Scandium oxide modified aluminum oxide-zirconium oxide high-temperature-resistant composite ceramic fiber and preparation method thereof

By modifying with appropriate amounts of scandium oxide and optimizing the process, alumina-zirconia composite ceramic fibers were prepared, solving the problem of grain growth in alumina-based ceramic fibers at high temperatures and improving high-temperature stability and mechanical properties, making them suitable for aerospace and industrial high-temperature components.

CN121951740APending Publication Date: 2026-05-01CENT SOUTH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610133272.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-30
Publication Date
2026-05-01

AI Technical Summary

Technical Problem

Existing alumina-based ceramic fibers are prone to abnormal grain growth in high-temperature environments, leading to a significant decrease in mechanical properties. Current technologies have failed to effectively address the issue of scandium oxide and zirconium oxide forming a composite pinning effect in alumina fibers to improve toughness and high-temperature stability.

Method used

Alumina-zirconia composite ceramic fibers were prepared by modifying with appropriate amounts of scandium oxide and optimizing the process. The ratio of scandium oxide to zirconia and the preparation process were controlled. The sol-gel method and dry spinning were combined with a multi-step sintering process to form uniformly distributed scandium oxide and zirconia, thereby improving the high-temperature stability and mechanical properties of the fibers.

Benefits of technology

When used for extended periods at temperatures above 1200 degrees Celsius, the alumina grain size is less than 0.33 micrometers, and the tensile strength of the fiber monofilament is greater than 1.65 GPa, significantly improving high-temperature stability and mechanical properties, making it suitable for extreme environments such as hot-end components of aero-engines and high-temperature furnace linings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121951740A_ABST
    Figure CN121951740A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of inorganic ceramic materials, particularly relates to a scandium oxide modified continuous aluminum oxide-zirconium oxide high-temperature-resistant composite ceramic fiber and a preparation method thereof, and particularly relates to a technology for regulating and controlling the microstructure of the composite fiber through the synergistic effect of rare earth oxide and a preparation process so as to improve the high thermal stability. The fiber composite ceramic fiber comprises the following components in percentage by mass: 0.1 to 3 percent of scandium oxide, preferably 0.5 to 2.5 percent, further preferably 0.8 to 1.2 percent, 8 to 9.5 percent of zirconium oxide, preferably 8.8 to 9.2 percent, and the balance of aluminum oxide, the grain size of the aluminum oxide is 150 to 200nm, the grain size of the zirconium oxide at the grain boundary is 40 to 80nm, and the grain size of the zirconium oxide at the intragranular position is 5 to 20nm. The obtained product is subjected to heat preservation service for 100 hours at the temperature of 1200 DEG C in the air atmosphere and then cooled to the room temperature, and the grain size of aluminum oxide in the product is only 0.21-0.33 micron. The composition is reasonable in design, the preparation process is simple and controllable, and the obtained product is extremely excellent in heat resistance and mechanical property and convenient for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inorganic ceramic materials, specifically relating to a scandium oxide-modified continuous alumina-zirconia high-temperature resistant composite ceramic fiber and its preparation method, and particularly to a technology that improves high thermal stability by regulating the microstructure of the composite fiber through rare earth oxides. Background Technology

[0002] Continuous alumina-based ceramic fibers have significant application value in aerospace, high-temperature oxidation resistance, and insulation properties, making them valuable in fields such as aerospace and high-temperature industrial components. However, when alumina-based fibers operate in environments exceeding 1000°C, alumina grains are prone to abnormal growth, leading to a significant decline in fiber mechanical properties. Introducing second-phase particles (such as zirconium oxide) is a common method to suppress grain growth in ceramic materials; the addition of zirconium oxide can improve the thermal stability, strength, and toughness of alumina fibers. However, when two phases coexist, phase interface control, phase transformation path control, and maintenance of microstructure stability remain challenging problems in the field of materials science.

[0003] In the prior art, the method of regulating the microstructure of ceramic fibers by adding rare earth oxides has been widely studied. For example, adding yttrium oxide can stabilize the tetragonal phase of zirconium oxide. Patent CN118302398A involves a ceramic matrix composite material and its manufacturing method, which includes a ceramic matrix, continuous ceramic fibers, and at least two sintering inhibitors. The sintering inhibitors are selected from two or more of the following groups: silicon dioxide, germanium oxide, zirconium oxide, yttrium oxide, titanium dioxide, hafnium oxide, magnesium oxide, scandium oxide, lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, erbium oxide, ytterbium oxide, lutetium oxide, and mullite. The typical preparation method involved includes: mixing 49g of α-alumina powder (average particle size: 0.15μm), 0.15g of spherical silica powder (average particle size: 0.24μm), 1.0g of zirconium powder containing 3mol% yttrium (average particle size: 0.04μm; 3YSZ powder), and 50g of ethanol in a ball mill with 10mm diameter alumina balls as the grinding medium for 24 hours to obtain a raw material slurry with a solid content concentration of 50% by mass, which is used as the raw material slurry in this synthesis example. The raw material slurry of this synthesis example is then subjected to atmospheric conditions at 60°C to remove the solvent, resulting in the powder of this synthesis example. This patent does not involve characterizing the high-temperature resistance of the product. Patent CN117702306 A yields alumina-zirconia composite ceramic fibers with extremely high strength, but does not describe the mechanical property parameters of the product after service at 1200°C.

[0004] Meanwhile, the search revealed that there are no existing records of how scandium oxide and zirconium oxide work together in appropriate amounts and proportions to form a composite pinning effect in alumina fibers, thereby obtaining continuous ceramic fibers with high toughness. Summary of the Invention

[0005] This invention addresses the need for further improvement in the overall performance of existing high-temperature ceramic fibers. Building upon patent CN117702306 A, it is the first to synthesize alumina-zirconia composite fibers that maintain extremely superior mechanical properties even after service at 1200 degrees Celsius through synergistic modification with appropriate scandium oxide and process optimization. These fibers can be applied to extreme environments such as hot-end components of aero-engines and high-temperature furnace linings, solving the failure problem caused by grain growth in existing materials and promoting technological advancements in high-temperature structural materials.

[0006] This invention discloses a scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber. In the composite ceramic fiber, by mass percentage, scandium oxide is 0.1-3%, preferably 0.8-1.2%, zirconia is 8-9.5%, preferably 8.8-9.2%, and the balance is alumina. The alumina grain size is 150-200 nm, the zirconia grains at the grain boundaries are 40-80 nm, and the zirconia grains within the grains are 5-20 nm.

