Composite membrane for high-temperature proton exchange membrane fuel cell as well as preparation method and application of composite membrane
By employing a three-dimensional network structure with covalent cross-linking and hydrogen bonding in a high-temperature proton exchange membrane fuel cell, the problems of insufficient mechanical strength and phosphoric acid retention in traditional membranes have been solved, achieving high proton conductivity and long-term stability, thus advancing the commercial application of fuel cells.
Patent Information
- Application Number
- CN202610012835.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-07
- Publication Date
- 2026-05-01
AI Technical Summary
While the phosphoric acid-doped polybenzimidazole membrane in traditional high-temperature proton exchange membrane fuel cells improves proton conductivity, it suffers from insufficient mechanical strength and phosphoric acid retention capacity, leading to membrane electrode assembly failure and rapid battery performance degradation, thus hindering its commercialization.
A three-dimensional network structure with synergistic effects of covalent crosslinking and hydrogen bonding is adopted. A dense covalent crosslinking network is formed by chloromethylated polysulfone (CMPSF) and polybenzimidazole (OPBI), and nitrogen-rich ion polymer (NIP) is introduced as a functional additive to form a strong hydrogen bond network to anchor phosphoric acid and broaden the proton transport channel.
It significantly enhances the mechanical strength and phosphate retention capacity of the membrane, while improving proton conductivity and long-term operational stability, thereby improving the output performance and lifespan of the fuel cell.
Smart Images

Figure CN121964736A_ABST
Abstract
Description
A composite membrane for high-temperature proton exchange membrane fuel cells, its preparation method and application Technical Field
[0001] This invention belongs to the field of fuel cell material technology, specifically relating to a proton exchange membrane for high-temperature proton exchange membrane fuel cells (HT-PEMFC), and more particularly to a composite membrane with high proton conductivity, excellent mechanical strength and good durability through covalent and hydrogen bond synergistic crosslinking, and its preparation method. Background Technology
[0002] High-temperature proton exchange membrane fuel cells (PEMFCs) have attracted widespread attention due to their high energy conversion efficiency, simplified hydrothermal management system, and lower requirements for hydrogen purity. Among them, phosphoric acid (PA)-doped polybenzimidazole (PBI) membranes are currently the most mainstream electrolyte material. Their proton conduction mainly relies on the Grotthuss mechanism under anhydrous conditions, i.e., protons are transported by jumping along a continuous hydrogen bond network. Proton conductivity is directly related to the phosphoric acid doping level (ADL) of the membrane.
[0003] However, traditional PA / PBI membranes face two major challenges: First, while high ADL can improve conductivity, the plasticizing effect of phosphoric acid can severely damage the mechanical strength and dimensional stability of the membrane, leading to the failure of the membrane electrode assembly. Second, during long-term operation, phosphoric acid is easily lost from the membrane, causing a decrease in proton conductivity and rapid degradation of battery performance, which seriously restricts the commercialization process of HT-PEMFC.
[0004] To improve the overall performance of PA / PBI membranes, existing technologies mainly focus on two directions: first, introducing physical fillers such as inorganic nanoparticles (e.g., BN, SiO2), metal-organic frameworks (MOFs), or covalent organic frameworks (COFs) to enhance phosphate retention; and second, improving mechanical stability through chemical crosslinking (e.g., using epoxy resins or multifunctional crosslinking agents). However, these methods often struggle to improve one aspect of performance without compromising the other. For example, enhanced crosslinking may restrict polymer chain movement, hindering proton conduction; while simply introducing adsorbent materials may contribute little to mechanical strength and is prone to phase separation.
[0005] Therefore, developing a composite membrane structure that can synergistically improve proton conductivity, mechanical strength, and phosphate retention capacity is a technical problem that urgently needs to be solved in this field.
