2026-05-01SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610173400.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-06
Publication Date
2026-05-01

AI Technical Summary

Technical Problem

Tin-based thin films suffer from poor uniformity, low crystallinity, and weak stability in traditional single-pass PCB manufacturing processes, making it difficult to form long-range ordered lattices and resist environmental corrosion.

Method used

A gradient step-by-step deposition method with multiple plate passes was adopted. By controlling the deposition rate and temperature in stages, a nucleation and growth path of 'disordering induction-critical nucleation-directional growth' was constructed, including an initial fast plate pass, subsequent medium-speed plate passes, and a final slow plate pass, thereby optimizing the atomic diffusion and nucleation process.

Benefits of technology

A tin-based thin film with high uniformity, high crystallinity and strong stability was achieved. The crystallinity was improved, the electrical properties were excellent, the film non-uniformity was low, the crystallinity was as high as 53-63%, the sheet resistance change was less than 5%, the conductivity was high and the stability was improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121951456A_ABST
    Figure CN121951456A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thin films, and discloses a tin-based thin film and a preparation method and application thereof. The tin-based thin film is formed by depositing a tin-based material through a physical vapor deposition method, the deposition mode is gradient step-by-step deposition, the number n of times of gradient step-by-step deposition is larger than or equal to 2, and technological parameters of gradient step-by-step deposition meet the following relational expressions: when n is equal to 2, the first-time carrier plate moving speed is gt; the last moving speed of the carrier plate; when ngt; when 2, the first-time moving speed of the carrier plate is gt; the carrier plate moving speed gt of the middle times; and the last carrier plate moving speed. According to the method, a gradient step-by-step deposition method of multi-time plate walking is adopted, the thickness and component deviation of single-time plate walking are compensated, multi-time ion bombardment is used for promoting interdiffusion of interface atoms and accelerating lattice diffusion of doped elements, and the density of a surface layer is optimized through segmented deposition; and finally, the tin-based thin film with high uniformity, high crystallinity, strong stability and excellent electrical properties is prepared at low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of thin film technology, specifically relating to a tin-based thin film, its preparation method, and its application. Background Technology

[0002] Tin-based thin films play a crucial role in solar cells, displays, and transparent conductive electrodes due to their unique photoelectric response, catalytic activity, and dielectric properties. However, the preparation of such materials using traditional physical vapor deposition (PVD, such as magnetron sputtering, electron beam evaporation, reactive plasma deposition, etc.) single-pass or static deposition processes has long faced the following three major technical bottlenecks: First, poor uniformity. During a single continuous deposition process, the deposition rate and energy distribution of target particles on the substrate surface fluctuate over time, easily leading to thickness gradient deviations and compositional segregation, severely affecting batch-to-batch device consistency. Second, low crystallinity. The high energy barrier for atomic migration on the substrate surface makes it difficult to form a long-range ordered lattice in a single deposition, resulting in mostly amorphous or nanocrystalline phases. This hinders carrier transport and degrades electrical performance. Third, weak stability. The high density of oxygen vacancies and grain boundary defects in amorphous structures makes them susceptible to water and oxygen erosion or thermal stress-induced lattice distortion, leading to significant performance degradation after long-term service.

[0003] To address the aforementioned technical problems, existing technologies often employ a single optimization strategy, such as increasing the substrate temperature to improve atomic mobility, but this can easily lead to stress cracking in the thin film; or performing post-annealing to promote crystallization, but this increases energy consumption and causes component volatilization and segregation. Summary of the Invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a tin-based thin film, a method for preparing the same, and its applications. The tin-based thin film exhibits high uniformity, high crystallinity, strong stability, and excellent electrical properties.