[0007] Preferably, in this invention, the mass ratio of Sc to Zr in the fiber-composite ceramic fiber is 1:8-15, preferably 1:9-11, and more preferably 1:10; and the scandium oxide content is controlled at 0.1-3%, preferably 0.8-1.2%, and the zirconium oxide content at 8-9.5%, preferably 8.8-9.2%. This is because an appropriate amount of scandium combined with an appropriate amount of zirconium, in a reasonable ratio, is beneficial for obtaining a better fiber structure, high monofilament tensile strength, faster densification rate, and high thermal stability. In particular, with the coordination of the preparation process, it is beneficial for improving the long-term use of the product at 1200 degrees Celsius and above. If the amount of Zr is too large and the molar ratio of Sc to Zr is too small, it will lead to coarse alumina grains, reduced refining effect of scandium oxide on alumina and zirconium oxide grains, decreased mechanical properties of the fiber, and a series of problems such as rapid decay of mechanical properties of the fiber during high-temperature service at 1200 degrees Celsius.

[0008] This invention discloses a scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber. After being kept at 1200°C for 100 hours in air and then cooled to room temperature, the alumina grain size in the product is less than or equal to 0.33 micrometers, and only 0.21-0.33 micrometers, such as 0.20-0.33 micrometers.

[0009] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers, comprising the following steps:

[0010] Step 1: Mixing

[0011] According to the designed proportions, aluminum sol, zirconium acetate, iron sol, PVP solution, yttrium nitrate solution, and scandium nitrate solution are mixed evenly to obtain a mixture.

[0012] Step Two: Concentration

[0013] The mixture is stirred at 35-65℃, preferably 40-60℃, and concentrated in at least two steps to a viscosity of 10-100 Pa / s to obtain a spinning gel.

[0014] Step 3: Spinning

[0015] The obtained gel was dry-spun to obtain gel precursor fibers. During dry spinning, the spinning kettle temperature was controlled at 40-60℃; the spinneret orifice diameter was 70-90μm; the channel length was 3m; the channel temperature was 120-160℃; and the winding machine take-up rate was 60-90r / min.

[0016] Step Four

[0017] The gel precursor fiber is placed in a sintering device, pre-sintered at 450-550℃ for at least 60 min, sintered at 1000℃ for 8-12 min, and then sintered at 1395-1405℃ for 60s-420s.

[0018] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers, which employs a sol-gel method to prepare aluminum sol. The sol-gel method for preparing aluminum sol includes the following operations:

[0019] Add 6000ml of deionized water to a reaction vessel kept at 80℃ and start stirring. Then add 470g of formic acid (Aladdin) and 540g of glacial acetic acid (Aladdin) to the deionized water and stir. Then add 400g of aluminum powder (Aladdin 1-3um) to the reaction vessel in at least three portions, one hour apart, and react with the formic acid and acetic acid until fully reacted. Mix and stir for at least 24 hours.

[0020] During the reaction, 2wt% dilute nitric acid was added dropwise as a reaction aid. After the aluminum powder was added, 1100g of 2wt% dilute nitric acid was added into the reaction vessel through a separatory funnel.

[0021] After the reaction is complete, stop stirring and heating. After the liquid in the reactor cools to room temperature, filter it to obtain aluminum sol.

[0022] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers, wherein the iron sol is prepared through the following steps:

[0023] Take 110g of ferric nitrate nonahydrate according to the proportion, add it to 2550ml of deionized water, keep it warm in a water bath at 70℃ and stir, while adding a solution made of 54g of ammonium bicarbonate and 540g of deionized water dropwise at a rate of 1-3 drops per second; after the addition is complete, keep it warm in the water bath for at least 1 hour to complete the preparation of the iron sol, and then stop heating and stirring.

[0024] In this invention, iron sol is used as a nucleating agent to promote the nucleation of alumina and zirconium oxide crystals, and at the same time promotes grain refinement. The addition ratio is 1%-5%, and the optimal addition amount is 4%, which is 4% of the solid content of alumina.

[0025] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers.

[0026] Add 27g of PVP (5% of the alumina solid content) to 270g of deionized water according to the ratio. After stirring in a 40℃ water bath for 1 hour, stop heating and stirring. The PVP solution is now ready.

[0027] In this invention, PVP is a spinning aid that promotes the spinnability of alumina-zirconia fibers.

[0028] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers.

[0029] Take yttrium nitrate hexahydrate according to the ratio, add an appropriate amount of deionized water, stir to dissolve completely, and obtain a uniformly mixed yttrium nitrate solution with the desired concentration.

[0030] As a preferred option, take 21g of yttrium nitrate hexahydrate (the content of the yttrium oxides generated accounts for 1% of the mass of the final alumina) according to the proportion, add an appropriate amount of deionized water, stir to dissolve fully, and obtain a uniformly mixed yttrium nitrate solution.

[0031] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers. The method involves taking a corresponding proportion of scandium nitrate pentahydrate, adding an appropriate amount of deionized water, stirring evenly, and dissolving thoroughly to obtain a uniformly mixed scandium nitrate solution.

[0032] This invention discloses a method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fibers. The method employs preliminary and final concentration. During preliminary concentration, the temperature is controlled at 50-60°C and the rotation speed at 5-40 r / min, removing 70-80% of the moisture. Then, the temperature is lowered to 40-45°C, and the rotation speed is increased to 45-80 r / min until a spinning gel with a viscosity of 10-100 Pa / s, preferably 80-100 Pa / s, is obtained. This distributional concentration method ensures more uniform material composition. Specifically, using a higher temperature and lower rotation speed initially, followed by a lower temperature and higher rotation speed later, allows for greater uniformity of components in the gradually formed gel. This also provides the necessary conditions for the uniform distribution of Zr and Sc during subsequent sintering. The uniform distribution of Zr and Sc is beneficial for improving the strength of the product after long-term service at high temperatures (e.g., 1200°C). This invention is the first to discover and apply this point, and in conjunction with the subsequent multi-step sintering process, it has yielded excellent products with a strength greater than 1.65 GPa after long-term service at high temperatures (such as 1200 degrees Celsius).

[0033] During dry spinning, the spinning kettle temperature is controlled at 45-55 ℃; the spinneret orifice diameter at 70-90 μm; the duct length at 3 m; the duct temperature at 135-145 ℃, preferably 140 ℃; and the winding machine take-up rate at 75-85 r / min, preferably 80 r / min. Compared to the previously developed technology, the duct temperature is appropriately increased because the addition of rare earth elements reduces the viscosity of the spinning process. Increasing the duct temperature is beneficial for fiber formation during spinning, and increasing the take-up rate is also beneficial because the reduced fiber viscosity allows for faster take-up, thereby reducing fiber diameter and grain size, which improves the mechanical properties of the fiber, especially the high-temperature mechanical properties of the product.

[0034] This invention involves pre-sintering in an air atmosphere to remove water, PVP, acids, and other impurities from the fiber, yielding pre-sintered fiber. The pre-sintered fiber is then subjected to high-temperature sintering in an air atmosphere to obtain scandium oxide-added alumina-zirconia multiphase ceramic fiber.