[0006] Based on the above reasons, this application is hereby submitted. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a composite membrane for high-temperature proton exchange membrane fuel cells and its preparation method. This composite membrane, by constructing a three-dimensional network structure with synergistic effects of covalent cross-linking and hydrogen bonding, significantly enhances mechanical strength and suppresses excessive swelling and phosphate loss while maintaining a high level of phosphate doping, thereby achieving high proton conductivity and long-term operational stability.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: 1. Composition of the composite membrane: The composite membrane uses polybenzimidazole (OPBI) as a matrix and simultaneously contains chloromethylated polysulfone (CMPSF) and nitrogen-rich ion polymer (NIP). CMPSF acts as a covalent crosslinking agent, and its chloromethyl (-CH2Cl) undergoes a nucleophilic substitution reaction with the imidazole group (-NH-) on the OPBI molecular chain to form a dense three-dimensional covalent crosslinking network, which is the structural basis for the membrane's high mechanical strength and excellent dimensional stability. NIP acts as a functional additive, and the basic nitrogen atoms (such as imidazolium and triazine nitrogen) abundant in its molecular structure can serve as strong Lewis base sites. On the one hand, they form strong acid-base interactions and hydrogen bond networks with phosphate molecules, effectively anchoring phosphate and enhancing its absorption and retention capacity; on the other hand, these nitrogen sites themselves can also serve as "transfer stations" for proton hopping, broadening and connecting proton transport channels and promoting Grothuss conduction.
[0009] 2. Key component characteristics: (1) The degree of chloromethylation of CMPSF is preferably 0.1 to 1.5, which is adjusted by controlling the reaction time (e.g., 36, 48, 60 hours). The appropriate degree of chloromethylation ensures sufficient crosslinking point density to build a stable network. The mass ratio of CMPSF in the composite membrane is 1%-30%.
[0010] (2) NIP was prepared via a two-step method. First, a 2,4,6-tris(1H-imidazol-1-yl)-1,3,5-triazine (TIT) precursor was synthesized, and then it was subjected to a quaternization polymerization reaction with α,α'-dichloro-p-xylene to form a nitrogen-rich polymer network with three-dimensional crosslinking potential. The amorphous structure of NIP is beneficial to its uniform dispersion and good compatibility in the OPBI matrix.
[0011] 3. A method for preparing a composite membrane, comprising the following steps: (1) uniformly dispersing a predetermined mass of NIP powder in N-methyl-2-pyrrolidone (NMP) solvent.
[0012] Add predetermined amounts of CMPSF and OPBI to the above dispersion and stir continuously at room temperature (e.g., for 12 hours) until a uniform and stable casting solution is formed. Pour the casting solution onto a clean substrate such as a glass plate, and control the thickness using a doctor blade.
[0013] (2) Place the substrate with the liquid film on a hot plate and dry it at a lower temperature (e.g., 80 °C) for a period of time to slowly remove most of the solvent and prevent skin formation on the surface; then dry it at a higher temperature (e.g., 120 °C) for a period of time. This process not only completely removes the residual solvent, but also promotes the full crosslinking reaction between CMPSF and OPBI, and finally obtains a dense and flat composite film.
[0014] 4. By optimizing the addition ratio of CMPSF to NIP (e.g., 10 wt% CMPSF and 10 wt% NIP), the resulting composite film exhibits excellent overall performance under a phosphoric acid doping level of approximately 396%: a proton conductivity as high as 163.44 mS / cm at 160 °C in anhydrous conditions. -1 The tensile strength was increased to 10.04 MPa, far exceeding that of pure OPBI film (approximately 5.3 MPa); when assembled into a single cell for testing, the peak power density reached 1001.7 mW / cm². -2 In addition, the membrane also exhibits excellent antioxidant stability (high mass retention after 96 hours in Fenton's reagent at 80 °C) and long-term phosphoric acid retention (it can still retain most of the phosphoric acid after 100 hours in dry hot air at 160 °C).