[0005] The inventive concept of this invention is as follows: Tin-based materials exhibit relatively slow phase transformation kinetics, meaning that even if a small number of nuclei are formed during deposition, subsequent grain growth still requires atoms to arrange themselves in an orderly manner on the nucleus surface. This process demands sufficient relaxation time and energy from the atoms. Traditional single-pass deposition processes, due to limited deposition time, prevent atoms from fully diffusing and rearranging, hindering grain growth and ultimately resulting in a hybrid "microcrystalline + amorphous" structure. Furthermore, the single-pass deposition mode, which maintains the same process parameters throughout, cannot meet the differentiated requirements of the two core stages of thin film growth: the initial growth stage requires a high deposition rate to generate a disordered structure, while the nucleation and growth stages require a slower rate to allow sufficient time for nuclei to form and grow. These two stages are fundamentally contradictory in their kinetic mechanisms, and single-pass deposition struggles to reconcile this inherent conflict.

[0006] To address the aforementioned technical problems of single-pass deposition, this invention proposes a multi-pass (i.e., gradient step-by-step deposition) strategy to enhance the crystallinity of tin-based materials. By controlling the deposition rate in stages, a nucleation and growth path of "disorder induction - critical nucleation - directional growth" is constructed. Specifically, a fast pass is used initially to induce initial film disorder using a high deposition rate, reducing the subsequent nucleation barrier and providing abundant nucleation sites. Intermediate passes (which may be excluded) use a medium-speed pass to balance particle energy and surface diffusion capacity, controlling the nuclei to enter the "critical nucleation state" and avoiding the uncontrolled "initially ordered, then disordered" state of a single pass. The final pass uses a slow pass to further optimize atomic stacking precision and reduce growth defects. Through this multi-step gradient deposition, the initial disorder of the film synergistically integrates with subsequent controllable nucleation and growth, thereby preparing a highly crystallinity tin-based thin film with excellent optoelectronic properties.

[0007] To address the aforementioned technical problems, a first aspect of the present invention provides a method for preparing a tin-based thin film, wherein the tin-based thin film is deposited from a tin-based material using physical vapor deposition, the deposition method being gradient stepwise deposition, the number of gradient stepwise depositions n≥2, and the process parameters of the gradient stepwise deposition satisfy the following relationship: When n=2, the initial plate movement speed is greater than the final plate movement speed. When n>2, the speed of the first plate movement is greater than the speed of the intermediate plate movements, which is greater than the speed of the last plate movement.

[0008] The carrier plate mentioned in this invention refers to a carrier on which a substrate is loaded. During the deposition process, the carrier plate enters or leaves the vacuum coating chamber at a certain speed, which is called the carrier plate movement.

[0009] This invention employs a gradient step-by-step deposition method with multiple board passes. By moving the carrier plate linearly back and forth within the vacuum deposition chamber, the interaction time between the carrier plate and the plasma or ion beam is extended, compensating for thickness and composition deviations in a single board pass. Multiple ion bombardments promote inter-atomic interdiffusion at the interface and accelerate lattice diffusion of dopant elements. Furthermore, the surface layer density is optimized through segmented deposition, ultimately achieving the preparation of tin-based thin films with high uniformity, high crystallinity, strong stability, and excellent electrical properties at low temperatures.

[0010] In some embodiments of the present invention, the initial carrier plate moving speed is 15-300 mm / s.

[0011] In some embodiments of the present invention, the initial carrier plate moving speed is 20-300 mm / s.

[0012] In some embodiments of the present invention, the intermediate-time carrier plate moving speed is 8-200 mm / s.

[0013] In some embodiments of the present invention, the intermediate-time carrier plate moving speed is 10-150 mm / s.

[0014] In this invention, the carrier plate moving speed in intermediate cycles is between the first and last carrier plate moving speeds. There are no specific requirements for the carrier plate moving speeds in each intermediate cycle; they can be equal or unequal; they can exhibit a gradient change or not.

[0015] In some embodiments of the present invention, the final carrier plate moving speed is 2-150 mm / s.

[0016] In some embodiments of the present invention, the final carrier plate moving speed is 5-100 mm / s.

[0017] In some embodiments of the present invention, the gradient step deposition is performed 2-10 times.

[0018] In some embodiments of the present invention, the time interval between each two gradient step depositions is 5-50 seconds, that is, the time the carrier plate stays at both ends of the linear reciprocating motion is 5-50 seconds.