[0035] Preferably, the present invention employs a stepped heating regime during pre-sintering, wherein the stepped heating regime is as follows:

[0036] The heating rate from room temperature to 100°C is 2°C / min.

[0037] The temperature range is 100℃-250℃, with a heating rate of 1~1.5℃ / min.

[0038] 250-500℃, heating rate is 0.5~1℃ / min.

[0039] In this invention, the pre-sintering employs the aforementioned gradient heating regime to avoid creating large pores inside the pre-sintered fibers, particularly closed pores that are large inside and small outside, or even sealed within the pre-sintered fibers.

[0040] In the pre-firing process of this invention, the temperature is 100℃-250℃ and the heating rate is 1~1.5℃ / min. This is because the fiber can remove moisture and some impurities as much as possible at low temperature during the pre-firing process, effectively reducing the porosity and impurities in the fiber.

[0041] Principles and advantages

[0042] This invention introduces an appropriate amount of nano-scandium oxide in situ. Under the synergistic effect of nano-scandium oxide and zirconium oxide in appropriate proportions and with the coordination of appropriate process parameters, a system reinforcement is formed. This results in high-temperature resistant composite ceramic fibers of scandium oxide modified alumina-zirconia with excellent heat resistance and mechanical strength. Attached Figure Description

[0043] Figure 1 X-ray diffraction patterns of fibers with different scandium oxide additions after being kept at 1400℃ for 10 hours;

[0044] Figure 2 Scanning electron microscope (SEM) images of fibers with different scandium oxide addition amounts;

[0045] Figure 3 SEM images of fibers with different scandium oxide additions after 0, 10, 50, and 100 hours of service at 1200℃;

[0046] Figure 4 SEM images of fibers obtained by sintering pre-sintered fibers at different maximum sintering temperatures for 7 minutes, as shown in Comparative Example 6.

[0047] Figure 1In the figures, the curve for 0% Sc2O3 is the XRD pattern of the product obtained in Comparative Example 1 after 10 hours of service at 1400°C; the curve for 0.5% Sc2O3 is the XRD pattern of the product obtained in Example 7 after 10 hours of service at 1400°C; the curve for 1% Sc2O3 is the XRD pattern of the product obtained in Example 2 after 10 hours of service at 1400°C; the curve for 3% Sc2O3 is the XRD pattern of the product obtained in Example 10 after 10 hours of service at 1400°C; the curve for 5% Sc2O3 is the XRD pattern of the product obtained in Comparative Example 3 after 5 minutes of high-temperature sintering at 1400°C; the curve for 7% Sc2O3 is the XRD pattern of the product obtained in Comparative Example 4 after 5 minutes of high-temperature sintering at 1400°C; and the curve for 10% Sc2O3 is the XRD pattern of the product obtained in Comparative Example 5 after 10 hours of service at 1400°C. The XRD pattern afterward. From Figure 1 As can be seen, when the scandium oxide content is below 3%, the phase composition of the fiber is mainly α-Al2O3 and t-ZrO2, with no other impurity phases appearing. However, when the scandium oxide content exceeds a certain limit, a Zr-Sc composite phase appears in the spectrum.

[0048] Figure 2 In the images, (a)-(d) are SEM images of fibers obtained by sintering at 1400℃ for 1, 3, 5, and 7 min under the conditions of Comparative Example 1, respectively; (e)-(h) are SEM images of fibers obtained in Examples 5, 6, 7, and 8, respectively; (i)-(l) are SEM images of fibers obtained in Examples 1, 2, 3, and 4, respectively; and (m)-(p) are SEM images of fibers obtained in Examples 9, 10, 11, and 12, respectively. Figure 2 As can be seen, the undoped sample exhibited fine grains and obvious intergranular porosity after calcination at 1400 °C for 1 minute. These porosity are attributed to the increased density caused by the formation of new phases. With prolonged calcination time, the fiber density gradually increased, and the fine grains gradually aggregated and coarsened. After 7 minutes of calcination, the fiber achieved complete densification. Sc2O3 doping promoted the development of α-Al2O3 and t-ZrO2 phases. Therefore, in the sample calcined at 1400 °C for 1 minute, the grain size increased with increasing Sc2O3 content. Furthermore, samples doped with 0.5, 1.0, and 3.0 wt.% Sc2O3 required 5, 3, and 6 minutes, respectively, to obtain fully densified fibers. These results indicate that Sc2O3 doping improves the densification degree of the fiber, with the fastest densification rate observed at 1.0 wt.% Sc2O3. The Sc2O3 content also affects the fiber grain size. The sample doped with 1.0 wt.% Sc2O3 had the smallest average grain size of 0.17 μm.

[0049] Figure 3 In the figures, (a)-(d) are SEM images of the product obtained in Comparative Example 1 after 0, 10, 50, and 100 hours of service at 1200°C, respectively; (e)-(h) are SEM images of the product obtained in Example 7 after 0, 10, 50, and 100 hours of service at 1200°C, respectively; (i)-(l) are SEM images of the product obtained in Example 2 after 0, 10, 50, and 100 hours of service at 1200°C, respectively; and (m)-(p) are SEM images of the product obtained in Example 11 after 0, 10, 50, and 100 hours of service at 1200°C, respectively. Figure 3 As can be seen, after being kept at 1200℃ for 100 hours, the grain growth rate of the fiber with added scandium oxide was significantly smaller than that of the fiber without added scandium oxide, especially when the scandium oxide addition was 1%, the grain growth rate was the smallest. This indicates that the addition of scandium oxide in this invention significantly improves the stability of the composite fiber under high-temperature, long-term service conditions. In high-temperature environments, the stability of a material is a key factor determining its service life and performance reliability. This invention, by improving the high-temperature stability of the fiber, enables it to maintain good performance under extreme operating conditions, broadening the application range of composite fibers and providing an effective solution to the problem of performance degradation caused by grain growth in existing high-temperature materials during practical use.

[0050] Figure 4 In the image, (a) is a SEM image of the product sintered at a maximum sintering temperature of 1100℃, (b) is a SEM image of the product sintered at a maximum sintering temperature of 1200℃, (c) is a SEM image of the product sintered at a maximum sintering temperature of 1300℃, (d) is a SEM image of the product sintered at a maximum sintering temperature of 1400℃, and (e) is a SEM image of the product sintered at a maximum sintering temperature of 1500℃. Figure 4 It can be seen that excessive addition of zirconium oxide leads to a significant decrease in the fiber's microstructure and mechanical properties. Detailed Implementation

[0051] Comparative Example 1 (Alumina-zirconia multiphase fibers with 0% scandium oxide addition, 1400℃ / 7min)

[0052] 1) Aluminum sol was prepared by sol-gel method. 6000ml of deionized water was added to a reaction vessel kept at 80℃ and stirred. Then, 470g of formic acid (Aladdin) and 540g of glacial acetic acid (Aladdin) were added to the deionized water and stirred. Then, 400g of aluminum powder (Aladdin 1-3um) was added to the reaction vessel in three portions, one hour apart, and reacted fully with formic acid and acetic acid. The mixture was stirred for 24 hours.