[0015] Compared with the prior art, the present invention has the following significant advantages: (1) It creatively combines the covalent crosslinking of CMPSF with the hydrogen bond network of NIP. Covalent crosslinking provides a rigid framework to ensure mechanical integrity; the abundant nitrogen sites of NIP "lock" phosphate through strong hydrogen bonds and construct efficient proton channels. The two work together to achieve the unity of "strong framework" and "high conductivity".
[0016] (2) The composite membrane of the present invention successfully breaks the “trade-off” effect between the properties of traditional PA / PBI membranes, and obtains high proton conductivity, high mechanical strength, low swelling rate, excellent phosphoric acid retention and antioxidant stability, which are difficult to achieve by a single modification method.
[0017] (3) The preparation process is based on the mature solution casting method. The raw materials are readily available, the reaction conditions are mild, and no complicated equipment is required, making it suitable for large-scale production.
[0018] (4) The composite membrane significantly improves the output performance and operating life of HT-PEMFC, providing a key material solution for promoting the commercial application of high-temperature fuel cells. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 is a schematic diagram of the CMPSF synthesis of the present invention, illustrating the CMPSF chloromethylation step.
[0021] Figure 2 is a schematic diagram of NIP synthesis according to the present invention, illustrating the NIP synthesis steps.
[0022] Figure 3 shows the structural characterization of the materials. (a) PSF and CMPSF-0.34 1 (b) H NMR spectra of CMPSF-0.66 and CMPSF-1.18 1 (c) FT-IR spectrum of CMPSF. (d) XPS full-spectrum scan of NIP. (e) N1s XPS spectrum of NIP. (f) Cl 2p XPS spectrum of NIP.
[0023] Figure 4 shows the structural characterization of the composite membrane in the embodiment. (a) Surface SEM image of the OPBI membrane. (b) Cross-sectional SEM image of the OPBI membrane. (c) Surface SEM image of the OPBI / CI membrane. (d) Cross-sectional SEM image of the OPBI / CI membrane.
[0024] Figure 5 shows the performance characterization of the composite membrane in the examples. (a) Mechanical properties of the OPBI / CI membrane. (b) Phosphoric acid absorption and size swelling of the OPBI / CI membrane.
[0025] Figure 6 shows the performance characterization of the composite membrane in the examples. (a) Photographs of the membrane before and after dissolution in NMP. (b) Residual mass of the OPBI / CI membrane.
[0026] Figure 7 shows the performance characterization of the composite membrane in the examples. (a) Oxidative stability, (b) Phosphoric acid retention rate, and (c) TG curve.
[0027] Figure 8 shows the performance characterization of the composite membrane in the embodiment. (a) Proton conductivity of the OPBI / CI membrane. (b) Activation energy of the OPBI / CI membrane.
[0028] Figure 9 shows the performance characterization of the composite membrane in the embodiment. (a) Composed of OPBI membrane and OPBI / C 10% -I 10wt% Polarization curves of membrane-assembled fuel cells at 160°C. (b) OPBI membrane and OPBI / C10% -I 10wt% EIS spectra of the membrane. (c) Composed of OPBI membrane and OPBI / C 10% -I 10wt% Membrane-assembled fuel cells at 160°C and 200 mA cm⁻¹ -2 Stability test under the condition of running for 55 hours. Detailed Implementation
[0029] The present invention will be further described in detail below through implementation examples. These implementation examples are carried out based on the technology of the present invention. Detailed implementation methods and specific operating procedures are provided to illustrate the inventiveness of the present invention, but the scope of protection of the present invention is not limited to the following implementation examples.
[0030] Based on the information contained in this application, various modifications to the precise description of the invention can be readily made by those skilled in the art. It should be understood that the scope of the invention is not limited to the defined processes, properties, or components, as these embodiments and other descriptions are merely illustrative of specific aspects of the invention.
[0031] To better understand the invention and not to limit its scope, all figures indicating amounts, percentages, and other numerical values used in this application should, in all cases, be understood to be modified by the word "approximately." Therefore, unless otherwise stated, the numerical parameters listed in the specification are approximate values and may vary depending on the desired properties being sought. Each numerical parameter should at least be considered as obtained based on reported significant figures and through conventional rounding methods.