[0019] In some embodiments of the present invention, the process parameters of the gradient step deposition also satisfy the following relationship: When n=2, the initial deposition temperature is less than the final deposition temperature; When n>2, the initial deposition temperature < intermediate deposition temperatures < final deposition temperature.

[0020] In some embodiments of the present invention, the initial deposition temperature is 20-200°C.

[0021] In some embodiments of the present invention, the initial deposition temperature is 25-85°C.

[0022] In some embodiments of the present invention, the intermediate deposition temperature is 20-200°C.

[0023] In some embodiments of the present invention, the intermediate deposition temperature is 35-165°C.

[0024] Similarly, the intermediate deposition temperatures fall between the first and last deposition temperatures. There are no specific requirements for the deposition temperatures of each intermediate deposition; they can be equal or unequal; they can vary in a gradient or not.

[0025] In some embodiments of the present invention, the final deposition temperature is 20-200°C.

[0026] In some embodiments of the present invention, the final deposition temperature is 35-185°C.

[0027] In some embodiments of the present invention, the tin-based material is a tin-based ceramic target or tin-based particles.

[0028] In some embodiments of the present invention, the tin-based material may be doped with other metal elements, or it may not be doped.

[0029] In some embodiments of the present invention, the doping metal element of the tin-based material is selected from at least one of niobium, aluminum, zinc, tantalum, tungsten, manganese, vanadium, nickel, and indium.

[0030] In some embodiments of the present invention, the doping amount of the tin-based material is 0-50 wt%.

[0031] In some embodiments of the present invention, the physical vapor deposition method is selected from any one of sputtering, evaporation, ion plating, and reactive plasma deposition.

[0032] In some embodiments of the present invention, the deposition process parameters include at least one of the following parameters: 1) Deposition current: 30-300A; 2) Deposition voltage: 10-300V; 3) Partial pressure of the reactant gas: 0.01-5 Pa; 4) Partial pressure of the ignition gas: 0.02-5 Pa; 5) Target-base distance: 200-1500mm.

[0033] In some embodiments of the present invention, the ignition gas is selected from at least one of helium, neon, argon, krypton, and xenon.

[0034] In some embodiments of the present invention, the reaction gas is selected from at least one of oxygen, nitrogen, fluorine, nitrogen trifluoride, acetylene, hydrogen, and water vapor.

[0035] In some embodiments of the present invention, the volume fraction of the reactant gas is 5-95%.

[0036] In some embodiments of the present invention, the target-substrate distance (the distance between the target and the substrate) is 300-1100 mm.

[0037] In some embodiments of the present invention, after depositing a tin-based thin film using physical vapor deposition, a post-processing step is further included, wherein the temperature of the post-processing is 200-550°C.

[0038] In some embodiments of the present invention, the post-processing temperature is 365-425°C.

[0039] In this invention, the deposited thin film can be post-processed to achieve the growth of large grains that penetrate crystallization (the lateral size of the grains can reach 300-600 nm), thereby further improving the carrier mobility of the thin film and enhancing its electrical performance.

[0040] A second aspect of the present invention provides a tin-based thin film, which is prepared by the method for preparing tin-based thin films described in the first aspect of the present invention.

[0041] A third aspect of the present invention provides an optoelectronic device comprising the tin-based thin film described in the second aspect of the present invention.

[0042] Compared with the prior art, the above-described technical solution of the present invention has at least the following technical effects or advantages: (1) The method for preparing tin-based thin films provided by the present invention employs a gradient step-by-step deposition method with multiple plate runs. Multiple plate runs, through dynamic adjustment of deposition parameters and gradient step-by-step deposition, balance the spatiotemporal fluctuations of particle transport in the vacuum chamber, avoiding the accumulation of thickness gradients in a single deposition. For multi-component systems, the composition ratio is finely adjusted in each round, and atomic diffusion is promoted to reduce elemental segregation, achieving dual homogenization of thickness and composition, thus improving the uniformity of the thin film.