[0053] 2) Adding dilute nitric acid: During the reaction, 2wt% dilute nitric acid is added dropwise as a reaction aid. After the aluminum powder is added, 1100g of 2wt% dilute nitric acid is added to the reaction vessel through a separatory funnel.

[0054] 3) After the reaction is complete, stop stirring and heating. Filter the liquid in the reactor after it has cooled to room temperature. (Filter multiple times, first using filter paper with larger pores to remove unreacted aluminum powder or other particles, then using filter paper with smaller pores for at least two more filtrations to ensure the purity of the sol.)

[0055] 4) Preparation of iron sol: Take 110g of ferric nitrate nonahydrate, add it to 2550ml of deionized water, and keep it warm and stirred in a water bath at 70℃. At the same time, add a solution prepared by 54g of ammonium bicarbonate and 540g of deionized water dropwise at a rate of 1 drop per second. After the addition is complete, keep it in the water bath for 1 hour to complete the preparation of the iron sol, and then stop heating and stirring.

[0056] 5) PVP preparation: Add 27g of PVP (i.e., 5wt% of the mass of Al2O3 in the product) to 270g of deionized water, keep warm and stir in a 40℃ water bath for 1h, then stop heating and stirring. The PVP solution preparation is complete.

[0057] 6) Take 21g of yttrium nitrate hexahydrate (i.e., 1wt% relative to the mass of Al2O3 in the product), add an appropriate amount of deionized water, and stir until fully dissolved;

[0058] 7) Mixing and stirring: Take 6000g of aluminum sol prepared in steps 1 and 2, 230g of zirconium acetate (Aladdin), iron sol prepared in step 4, PVP solution prepared in step 5, and yttrium nitrate solution prepared in step 6, and pour them into a glass concentration bottle and stir. Mix for 24 hours to form a uniform mixture.

[0059] 8) Preliminary concentration: The homogeneous mixture after stirring is distilled using a rotary evaporator to concentrate most of the water (6500g of water). The remaining liquid is then poured into a small rotary evaporator for final concentration. The preliminary concentration temperature is 50 degrees Celsius, and the rotation speed is 40 r / min.

[0060] 9) Final Concentration: Slowly concentrate the remaining liquid, observing the viscosity of the solution. Concentrate until it reaches a spinnable viscosity, at which point it becomes a gel. The concentration temperature is 40℃-45℃, and the concentration rotation speed is 5-40 r / min, gradually decreasing the speed. The concentration time is approximately 3 hours. Stop concentration when the fiber reaches a spinnable viscosity; at this point, the gel viscosity is 80 Pa / s.

[0061] 10) Dry spinning; The concentrated gel from step 9 is dry spun to obtain gel precursor fibers. During dry spinning, the spinning kettle temperature is controlled as follows: 50℃; spinneret orifice diameter: 80μm; duct length: 3m; duct temperature: 140℃; winding machine take-up rate: 80r / min.

[0062] 11) Sintering: The precursor fibers are pre-sintered to remove water, PVP, acids, and other impurities, obtaining pre-sintered fibers. The pre-sintered fibers are then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia multiphase ceramic fibers. The pre-sintering temperature is 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 400℃, and 0.6℃ / min from 400℃ to 500℃. The high-temperature section employs a two-step sintering method: holding at 1000℃ for 10 min, followed by holding at 1400℃ for 7 min.

[0063] XRD analysis of the fibers revealed no other phase formation. The resulting alumina-scandium oxide composite ceramic fibers had a diameter of 10-12 μm, and the fibers were as shown in SEM images. Figure 2 As shown in (d), the fiber densification process was completed by sintering at 1400℃ for 7 minutes. The excessively long sintering time required for densification led to excessive grain growth, with a grain size reaching 230 nm. The measured tensile strength of the single filament of the densified fiber was 1.78 GPa. High-temperature stability was characterized by holding the fiber at 1200℃ for 1-100 hours and observing the morphology of the fiber cross-section using SEM. The SEM image after high-temperature sintering is shown in the figure. Figure 3 As shown in (ad), the microstructure of 0% scandium oxide after 1-100 hours is shown. After 100 hours, the fiber microstructure is coarse and has poor high-temperature stability. At this time, the tensile strength of the single filament is only 0.73 GPa.

[0064] Example 1 (High-temperature sintering of alumina-zirconia multiphase fibers with 1% scandium oxide at 1400℃ / 1min)

[0065] Steps 1-6 are the same as in Comparative Example 1;

[0066] 7) Dissolve 18.08g of scandium nitrate pentahydrate in an appropriate amount of deionized water. (SC2O3 content is 1wt% Al2O3)

[0067] Steps 8-11 are the same as steps 7-10 in Comparative Example 1;

[0068] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. Dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, yielding pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. The high-temperature sintering process employed a two-step method: holding at 1000℃ for 10 min, followed by holding at 1400℃ for 1 min, to obtain alumina-zirconia composite fiber ceramics.

[0069] XRD analysis of the fibers revealed no other phase formation. The resulting scandium oxide-added alumina-zirconia multiphase ceramic fibers had a diameter of 10-12 μm, and their appearance was as follows. Figure 2 As shown in (i), the fiber was sintered at 1400℃ for 1 min. The fiber structure was not fully dense, with many pores, resulting in poor mechanical properties. Tensile testing could not be performed to measure fiber properties, failing to meet testing requirements, and the room temperature performance was too poor. The sintering time was too short, and the fiber was not dense enough.

[0070] Example 2 (Alumina-zirconia multiphase fiber with 1% scandium oxide added, 1400℃ / 3min)

[0071] Steps 1-11 are the same as in Example 1.

[0072] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. Dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. The high-temperature sintering process employed a two-step method: holding at 1000℃ for 10 min, followed by holding at 1400℃ for 3 min, to obtain alumina-zirconia composite fiber ceramics.

[0073] The obtained scandium oxide-added alumina-zirconia multiphase ceramic fibers had a diameter of 9-11 μm, and the measured tensile strength of the single filaments was 1.99 GPa. The fiber appearance is as follows... Figure 2 As shown in (j), the fibers formed a dense structure; XRD analysis revealed no other phases. High-temperature stability testing was performed, with the fibers incubated at 1200℃ for 1-100 hours, and the morphology of the fiber cross-section was observed using SEM. Figure 3(il), SEM results after high-temperature service show that the fiber structure maintains a good morphology from 1h to 100h, with no coarse grains formed at 100h, indicating good high-temperature stability. After 100h service at 1200℃, the average alumina grain size in the product is 300nm. (After 100h service at 1200℃, the tensile strength of the product is 1.75GPa, with a strength retention rate of 88%, indicating good high-temperature stability).