[0032] The equipment and raw materials used in this invention are all commercially available or commonly used in the field. Unless otherwise specified, the methods in the following embodiments are conventional methods in the field.
[0033] Example 1 This example describes a method for preparing a liquid electrolyte with a high flame-retardant two-component functional additive that enhances ion transport and interfacial stability. The method specifically includes the following steps: (1) Preparation of chloromethylated polysulfone (CMPSF) As shown in Figure 1, under argon protection, 10 g of polysulfone (PSF) was dissolved in 500 mL of chloroform, followed by the sequential addition of 6.79 g of paraformaldehyde and 28.8 mL of trichlorosilane; 0.525 mL of anhydrous tin tetrachloride was slowly added dropwise as a catalyst under vigorous stirring, and the reaction was carried out at 55°C for 48 hours; after the reaction was completed, the mixture was cooled to room temperature, and the reaction solution was poured into methanol to precipitate. The solid product was collected, washed three times with methanol and deionized water respectively, and dried under vacuum at 60°C to finally obtain white fibrous chloromethylated polysulfone (CMPSF). 1¹H NMR analysis showed that its chloromethylation degree was approximately 1.18.
[0034] (2) Preparation of the precursor TIT: The synthesis steps of the precursor TIT are shown in Figure 2a. 4.08 g of imidazole was dissolved in 30 mL of acetonitrile and heated to 70 °C with stirring to dissolve. Separately, 1.84 g of cyanuric chloride (TCCA) was dissolved in 30 mL of acetonitrile at 70 °C to obtain a clear solution. The TCCA solution was slowly added dropwise to the imidazole solution with stirring. After the addition was complete, the reaction was continued at 70 °C. After the reaction was completed, the solid was collected by filtration, washed successively with acetonitrile and deionized water, and finally dried under vacuum at 60 °C to obtain the pale yellow powder product TIT.
[0035] (3) Preparation of NIP The synthesis of NIP is shown in Figure 2b. 1.67 g (3 mmol) of TIT and 1.58 g (6 mmol) of α,α'-dichloro-p-xylene were added to a reaction flask containing 80 mL of acetonitrile. The mixture was stirred at 90 °C for 24 hours under nitrogen protection. After the reaction was complete, the mixture was filtered, the solid product was washed with acetonitrile, and dried under vacuum at 50 °C for 24 hours to obtain a pale yellow solid, NIP. Its chemical structure was confirmed by FT-IR and XPS analysis.
[0036] (4) OPBI / C 10% -I 5wt% Preparation and Performance of Composite Membrane: 0.85 g of OPBI, 0.1 g of CMPSF with a chloromethylation degree of 1.18, and 0.05 g of NIP were weighed as raw materials, and 20 g of N-methyl-2-pyrrolidone (NMP) was used as solvent. NIP was first ultrasonically dispersed in a portion of NMP, and then CMPSF and OPBI were added. The mixture was stirred at room temperature for 24 hours to obtain a uniform casting solution. After casting the solution into a film, it was subjected to a stepped heat treatment of drying at 80℃ for 5 hours and drying at 120℃ for 10 hours to complete the solvent removal and crosslinking reaction between CMPSF and OPBI.
[0037] In Example 2, 0.8 g of OPBI, 0.1 g of CMPSF with a chloromethylation degree of 1.18, and 0.1 g of NIP were weighed as raw materials, and 20 g of N-methyl-2-pyrrolidone (NMP) was used as solvent. NIP was first ultrasonically dispersed in a portion of NMP, and then CMPSF and OPBI were added. The mixture was stirred at room temperature for 24 hours to obtain a uniform casting solution. After casting the solution into a film, it was subjected to a step heat treatment of drying at 80°C for 5 hours and drying at 120°C for 10 hours to complete the solvent removal and crosslinking reaction between CMPSF and OPBI.