[0043] (2) The method for preparing tin-based thin films provided by the present invention adopts the "disordering induction-critical nucleation-directional growth" mode for multiple plate runs. After each round of deposition, the heat preservation is activated to activate atomic migration and overcome the energy barrier of lattice formation. The first layer forms amorphous nucleation sites, and subsequent plate runs guide the atoms to directional arrangement, which significantly improves the crystallinity and the grain order, thereby increasing the crystallinity of the thin film.

[0044] (3) The method for preparing tin-based thin films provided by the present invention involves multiple pass-throughs to deposit thin films in a gradient stepwise manner. Subsequent layers diffuse to fill defects such as oxygen vacancies and interstitial atoms in the preceding layers to reduce chemical activity. Moreover, the multilayer structure can disperse the lattice mismatch stress between the film and the substrate, alleviating the propagation of microcracks. At the same time, the dense multilayer structure blocks the water vapor permeation path and inhibits environmental corrosion, thereby improving the stability of the film.

[0045] (4) The tin-based thin film prepared by this invention has high uniformity, high crystallinity, strong stability and excellent electrochemical performance. It achieves a non-uniformity as low as 3-5%, a crystallinity as high as 53-63%, a sheet resistance change of less than 5% for more than 400 hours, and a conductivity of 1.21×10 2 -1.19×10 3 S / cm. Attached Figure Description

[0046] Figure 1 The images show the XRD patterns of the tin-based thin films prepared in Examples 2, 6, 9, 13 and Comparative Examples 1 and 3. Detailed Implementation

[0047] The present invention will now be described in detail with reference to embodiments to facilitate understanding of the invention by those skilled in the art. It is particularly important to note that the embodiments are merely illustrative of the invention and should not be construed as limiting the scope of protection of the invention. Non-essential improvements and adjustments made to the invention by those skilled in the art based on the above description should still fall within the scope of protection of the invention. Furthermore, all raw materials mentioned below, unless otherwise specified, are commercially available products; all process steps or preparation methods not mentioned in detail are process steps or preparation methods known to those skilled in the art.

[0048] Example 1 A method for preparing tin-based thin films using reactive plasma deposition includes the following steps: (1) Clean the glass substrate, perform ultrasonic deep cleaning and drying; perform ultrasonic cleaning, plasma cleaning and drying on the tin-based ceramic target (the mass fraction ratio of tin dioxide and tantalum pentoxide is 97:3); then place the tin-based ceramic target on the target ingot base, and then load the glass substrate onto the carrier plate, fixing the target-base distance to 700mm.

[0049] (2) Using a reactive plasma deposition apparatus, the vacuum chamber is closed. First, a rough pump is used to evacuate the vacuum chamber. After the vacuum level reaches a certain level, the molecular pump is then turned on to perform a deep evacuation of the vacuum chamber, controlling the background pressure of the chamber to be lower than 8×10⁻⁶. -4 Pa; then argon gas was introduced into the vacuum chamber at a flow rate of 120 sccm, and argon gas was continuously introduced for purging for 10 min; then the electron gun power supply was turned on, and the electron gun current was 150 A. After the electron gun was successfully ignited, the electron gun was pre-deposited onto the target material for 5 min, and then oxygen gas (content of 40%) was introduced at a flow rate of 56 sccm and a partial pressure of 0.17 Pa. During deposition, the argon gas flow rate was 84 sccm and the partial pressure of argon gas was 0.28 Pa. After introducing oxygen for 5 min, the baffle separating the target material from the substrate was opened, and the deposition process parameters were: current 150 A, voltage 80 V.

[0050] (3) After the deposition atmosphere stabilizes, set the parameters for multiple board runs: the number of runs is 2, the first board running speed is 50 mm / s, the first deposition temperature is 65°C; the second board running speed is 6 mm / s, the second deposition temperature is 95°C, and the interval between the two runs is 10 s. After the coating is completed, close the electron gun and the reaction gas valve. After the vacuum chamber and electron gun have cooled down, close the argon gas valve. Finally, open the vacuum chamber and obtain the tin-based thin film of this embodiment from the withdrawn glass substrate.