[0074] Example 3 (Alumina-zirconia multiphase fiber with 1% scandium oxide added, 1400℃ / 5min)

[0075] Steps 1-11 are the same as in Example 1.

[0076] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. Dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. The high-temperature sintering process employed a two-step method: holding at 1000℃ for 10 min, followed by holding at 1400℃ for 5 min, to obtain alumina-zirconia composite fiber ceramics.

[0077] The obtained scandium oxide-added alumina-zirconia multiphase ceramic fibers had a diameter of 9-11 μm, and the measured tensile strength of the single filament was 1.80 GPa. The fiber appearance is as follows... Figure 2 As shown in (k); XRD testing of the fiber revealed no other phase formation. Driven by heat, the fiber grains continued to grow, resulting in excessively large grains and some intergranular gaps. Compared to Example 1, the fiber's microstructure and mechanical properties were somewhat reduced. After 100 hours of service at 1200°C, the alumina grain size in the product was 350 nm. (After 100 hours of service at 1200°C, the tensile strength of the product was 1.40 GPa, with a strength retention rate of 77.7%).

[0078] Example 4 (Alumina-zirconia multiphase fiber with 1% scandium oxide added, 1400℃ / 7min)

[0079] Steps 1-11 are the same as in Example 1.

[0080] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. Dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium-added alumina-zirconia multiphase ceramic fibers. The pre-sintering sintering regime was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. The high-temperature sintering process employed a two-step method: holding at 1000℃ for 10 min, followed by holding at 1400℃ for 7 min, to obtain alumina-zirconia composite fiber ceramics. The obtained scandium-added alumina-zirconia multiphase ceramic fibers had a diameter of 9-11 μm. XRD analysis of the fibers revealed no other phase formation. The measured tensile strength of the single filament was 1.72 GPa. The fiber appearance is shown below. Figure 2 As shown in (l) in the figure; driven by heat, the fiber grains continued to grow, and the excessive grain growth increased the intergranular gaps, resulting in a further reduction in the fiber's microstructure and mechanical properties compared to Example 1. After 100 hours of service at 1200°C, the alumina grain size in the product was 400 nm. (After 100 hours of service at 1200°C, the tensile strength of the product was 1.30 GPa, with a strength retention rate of 75.5%).

[0081] Comparative Example 2 (Alumina-zirconia multiphase fibers with 0% scandium oxide addition, 1400℃ / 7min) (pre-sintering was performed by single-step sintering)

[0082] Steps 1-10 are the same as in Example 1.

[0083] 11. Sintering: The precursor fibers were pre-sintered by gradually heating to a set temperature to remove impurities such as water and PVP from the fibers, obtaining pre-sintered fibers. The pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia composite ceramic fibers. The pre-sintering sintering regime was 500℃, with a heating rate of 3℃ / min from room temperature to 500℃. High-temperature sintering involved sintering at 1000℃ for 10 min, followed by sintering at 1400℃ for 7 min, to obtain alumina-zirconia composite fiber ceramics. XRD analysis of the fibers revealed... Figure 1 As shown, no other phases were found to be generated. SEM observation revealed numerous pores in the fiber, and the surface contained some impurities. During high-temperature sintering, the grain growth was rapid due to the presence of defects, resulting in coarse grains. Mechanical testing revealed that the tensile strength of the fiber monofilament was only 1.36 GPa, a significant decrease compared to Comparative Example 1. This is because the sintering process was too rapid during pre-sintering, leading to incomplete removal of substances and the presence of impurities and defects within the fiber.

[0084] Example 5 (Alumina-zirconia multiphase fiber with 0.5% scandium oxide added, 1400℃ / 1min)

[0085] Steps 1-6 are the same as in Example 1.

[0086] 7) Dissolve 9.04g of scandium nitrate pentahydrate in an appropriate amount of deionized water. (SC2O3 content is 0.5wt% Al2O3)

[0087] Steps 8-12 are the same as steps 8-12 in Example 1;

[0088] The obtained scandium oxide-added alumina-zirconia multiphase ceramic fibers, with a diameter of 9-12 μm, showed no other phase formation upon XRD analysis. The fiber appearance and cross-sectional microstructure are shown below. Figure 2 As shown in (e), the fiber was sintered at 1400℃ for only 1 minute. The fiber structure had not yet completed the densification process and had not formed a dense structure. The fiber contained many pores, resulting in poor mechanical properties. Tensile testing could not be performed to measure the fiber's performance, and the test requirements were not met; the performance was too poor. The sintering time was too short.

[0089] Example 6 (Alumina-zirconia multiphase fiber with 0.5% scandium oxide added, 1400℃ / 3min)

[0090] Steps 1-11 are the same as in Example 5.

[0091] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. Dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, yielding pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia multiphase ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering was performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 3 min, resulting in alumina-zirconia composite fiber ceramics. The obtained alumina-added alumina-zirconia multiphase ceramic fibers had a diameter of 10-12 μm. The fiber appearance and cross-sectional microstructure are shown in the figure. Figure 2As shown in (f), the fiber was sintered at 1400℃ for 3 min. The fiber grains completed the growth and merging process, but due to insufficient sintering time, the densification process was not completely completed, resulting in small pores and some intergranular gaps. XRD testing of the fiber revealed no other phase formation. A single-filament tensile test was conducted, yielding a tensile strength of 1.56 GPa. Compared to Example 2, the mechanical properties decreased significantly, and the fiber grain size was larger. After 100 h of service at 1200℃, the alumina grain size in the product was 400 nm. (After 100 h of service at 1200℃, the tensile strength of the product was 1.08 GPa, with a strength retention rate of 69.2%).

[0092] Implementation Case 7 (Alumina-zirconia multiphase fiber with 0.5% scandium oxide added, 1400℃ / 5min)

[0093] Steps 1-11 are the same as in Example 5.

[0094] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. First, dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, yielding pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering was performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 5 min, resulting in alumina-zirconia composite fiber ceramics.

[0095] The resulting alumina-zirconia composite ceramic fibers, with a diameter of 9-12 μm, are shown in the following images: (The images are not provided in the original text.) Figure 2 As shown in (g). The fiber was sintered at 1400℃ for 5 min, during which the fiber grains completed the densification process, forming a dense structure without obvious defects. XRD analysis of the fiber revealed no other phase formation. A monofilament tensile test was conducted, yielding a tensile strength of 1.80 GPa. High-temperature stability testing was performed, holding the fiber at 1200℃ for 1-100 h, and the morphology of the fiber cross-section was observed using SEM. Figure 3 (eh), SEM results after high-temperature sintering show that the fiber structure in the range of 1h-100h is still relatively good at 1h and 10h, but at 50h and 100h, the grains grow abnormally, producing coarse grains, and the mechanical properties of the fiber drop rapidly.