[0038] In Example 3, 0.75 g of OPBI, 0.1 g of CMPSF with a chloromethylation degree of 1.18, and 0.15 g of NIP were weighed as raw materials, and 20 g of N-methyl-2-pyrrolidone (NMP) was used as solvent. NIP was first ultrasonically dispersed in a portion of NMP, and then CMPSF and OPBI were added. The mixture was stirred at room temperature for 24 hours to obtain a uniform casting solution. After casting the solution into a film, it was subjected to a step heat treatment of drying at 80°C for 5 hours and drying at 120°C for 10 hours to complete the solvent removal and crosslinking reaction between CMPSF and OPBI.
[0039] The microstructure characterization of composite membranes is crucial for maintaining high mechanical strength and reducing fuel permeation. This directly affects the efficiency and durability of fuel cells. Figures 4a-d show the differences between pure OPBI membranes and OPBI / C membranes. 10% -I 10wt% Surface and cross-sectional images of the composite membrane. The pure OPBI membrane has a smooth, dense, and defect-free surface, and its fracture surface is uniform and dense without obvious pores. As shown in Figure 4c, NIP particles are uniformly dispersed in the OPBI / CI composite membrane. In particular, no obvious phase separation phenomenon was observed between the NIP particles and the OPBI polymer matrix, indicating that NIP and the OPBI matrix have excellent compatibility. Figure 4d shows that the cross-sectional morphology of the OPBI / CI composite membrane is similar to that of the pure OPBI membrane, exhibiting a completely dense structure.
[0040] The mechanical tensile strength of the composite membrane is characterized as shown in Figure 5a. The mechanical strength of the composite membrane initially increases and then decreases with changing NIP content. OPBI / C 10% -I 5wt% The tensile strength of the membrane was 8.7 MPa, which is superior to that of the pure OPBI membrane (5.3 MPa). When the NIP content was 10 wt%, the tensile strength reached its optimal value of 10.04 MPa, demonstrating the best synergy between the CMPSF covalent network and the NIP reinforcement. When the NIP content was further increased to 15 wt%, the tensile strength decreased slightly to 9.1 MPa, possibly because the slight aggregation of excess NIP interfered with the continuity of the polymer matrix to some extent.
[0041] Characterization of Phosphoric Acid Doping Level and Swelling Properties of Composite Membranes Figure 5b shows the phosphoric acid doping level and swelling properties of the composite membranes. All three composite membranes exhibited good phosphoric acid adsorption capacity, but the swelling control effects differed significantly. OPBI / C 10% -I 5wt% The membrane's ADL is 389%, and its volume swelling ratio is 240%; the optimal OPBI / C 10% -I 10wt%While maintaining a high ADL (396%), the membrane significantly reduced its volume swelling ratio to approximately 210%; while OPBI / C 10% -I 15wt% The membrane's ADL was 375%, and the swelling ratio was further reduced to 195%. This indicates that the introduction of NIP effectively suppressed excessive swelling of the membrane while maintaining a high acid loading capacity, through its interaction with phosphoric acid and the matrix crosslinking network.
[0042] The solvent resistance of the composite membranes was characterized as shown in Figures 5a and 6b. The mass of the insoluble portion of the membrane samples was measured by immersing them in NMP at 80°C for 4 hours. All composite membranes containing CMPSF exhibited excellent solvent resistance. Three ratios of membranes (I...) 5wt% I 10wt% I 15wt% The gel fractions of the CMPSF and OPBI membranes were all above 75%, significantly higher than that of the completely dissolved pure OPBI membrane. This directly confirms that a robust three-dimensional covalent cross-linked network was successfully formed between CMPSF and OPBI, enabling the membrane to maintain its structural integrity in highly polar solvents.