[0051] Example 2 Referring to the preparation method of the tin-based thin film in Example 1, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 3, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second board-walking speed was 15 mm / s, and the second deposition temperature was 95°C; the third board-walking speed was 8 mm / s, and the third deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0052] Example 3 Referring to the preparation method of the tin-based thin film in Example 1, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 4, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second and third board-walking speeds were 30 mm / s, and the second and third deposition temperatures were 95°C; the fourth board-walking speed was 8 mm / s, and the fourth deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0053] Example 4 Referring to the preparation method of the tin-based thin film in Example 1, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 5, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second to fourth board-walking speeds were 40 mm / s, and the second to fourth deposition temperatures were 95°C; the fifth board-walking speed was 8 mm / s, and the fifth deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0054] Example 5 Referring to the preparation method of the tin-based thin film in Example 1, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 10, the first board-walking speed was 100 mm / s, and the first deposition temperature was 65°C; the second to ninth board-walking speeds were 80 mm / s, and the second to ninth deposition temperatures were 95°C; the tenth board-walking speed was 8 mm / s, and the tenth deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0055] Example 6 Referring to the preparation method of the tin-based thin film in Example 1, the tin source in step (1) was changed to metallic tin particles, the oxygen content in step (2) was changed to 90%, and the multiple board-walking parameters in step (3) were changed: the number of board-walking times was 3, the first board-walking speed was 60 mm / s, the first deposition temperature was 65°C; the second board-walking speed was 25 mm / s, the second deposition temperature was 95°C; the third board-walking speed was 10 mm / s, the third deposition temperature was 115°C, and the interval between each two board-walking times was 10 s, thus obtaining the tin-based thin film of this example.

[0056] Example 7 Referring to the preparation method of the tin-based thin film in Example 1, the reaction gas in step (2) was changed to oxygen and hydrogen, with the oxygen content being 40% and the hydrogen content being 1%. The parameters of the multiple board-walking in step (3) were also changed: the number of board-walking times was 3, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second board-walking speed was 15 mm / s, and the second deposition temperature was 95°C; the third board-walking speed was 8 mm / s, and the third deposition temperature was 115°C. The interval between each two board-walking times was 10 s, and the tin-based thin film of this example was obtained.

[0057] Example 8 A method for preparing tin-based thin films using magnetron sputtering includes the following steps: (1) Clean the glass substrate, perform ultrasonic deep cleaning and drying; perform ultrasonic cleaning, plasma cleaning and drying on the tin-based ceramic target (the mass fraction ratio of tin dioxide and tantalum pentoxide is 97:3); then place the tin-based ceramic target on the target ingot base, and then load the glass substrate onto the carrier plate, fixing the target-base distance to 700mm.

[0058] (2) Using a magnetron sputtering device, the vacuum chamber is closed. First, a rough pump is used to evacuate the vacuum chamber. After the vacuum level reaches a certain level, the molecular pump is turned on to perform a deep evacuation of the vacuum chamber, controlling the background pressure of the chamber to be lower than 8×10. - 4 Pa; then argon gas is introduced into the vacuum chamber at a flow rate of 50 sccm, and argon gas is continuously introduced for purging for 10 min; then the magnetron power supply is turned on, the sputtering power is set to 200W, and the target surface is pre-sputtered for 5 min; after the pre-sputtering is completed, the reactive gas oxygen (content is 40%) is introduced simultaneously at a flow rate of 20 sccm, and the argon gas flow rate introduced during deposition is 30 sccm.

[0059] (3) After the deposition atmosphere stabilizes, set the parameters for multiple board runs: the number of runs is 2, the first board running speed is 50 mm / s, the first deposition temperature is 65°C; the second board running speed is 6 mm / s, the second deposition temperature is 95°C, and the interval between the two runs is 10 s. After the coating is completed, turn off the magnetron power supply, wait for the vacuum chamber to cool down, and then turn off the argon gas valve; finally, open the vacuum chamber and obtain the tin-based thin film of this embodiment from the withdrawn glass substrate.