[0096] Compared to Example 2, the mechanical properties are improved due to the completion of densification. However, compared to Example 2, the fibers with 1% scandium oxide added exhibit superior mechanical properties upon reaching densification compared to those with 0.5% scandium oxide added, with better grain size and microstructure. Furthermore, the sintering time required to achieve densification for the 1% scandium oxide-added fibers is shorter than that for the 0.5% added fibers. Comparing the results after long-term high-temperature heat treatment, the microstructure and mechanical properties of the 0.5% scandium oxide-added fibers are superior to those without, but significantly inferior to the 1% added fibers, with much lower grain size and mechanical properties. After 100 hours of service at 1200℃, the alumina grain size in the product is 500 nm (after 100 hours of service at 1200℃, the tensile strength of the product is 1.26 GPa, with a strength retention rate of 70.0%).

[0097] Implementation Case 8 (Alumina-zirconia multiphase fiber with 0.5% scandium oxide added, 1400℃ / 7min)

[0098] Steps 1-11 are the same as in Example 5.

[0099] 12. Sintering: The precursor fibers underwent a two-stage pre-sintering process. First, dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, yielding pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering was performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 7 min, resulting in alumina-zirconia composite fiber ceramics.

[0100] The resulting alumina-zirconia composite ceramic fibers, with a diameter of 9-12 μm, are shown in the cross-sectional micrographs below. Figure 2 As shown in (h). After densification, the fiber grains continued to grow due to thermal drive, resulting in coarse grains and a decrease in mechanical properties. XRD testing of the fiber revealed no other phase formation. Monofilament tensile testing showed that the fiber's mechanical properties were 1.68 GPa, a decrease compared to Example 7, but still an improvement compared to Example 6 where densification was incomplete. Compared to Example 4, which was sintered at 1400℃ for 7 min with 1% addition, the mechanical properties were still lower. The overall performance of the fiber with 1% addition was superior to that with 0.5% addition. After 100 h of service at 1200℃, the alumina grain size in the product was 500 nm (after 100 h of service at 1200℃, the tensile strength of the product was 1.20 GPa, with a strength retention rate of 71.4%).

[0101] Implementation Case 9 (Alumina-zirconia multiphase fiber with 3% scandium oxide, 1400℃ / 1min)

[0102] Steps 1-6 are the same as in Comparative Example 1.

[0103] 7) Dissolve 54.24g of scandium nitrate pentahydrate in an appropriate amount of deionized water. (SC2O3 accounts for 3wt% of Al2O3)

[0104] Steps 8-12 are the same as steps 8-12 in Example 1.

[0105] The resulting alumina-zirconia composite ceramic fibers, with a diameter of 9-12 μm, are shown in the following images: (The images are not provided in the original text.) Figure 2 As shown in (m), due to the short sintering time, the fiber grains were not fully densified, but significant grain growth and merging were observed. However, the merging was incomplete, and numerous pores remained. XRD analysis of the fiber revealed no other phase formation. A monofilament tensile test was performed, and the Webuill tensile strength of the fiber was measured to be 1.35 GPa. Because the fiber was not fully densified, its performance did not meet practical application requirements and was considered poor.

[0106] Implementation Case 10 (Alumina-zirconia multiphase fiber with 3% scandium oxide added, 1400℃ / 5min)

[0107] Steps 1-11 are consistent with steps 1-11 in Implementation Case 9.

[0108] 12) Sintering: The precursor fibers undergo a two-stage pre-sintering process. First, dehydration is achieved through slow, gradual heating at a low temperature, followed by progressively accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers are then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature is 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering is performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 5 min, yielding alumina-zirconia composite fiber ceramics.

[0109] The resulting alumina-zirconia composite ceramic fibers, with a diameter of 9-12 μm, are shown in the cross-sectional micrographs below. Figure 2As shown in (n), intergranular gaps still exist in the fiber structure, and a dense structure has not been formed. XRD testing of the fiber revealed no other phase formation. A single-filament tensile test was performed, yielding a Weibull strength of 1.70 GPa. After 100 hours of service at 1200℃, the alumina grain size in the product was 490 nm (after 100 hours of service at 1200℃, the tensile strength of the product was 1.32 GPa, with a strength retention rate of 77.6%).

[0110] Implementation Case 11 (Alumina-zirconia multiphase fiber with 3% scandium oxide added, 1400℃ / 6min)

[0111] Steps 1-11 are consistent with steps 1-11 in Implementation Case 9.

[0112] 12) Sintering: The precursor fibers undergo a two-stage pre-sintering process. First, dehydration is achieved through slow, gradual heating at a low temperature, followed by progressively accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers are then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature is 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering is performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 6 min, yielding alumina-zirconia composite fiber ceramics.

[0113] The resulting alumina-zirconia composite ceramic fibers, with a diameter of 9-12 μm, are shown in the following images: (The images are not provided in the original text.) Figure 2 As shown in (o), the fiber structure has completed the densification process. XRD analysis of the fiber revealed no other phase formation. Monofilament tensile testing yielded a Weibull strength of 1.87 GPa. High-temperature stability testing was performed, with the fiber held at 1200℃ for 1-100 hours, and the morphology of the fiber cross-section was observed using SEM. Figure 3 (mp) SEM results after high-temperature sintering showed that the fiber structure maintained a good morphology from 1h to 100h and from 1h to 50h. During the 100h long-term holding period, abnormal grain growth occurred, forming coarse grains, but the morphology was still relatively good, superior to fibers with 0% and 0.5% added scandium oxide. After 100h of service at 1200℃, the alumina grain size in the product was 450nm (the tensile strength of the product after 100h of service at 1200℃ was 1.48GPa, with a strength retention rate of 79.1%).

[0114] Example 12 (Alumina-zirconia multiphase fiber with 3% scandium oxide added, 1400℃ / 7min)

[0115] Steps 1-11 are consistent with steps 1-11 in Implementation Case 9.

[0116] 12) Sintering: The precursor fibers undergo a two-stage pre-sintering process. First, dehydration is achieved through slow, gradual heating at a low temperature, followed by progressively accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers are then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia composite ceramic fibers. The pre-sintering temperature is 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering is performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 7 min, yielding alumina-zirconia composite fiber ceramics.