[0043] The oxidative stability of the composite membrane was characterized as shown in Figure 7a. Fenton's reagent (3% H₂O₂, 4 ppm Fe) was used at 80℃. 2+ Accelerated oxidation tests were conducted on the membranes. After 96 hours of treatment, the mass retention rate of all OPBI / CI composite membranes was higher than that of pure OPBI membranes (73%), and the antioxidant performance gradually improved as the NIP content increased from 5 wt% to 10 wt%. At a NIP content of 15 wt%, the antioxidant performance remained at a high level, but the rate of improvement slowed down. The abundant basic nitrogen sites in NIP may have stabilized the polymer chains through hydrogen bonding and partially quenched free radicals, thereby enhancing the membrane's resistance to oxidative degradation.
[0044] The phosphoric acid loss rate of the composite membranes is characterized as shown in Figure 7b. An accelerated test of 100 hours was conducted in dry hot air at 160°C and 0% RH to evaluate the membrane's phosphoric acid retention capacity. The phosphoric acid retention rate of the pure OPBI membrane was only 71.96%. In contrast, the retention rates of all composite membranes were improved. Among them, OPBI / C... 10% -I 10wt% The membrane exhibited the highest retention rate, demonstrating the strong anchoring effect of the optimal NIP content on phosphate molecules. OPBI / C 10% -I 15wt% The membrane retention rate was slightly lower than that of the 10wt% sample, which may be related to the slight aggregation of NIPs causing some effective adsorption sites to be masked.
[0045] The thermal stability of the composite membranes was characterized as shown in Figure 7c. TGA analysis indicated that the main thermal decomposition stage of all composite membranes occurred between 300-450℃, corresponding to the degradation of the polymer backbone. Compared with pure OPBI, the decomposition initiation temperature and the temperature corresponding to the maximum weight loss rate of the composite membranes containing CMPSF and NIP were delayed, indicating that the introduced components enhanced the thermal stability of the membranes. The thermogravimetric curves of the three composite membranes with different NIP contents showed little difference and tended to flatten above 600℃, indicating that they have sufficient thermal stability at the typical operating temperature of HT-PEMFC (<200℃).
[0046] Characterization of the proton conductivity performance of the composite membrane. Figure 8a shows the proton conductivity performance of the composite membrane. The proton conductivity was tested at 160℃ under anhydrous conditions. OPBI / C 10% -I 5wt% OPBI / C 10% -I 10wt% OPBI / C 10% -I 15wt% The membrane conductivity was 138.2, 163.44, and 152.8 mS·cm, respectively. -1 Both were significantly higher than those of pure OPBI membrane (86.57 mS·cm). -1 The conductivity initially increases and then decreases with increasing NIP content, reaching a peak at 10 wt%. This is attributed to the fact that an appropriate amount of NIP provides optimal additional proton hopping sites and a continuous hydrogen bond network, while excessive NIP (15 wt%) may aggregate and hinder the connectivity of proton transport channels.
[0047] The activation energy of the composite membrane is shown in Figure 8b. The activation energy of proton conduction (E) was obtained by Arrhenius fitting. a E of pure OPBI membrane. a It is 7.01 kJ·mol -1 With the introduction of NIP, E a Significantly reduced, OPBI / C 10% -I 5wt% OPBI / C 10% -I 10wt% OPBI / C 10% -I 15wt% membrane E a The values were 4.25, 3.38, and 3.95 kJ·mol⁻¹, respectively. -1 The lowest E a The presence of NIP at a content of 10 wt% indicates that the membrane has the smoothest proton transport path and the lowest energy barrier, which is consistent with the membrane's highest proton conductivity.
[0048] Battery performance testing compares pure OPBI film with optimized OPBI / C film. 10% -I 10wt% The performance of the composite membrane fuel cell was tested using single-cell experiments. The corresponding polarization (IV) curves and power density curves are shown in Figure 9a. The open-circuit voltages of all membrane electrode assemblies were higher than 0.9 V, confirming that the membrane remained dense and defect-free after battery assembly. OPBI / C fuel cell with phosphoric acid doping was used. 10% -I 10wt% The membrane-assembled battery achieves a peak power density of 1001.7 mW / cm². -2 The value is significantly higher than that of the phosphoric acid-doped pure OPBI film (555.2 mW cm⁻¹). -2 ).