[0060] Example 9 Referring to the preparation method of the tin-based thin film in Example 8, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 3, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second board-walking speed was 15 mm / s, and the second deposition temperature was 95°C; the third board-walking speed was 8 mm / s, and the third deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0061] Example 10 Referring to the preparation method of the tin-based thin film in Example 8, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 4, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second and third board-walking speeds were 30 mm / s, and the second and third deposition temperatures were 95°C; the fourth board-walking speed was 8 mm / s, and the fourth deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0062] Example 11 Referring to the preparation method of the tin-based thin film in Example 8, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 5, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second to fourth board-walking speeds were 40 mm / s, and the second to fourth deposition temperatures were 95°C; the fifth board-walking speed was 8 mm / s, and the fifth deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0063] Example 12 Referring to the preparation method of the tin-based thin film in Example 8, the parameters of multiple board-walking in step (3) were changed: the number of board-walking times was 10, the first board-walking speed was 100 mm / s, and the first deposition temperature was 65°C; the second to ninth board-walking speeds were 80 mm / s, and the second to ninth deposition temperatures were 95°C; the tenth board-walking speed was 8 mm / s, and the tenth deposition temperature was 115°C, with an interval of 10 s between each board-walking time, thus obtaining the tin-based thin film of this example.

[0064] Example 13 Referring to the preparation method of the tin-based thin film in Example 8, the tin source in step (1) was changed to metallic tin particles, the oxygen content in step (2) was changed to 90%, and the multiple board-walking parameters in step (3) were changed: the number of board-walking times was 3, the first board-walking speed was 60 mm / s, the first deposition temperature was 65°C; the second board-walking speed was 25 mm / s, the second deposition temperature was 95°C; the third board-walking speed was 10 mm / s, the third deposition temperature was 115°C, and the interval between each two board-walking times was 10 s, thus obtaining the tin-based thin film of this example.

[0065] Example 14 Referring to the preparation method of the tin-based thin film in Example 8, the reaction gas in step (2) was changed to oxygen and hydrogen, with the oxygen content being 40% and the hydrogen content being 1%. The parameters of the multiple board-walking in step (3) were also changed: the number of board-walking times was 3, the first board-walking speed was 50 mm / s, and the first deposition temperature was 65°C; the second board-walking speed was 15 mm / s, and the second deposition temperature was 95°C; the third board-walking speed was 8 mm / s, and the third deposition temperature was 115°C. The interval between each two board-walking times was 10 s, and the tin-based thin film of this example was obtained.

[0066] Comparative Example 1 Referring to the preparation method of the tin-based thin film in Example 1, the board parameters in step (3) were changed: the number of board passes was single, the board moving speed was 5 mm / s, and the deposition temperature was 115°C, thus obtaining the tin-based thin film of this comparative example.

[0067] Comparative Example 2 Referring to the preparation method of tin-based thin film in Example 1, the tin source in step (1) was changed to metallic tin particles, the oxygen content in step (2) was changed to 90%, and the board parameters in step (3) were changed: the number of board passes was single, the board moving speed was 5 mm / s, and the deposition temperature was 115°C, so as to obtain the tin-based thin film of this comparative example.

[0068] Comparative Example 3 Referring to the preparation method of the tin-based thin film in Example 8, the board parameters in step (3) were changed: the number of board passes was single, the board moving speed was 5 mm / s, and the deposition temperature was 115°C, thus obtaining the tin-based thin film of this comparative example.

[0069] Comparative Example 4 Referring to the preparation method of the tin-based thin film in Example 8, the tin source in step (1) was changed to metallic tin particles, the oxygen content in step (2) was changed to 90%, and the board parameters in step (3) were changed: the number of board passes was single, the board moving speed was 5 mm / s, and the deposition temperature was 115°C, so as to obtain the tin-based thin film of this comparative example.

[0070] Comparative Example 5 Referring to the preparation method of the tin-based thin film in Example 1, the board parameters in step (3) were changed: the number of board passes was 3, the board moving speed was kept constant at 12 mm / s, and the deposition temperature was kept constant at 95°C, thus obtaining the tin-based thin film of this comparative example.

[0071] Performance testing The properties of the tin-based thin films prepared in Examples 1-14 and Comparative Examples 1-5 were tested, and the results are shown in Table 1. Stability is defined as the time during which the sheet resistance change is less than 5% in the double 85 test.