[0117] The resulting alumina-zirconia composite ceramic fibers, with a diameter of 9-12 μm, are shown in the following images: (The images are not provided in the original text.) Figure 2 As shown in (p). XRD testing of the fiber revealed no other phase formation, indicating a dense fiber structure with some grains agglomerating and coalescing, resulting in the appearance of some coarse grains. Monofilament tensile testing yielded a fiber strength of 1.78 GPa. After 100 hours of service at 1200℃, the alumina grain size in the product was 480 nm (the tensile strength of the product after 100 hours of service at 1200℃ was 1.32 GPa, with a strength retention rate of 74.1%).

[0118] Example 13 (One-step concentration, 1% added at 1400 °C / 3 min)

[0119] Steps 1-7 are the same as in Example 2.

[0120] Step 8) Concentration: The homogeneous mixture after stirring is distilled using a rotary evaporator to concentrate most of the water (6500g of water). The remaining liquid is then poured into a small rotary evaporator for final concentration. (The initial concentration temperature is 50 degrees Celsius, and the rotation speed is 40 r / min; the same temperature and rotation speed are then used for further concentration until concentration is complete. This is a one-step concentration without changing the concentration temperature and rotation speed. The concentration time is approximately 2 hours. Concentration is stopped when the fiber reaches a spinnable viscosity; at this point, the gel viscosity is 80 Pa / s.)

[0121] 9) Dry spinning; The concentrated gel from step 8 is dry spun to obtain gel precursor fibers. During dry spinning, the spinning kettle temperature is controlled as follows: 50℃; spinneret orifice diameter: 80μm; duct length: 3m; duct temperature: 140℃; winding machine take-up rate: 80r / min.

[0122] 10) Sintering: The precursor fibers were pre-sintered to remove water, PVP, acids, and other impurities, yielding pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia multiphase ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 400℃, and 0.6℃ / min from 400℃ to 500℃. The high-temperature sintering process employed a two-step method: holding at 1000℃ for 10 min, followed by holding at 1400℃ for 3 min. The resulting scandium oxide-added alumina-zirconia multiphase ceramic fibers had a diameter of 10-13 μm, and the measured tensile strength of a single filament was 1.58 GPa. The fibers exhibited some pores and impurities; XRD analysis revealed no other phase formation. High-temperature stability tests were conducted. After 100 hours of service at 1200℃, the tensile strength of the product was 1.36 GPa, with a strength retention rate of 86.0%, indicating good high-temperature stability. The main reason for this phenomenon is that the concentration process was not segmented; the concentration temperature and rotation speed at the rear end were not reduced, resulting in excessively rapid concentration and water removal. This increased viscosity, coupled with the failure to reduce the concentration speed, led to the presence of numerous air bubbles and impurities in the spinning precursor. Consequently, some porosity remained in the fiber after high-temperature sintering. However, the good high-temperature stability is attributed to the grain growth during the long-term high-temperature sintering process, which filled the defects. Furthermore, the addition of scandium oxide further promoted high-temperature stability, resulting in good overall stability.

[0123] Example 14 (1% added, but spinning conditions were changed)

[0124] Other conditions are the same as in Example 2, except that: the spinning kettle temperature is controlled at 50°C; the spinneret orifice diameter is 80μm; the tunnel length is 3m; the tunnel temperature is 120°C; and the winding machine take-up rate is 60r / min.

[0125] After being kept at 1200℃ for 100 hours, the product had a tensile strength of 1.56 gPa and a strength retention rate of approximately 78.4%, indicating good high-temperature stability.

[0126] Comparative Example 3 (Alumina-zirconia multiphase fibers with 5% added scandium oxide)

[0127] Steps 1-6 are the same as in Comparative Example 1.

[0128] 7) Dissolve 90.40g of scandium nitrate pentahydrate in an appropriate amount of deionized water. (SC2O3 accounts for 5wt% of Al2O3)

[0129] Steps 8-11 are the same as in Implementation Case 1.

[0130] Sintering: 12) Sintering: The precursor fibers were pre-sintered in two stages. Dehydration was achieved by slow heating at a low temperature, followed by gradually accelerating heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. The pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium oxide-added alumina-zirconia multiphase ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering was performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 1 min, 3 min, 5 min, and 7 min respectively for four groups of samples. Four groups of fibers with 5% scandium oxide were obtained.

[0131] XRD tests on the fibers revealed the presence of phases other than Al₂O₃ and ZrO₂, specifically Zr₅SC₂O. 13 This process involves the formation of a three-phase structure with Al2O3 and ZrO2, altering the phase composition of the alumina-zirconia multiphase fiber. This altered phase composition contradicts the original product design intent, resulting in poor performance in both room temperature and high-temperature stability tests. After 100 hours of service at 1200℃, the fiber structure became coarse, with the average alumina size reaching 550 nm, and the fiber performance after high temperature was below 1.0 GPa.

[0132] Comparative Example 4 (Alumina-zirconia multiphase fibers with 7% added scandium oxide)

[0133] Steps 1-6 are the same as in Comparative Example 1.

[0134] 7) Dissolve 126.5g of scandium nitrate pentahydrate in an appropriate amount of deionized water. (SC2O3 accounts for 7wt% of Al2O3)

[0135] Steps 8-11 are the same as in Implementation Case 1.

[0136] 12) Sintering: The precursor fibers underwent a two-stage pre-sintering process. First, dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium-added alumina-zirconia multiphase ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering was performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 1 min, 3 min, 5 min, and 7 min respectively for four groups of samples. This yielded four groups of fibers with 5% scandium oxide addition.

[0137] XRD tests on the fibers revealed that, in addition to Al2O3 and ZrO2, two other phases were present in the XRD results. Relative to 5%, the fibers contained not only Zr5SC2O... 13 And Zr3Sc4O 12 This altered the phase composition of the alumina-zirconia multiphase fiber. After the product was kept at 1200℃ for 100 hours, the alumina grain size in the product was 600nm (after being kept at 1200℃ for 100 hours, the tensile strength of the product could not be tested due to its low tensile strength).

[0138] Comparative Example 5 (Alumina-zirconia multiphase fibers with 10% added scandium oxide)

[0139] Steps 1-6 are the same as in Comparative Example 1.

[0140] 7) Dissolve 180.8g of scandium nitrate pentahydrate in an appropriate amount of deionized water. (SC2O3 content is 10wt% Al2O3)

[0141] Steps 8-11 are the same as in Implementation Case 1.

[0142] 12) Sintering: The precursor fibers underwent a two-stage pre-sintering process. First, dehydration was achieved through slow, low-temperature heating, followed by gradually accelerated heating to remove PVP, acids, and other impurities from the fibers, resulting in pre-sintered fibers. These pre-sintered fibers were then subjected to high-temperature sintering to obtain scandium-added alumina-zirconia multiphase ceramic fibers. The pre-sintering temperature was 500℃, with heating rates of 2℃ / min from room temperature to 100℃, 1℃ / min from 100℃ to 250℃, and 0.6℃ / min from 250℃ to 500℃. High-temperature sintering was performed at 1000℃ for 10 min, followed by sintering at 1400℃ for 1 min, 3 min, 5 min, and 7 min respectively for four groups of samples. This yielded four groups of fibers with 5% scandium oxide addition.