[0049] To further elucidate the interfacial and bulk charge transfer characteristics, electrochemical impedance spectroscopy (EIS) was performed. Figure 9b compares the OPBI film with OPBI / C. 10% -I 10wt% Nyquist plot of the composite membrane. The impedance curve of the composite membrane is significantly closer to the origin, indicating a significant reduction in its ohmic impedance and charge transfer impedance. This result reflects the performance of the OPBI / C... 10% -I 10wt% Composite membrane batteries exhibit more efficient ion conduction and superior interfacial kinetics. In contrast, pure OPBI membranes exhibit a larger semicircle, implying higher charge transfer impedance and relatively poor bulk conductivity. The reduced impedance of the composite membrane is consistent with its higher proton conductivity and power output.
[0050] At 160°C, 200 mA cm -2 Long-term durability was evaluated under high current density constant current operation conditions. As shown in Figure 9c, the battery voltage remained highly stable over 55 hours, exhibiting only slight fluctuations: an initial small increase followed by a slow decrease, with a total voltage decay rate of only 2%. Such minimal decay highlights the performance of OPBI / C. 10% -I 10wt% The membrane exhibits excellent operational stability under actual high-temperature fuel cell conditions. The good voltage retention rate further confirms the effectiveness of the crosslinked network and NIP in maintaining mechanical integrity, phosphate retention, and continuous proton conduction channels during long-term operation.
Claims
1. A composite proton exchange membrane for use in high-temperature proton exchange membrane fuel cells, characterized in that, include: (1) Polybenzimidazole (PBI) matrix; (2) Chloromethylated polysulfone (CMPSF), which forms a covalent cross-linked network by nucleophilic substitution reaction between chloromethyl and imidazole groups in PBI; (3) Nitrogen-rich ion polymer (NIP), which is dispersed in PBI matrix. The NIP is obtained by reacting a precursor containing triazine ring and imidazole ring with a dihalogenated cross-linking agent. Its nitrogen site forms hydrogen bonds with phosphoric acid to enhance the adsorption and retention of phosphoric acid.
2. The composite membrane according to claim 1, characterized in that, The degree of chloromethylation of the CMPSF is from 0.1 to 1.
5.
3. The composite membrane according to claim 1, characterized in that, The polybenzimidazole (PBI) is selected from one or more of OPBI, mPBI, pPBI, ABPBI, or other modified PBI.
4. A method for preparing the precursor 2,4,6-tris(1H-imidazol-1-yl)-1,3,5-triazine (TIT) for synthesizing the NIP of claim 3, characterized in that, The process includes the following steps: reacting imidazole with cyanuric chloride in an acetonitrile solution at 70-80℃, followed by precipitation, washing, and drying to obtain TIT.
5. The composite membrane according to claim 1, characterized in that, The NIP is obtained by quaternization reaction of 2,4,6-tris(1H-imidazol-1-yl)-1,3,5-triazine (TIT) with α,α'-dichloro-p-xylene.
6. The composite membrane according to claim 1, characterized in that, The CMPSF accounts for 1% to 25% of the mass of the composite membrane, and the NIP accounts for 1% to 25% of the mass of the composite membrane.
7. A method for preparing the composite membrane according to any one of claims 1 to 5, characterized in that, The process includes the following steps: (1) dispersing NIP in an organic solvent; (2) adding CMPSF and PBI and stirring until uniform to obtain a casting solution; (3) coating the casting solution onto a substrate and drying it by step heating to form a film.
8. The preparation method according to claim 6, characterized in that, The drying conditions are as follows: first dry at 80℃ for 3-8 hours, then dry at 100-140℃ for 8-15 hours.
9. The application fields of a composite proton exchange membrane for high-temperature proton exchange membrane fuel cells include fuel cells, flow batteries, water electrolysis for hydrogen production, etc.