[0072] Table 1:

[0073] As shown in Table 1, the tin-based thin films prepared in Examples 1-14 all exhibit high uniformity, high crystallinity, strong stability, and excellent electrochemical performance. They achieved a non-uniformity as low as 3-5%, a crystallinity as high as 53-63%, a sheet resistance change of less than 5% for over 400 hours, and a conductivity of 1.21 × 10⁻⁶. 2 -1.19×10 3 S / cm. Compared to Example 1 or Example 8, the properties of the films in Comparative Examples 1-5 were significantly reduced due to the lack of gradient stepwise deposition.

[0074] Figure 1 The XRD patterns are of the tin-based thin films prepared in Examples 2, 6, 9, 13 and Comparative Examples 1 and 3. Figure 1 It can be seen that, regardless of whether magnetron sputtering or reactive plasma deposition is used, the gradient step-by-step deposition method with multiple substrate passes is more likely to obtain crystalline tin dioxide films. The main reason for this is that during multiple substrate passes, the substrate moves multiple times during the deposition process, allowing for differentiated control of the "disorder induction-critical nucleation-directional growth" process. This provides sufficient nucleation sites and ensures sufficient time for atomic diffusion and arrangement, making it easier to form long-range ordered crystal structures and thus more likely to obtain highly crystalline tin-based films.

[0075] For those skilled in the art, several simple deductions or substitutions can be made without departing from the inventive concept, without requiring creative effort. Therefore, any simple improvements made to this invention by those skilled in the art based on the disclosure of this invention should be within the scope of protection of this invention. The above embodiments are preferred embodiments of this invention, and all processes similar to this invention and equivalent changes should fall within the scope of protection of this invention.

Claims

1. A method for preparing a tin-based thin film, characterized in that, The tin-based thin film is deposited from a tin-based material using physical vapor deposition. The deposition method is gradient stepwise deposition, where the number of gradient stepwise depositions n≥2, and the process parameters of the gradient stepwise deposition satisfy the following relationship: When n=2, the initial plate movement speed is greater than the final plate movement speed. When n>2, the speed of the first plate movement is greater than the speed of the intermediate plate movements, which is greater than the speed of the last plate movement.

2. The method for preparing tin-based thin films according to claim 1, characterized in that, The initial carrier plate moving speed is 15-300 mm / s; and / or, the intermediate carrier plate moving speed is 8-200 mm / s; and / or, the final carrier plate moving speed is 2-150 mm / s.

3. The method for preparing a tin-based thin film according to claim 1 or 2, characterized in that, The time interval between each gradient step deposition is 5-50 seconds.

4. The method for preparing a tin-based thin film according to claim 1, characterized in that, The tin-based material is a tin-based ceramic target or tin-based particles.

5. The method for preparing a tin-based thin film according to claim 1, characterized in that, The physical vapor deposition method is selected from any one of sputtering, evaporation, ion plating, and reactive plasma deposition.

6. The method for preparing a tin-based thin film according to claim 5, characterized in that, The deposition process parameters include at least one of the following parameters: 1) Deposition current: 30-300A; 2) Deposition voltage: 10-300V; 3) Partial pressure of the reactant gas: 0.01-5 Pa; 4) Partial pressure of the ignition gas: 0.02-5 Pa; 5) Target-base distance: 300-1100mm.

7. The method for preparing a tin-based thin film according to claim 6, characterized in that, The ignition gas is selected from at least one of helium, neon, argon, krypton, and xenon; and / or the reaction gas is selected from at least one of oxygen, nitrogen, fluorine, nitrogen trifluoride, acetylene, hydrogen, and water vapor.

8. The method for preparing a tin-based thin film according to claim 1, characterized in that, After depositing a tin-based thin film using physical vapor deposition, a post-processing step is also included, wherein the temperature of the post-processing is 200-550°C.

9. A tin-based thin film, characterized in that, The tin-based thin film was prepared using the method described in any one of claims 1-8.

10. An optoelectronic device, characterized in that, Including the tin-based thin film as described in claim 9.