[0143] XRD analysis of the fibers revealed the presence of a phase other than Al₂O₃ and ZrO₂, specifically Zr₃Sc₄O₁₂, altering the phase composition of the alumina-zirconia multiphase fibers. Figure 1 The data shows that the product performance is too low to undergo testing and high-temperature stability testing.

[0144] Comparative Example 6 (0% scandium oxide added, and the ratio of alumina to zirconium oxide was adjusted to increase the zirconium oxide content to 50%)

[0145] Steps 1-5 are the same as in Comparative Example 1, with the amount of aluminum sol added remaining unchanged.

[0146] Step 6) Take 188g of yttrium nitrate hexahydrate (10wt% Al2O3), add an appropriate amount of deionized water, and stir to dissolve completely. Since the content of yttrium oxide accounts for 10% of zirconium oxide, and the ratio of aluminum oxide to zirconium oxide is 1:1, its content is increased to 10wt% Al2O3.

[0147] Step 7) Mixing and stirring: Take 6000g of aluminum sol prepared in steps 1 and 2, 2070g of zirconium acetate (Aladdin), iron sol prepared in step 4, PVP solution prepared in step 5, and yttrium nitrate solution prepared in step 6, and pour them into a glass concentration bottle for stirring. Mix for 24 hours to form a uniform mixture.

[0148] Steps 8-11 are the same as in Comparative Example 1.

[0149] XRD analysis of the fibers revealed that the phase composition remained unchanged, consisting of zirconium oxide and alumina. However, the increased zirconium oxide content resulted in a poor fiber microstructure, with numerous pores and excessively large grain sizes; the resulting alumina-scandium oxide composite ceramic fibers had a diameter of 13-15 μm. Simultaneously, monofilament tensile testing revealed low tensile strength, making further testing impossible. Furthermore, the high porosity of the fibers resulted in poor performance, hindering high-temperature stability testing.

Claims

1. A scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber, characterized in that: In the fiber composite ceramic fiber, by mass percentage, scandium oxide is 0.1-3%, preferably 0.8-1.2%, zirconium oxide is 8-9.5%, preferably 8.8-9.2%, and the balance is alumina. The alumina grain size is 150-200nm, the zirconium oxide grains at the grain boundaries are 40-80nm, and the zirconium oxide grains within the grains are 5-20nm.

2. The scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 1, characterized in that: The mass ratio of Sc to Zr in the fiber composite ceramic fiber is 1:8-15, preferably 1:9-11, and more preferably 1:

10.

3. The scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 1, characterized in that: After being kept at 1200℃ for 100 hours in air and then cooled to room temperature, the alumina grain size in the product is less than or equal to 0.33 micrometers.

4. A method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber as described in any one of claims 1-3, characterized in that: Includes the following steps, Step 1: Mixing According to the designed proportions, aluminum sol, zirconium acetate, iron sol, PVP solution, yttrium nitrate solution, and scandium nitrate solution are mixed evenly to obtain a mixture. Step Two: Concentration The mixture is stirred at 35-65℃, preferably 40-60℃, and concentrated in at least two steps to a viscosity of 10-100 Pa / s to obtain a spinning gel. Step 3: Spinning The obtained gel was dry-spun to obtain gel precursor fibers. During dry spinning, the spinning kettle temperature was controlled at 40-60℃; the spinneret orifice diameter was 70-90μm; the channel length was 3m; the channel temperature was 120-160℃; and the winding machine take-up rate was 60-90r / min. Step Four The gel precursor fiber is placed in a sintering device and pre-sintered at 450-550℃ for at least 60 minutes, then sintered at 1000℃ for 8-12 minutes, and then sintered at 1395-1405℃ for 60-420 seconds.

5. The method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 4, characterized in that: Aluminum sol is prepared using the sol-gel method, which includes the following steps: Add 6000ml of deionized water to a reaction vessel kept at 80℃ and start stirring. Then add 470g of formic acid and 540g of glacial acetic acid to the deionized water and stir. Then add 400g of aluminum powder with a particle size of 1-3um in at least three portions, one hour apart, to the reaction vessel and react fully with the formic acid and acetic acid. Mix and stir for at least 24 hours. During the reaction, 2wt% dilute nitric acid was added dropwise as a reaction aid. After the aluminum powder was added, 1100g of 2wt% dilute nitric acid was added into the reaction vessel through a separatory funnel. After the reaction is complete, stop stirring and heating. After the liquid in the reactor cools to room temperature, filter it to obtain aluminum sol.

6. The method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 4, characterized in that: Iron sol is prepared by the following steps: Take 110g of ferric nitrate nonahydrate according to the proportion, add it to 2550ml of deionized water, keep it warm in a water bath at 70℃ and stir, while adding a solution made of 54g of ammonium bicarbonate and 540g of deionized water dropwise at a rate of 1-3 drops per second; after the addition is complete, keep it warm in the water bath for at least 1 hour to complete the preparation of the iron sol, and then stop heating and stirring. Iron sol is used as a nucleating agent to promote the nucleation of alumina and zirconium oxide crystals, and at the same time promotes grain refinement. The addition ratio is 1%-5%, and the optimal addition amount is 4%, which is 4% of the solid content of alumina.

7. The method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 4, characterized in that: Add 27g of PVP to 270g of deionized water according to the ratio, keep warm and stir in a 40℃ water bath for 1 hour, then stop heating and stirring. The PVP solution is now ready.

8. The method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 4, characterized in that: Take yttrium nitrate hexahydrate according to the ratio, add an appropriate amount of deionized water, stir until fully dissolved, and obtain a homogeneous yttrium nitrate solution.

9. The method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 4, characterized in that: Take the appropriate proportion of scandium nitrate pentahydrate, add an appropriate amount of deionized water, stir evenly, and dissolve completely to obtain a uniformly mixed scandium nitrate solution.

10. The method for preparing scandium oxide-modified alumina-zirconia high-temperature resistant composite ceramic fiber according to claim 4, characterized in that: Concentration is achieved through preliminary concentration and final concentration. During preliminary concentration, the temperature is controlled at 50~60℃ and the rotation speed is 5~40r / min, removing 70~80% of the water. Then, the temperature is lowered to 40℃-45℃ and the rotation speed is increased to 45~80r / min. Until a spinning gel with a viscosity of 10-100 pa / s is obtained.

Citation Information

Patent Citations

  • Continuous alumina-zirconia composite ceramic fiber and preparation method thereof

    CN117702306A