Magnetic particles, magnetic particles for inspection, and method for producing magnetic particles
By preparing secondary particles with primary particles of a specific size and arranging a resin layer on the outside, the problem of insufficient magnetization of Fe3O4 particles in the prior art is solved, and the combination of superparamagnetism and high magnetization is achieved, which is suitable for rapid collection and separation in the biomedical field.
Patent Information
- Application Number
- CN202480057022.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-09-03
- Filing Date
- 2024-09-05
- Publication Date
- 2026-05-01
AI Technical Summary
Existing technologies struggle to maintain the superparamagnetism of Fe3O4 particles while simultaneously increasing their magnetization to enable rapid movement and transport applications in the biomedical field.
By preparing secondary particles with an average particle size of 500 nm or more and 5000 nm or less, primary particles with a particle size of 2 nm or more and 20 nm or less are aggregated, and a resin layer is arranged on the outside of the particles to form magnetic particles with superparamagnetism and high magnetization.
This technology enables the rapid collection and separation of magnetic particles in the biomedical field, improving work efficiency, especially in immunoassay applications in high-viscosity solutions.
Smart Images

Figure CN121970130A_ABST
Abstract
Description
Magnetic particles, magnetic particles for testing, and methods for manufacturing magnetic particles. Technical Field
[0001] This invention relates to magnetic particles, magnetic particles for testing, and methods for manufacturing magnetic particles. Background Technology
[0002] Magnetic particles containing Fe3O4 have been applied in the biomedical field, such as immunoassay, separation and purification of biomolecules, and drug delivery.
[0003] Fe3O4 particles used in such biomedical applications require high manipulability to external magnetic fields. The main magnetic properties of Fe3O4 particles closely related to this manipulability are remanent magnetization and saturation magnetization (hereinafter referred to as "magnetization"), and each magnetization depends on the particle size of each Fe3O4 particle.
[0004] To easily control the aggregation and dispersion of Fe3O4 particles in a medium using an external magnetic field, it is necessary to reduce the remanent magnetization of the Fe3O4 particles, which is the magnetization when the external magnetic field is no longer applied. It is known that the remanent magnetization of Fe3O4 particles decreases with decreasing particle size, and when the particle size is below 20 nm, the remanent magnetization is zero, exhibiting superparamagnetism.
[0005] Non-Patent Document 1 discloses the synthesis of Fe3O4 clusters by adding sodium acrylate to an ethylene glycol solution of ferric chloride (III) hexahydrate to reduce the particle size of each primary particle. Non-Patent Document 2 discloses the synthesis of Fe3O4 clusters by adding trisodium citrate to an ethylene glycol solution of anhydrous ferric chloride (III) to reduce the particle size of each primary particle. Both Fe3O4 clusters have a primary particle size of less than 20 nm, and therefore these Fe3O4 clusters are superparamagnetic materials.
[0006] Citation List
[0007] Non-patent literature
[0008] Non-patent literature 1: S. Xuan, YXJ Wang, JC Yu, KCF Leung, Chemistry of Materials, vol. 21, p. 5079-5087 (2009).
[0009] Non-patent literature 2: J. Liu, Z. Sun, Y. Deng, Y. Zou, C. Li, X. Guo, L. Xiong, Y. Gao, F. Li, D. Zhao, Angewandte Chemie International Edition, vol. 48, p.5875-5879 (2009). Summary of the Invention
[0010] Technical issues
[0011] The present invention relates to providing a magnetic particle, the magnetic particle comprising secondary particles, wherein a plurality of primary particles are aggregated in the secondary particles, each of the primary particles having a particle size that is considered to exhibit superparamagnetism, and the secondary particles having a large particle size.
[0012] Solution to the problem
[0013] To address the aforementioned problems, according to the present invention, a magnetic particle is provided, the magnetic particle comprising a secondary particle in which a plurality of primary particles are aggregated, wherein the average particle size of the secondary particles is 500 nm or more and 5000 nm or less, and wherein the average particle size of the primary particles is 2 nm or more and 20 nm or less.
[0014] Furthermore, according to the present invention, a magnetic particle for testing is provided, the magnetic particle comprising: the magnetic particle described above; and a resin layer disposed on the outside of the magnetic particle.
[0015] Furthermore, according to the present invention, a method for manufacturing magnetic particles is provided, the magnetic particles comprising secondary particles wherein a plurality of primary particles are aggregated therein, the method comprising: a step of obtaining an iron (III)-containing solution; a step of aging the iron (III)-containing solution; a step of obtaining a mixture of the iron (III)-containing solution obtained in the aging step with a precipitant; and a step of heating the mixture.
[0016] Beneficial effects of the invention
[0017] According to the present invention, Fe3O4 clusters that achieve both superparamagnetism and high magnetization can be provided. Attached Figure Description
[0018] Figure 1 is a schematic diagram of the structure of magnetic particles (Fe3O4 clusters) according to one embodiment of the present invention.
[0019] Figure 2 is a schematic diagram of magnetic particles for testing according to one embodiment of the present invention.
[0020] Figure 3 shows the synthesis process of Fe3O4 clusters.
[0021] Figure 4 shows the synthesis process of Fe3O4 clusters by blending.
[0022] Figure 5A is a SEM image (low magnification) of the Fe3O4 clusters produced in Example 1.
[0023] Figure 5B is a SEM image (high magnification) of the Fe3O4 clusters produced in Example 1.
[0024] Figure 6A is a SEM image (low magnification) of the Fe3O4 clusters produced in Example 2.
[0025] Figure 6B is a SEM image (high magnification) of the Fe3O4 clusters produced in Example 2.
[0026] Figure 7A is a SEM image (low magnification) of the Fe3O4 clusters produced in Example 6.
[0027] Figure 7B is a SEM image (high magnification) of the Fe3O4 clusters produced in Example 6.
[0028] Figure 8A is a SEM image (low magnification) of the Fe3O4 clusters produced in Example 8.
[0029] Figure 8B is a SEM image (high magnification) of the Fe3O4 clusters produced in Example 8.
[0030] Figure 9A is a SEM image (low magnification) of the Fe3O4 clusters produced in Example 14.
[0031] Figure 9B is a SEM image (high magnification) of the Fe3O4 clusters produced in Example 14.
[0032] Figure 10A is a SEM image of the Fe3O4 clusters produced in Example 22.
[0033] Figure 10B is a SEM image of the Fe3O4 clusters produced in Example 23.
[0034] Figure 10C is a SEM image of the Fe3O4 clusters produced in Example 24.
[0035] Figure 10D is a SEM image of the Fe3O4 clusters produced in Example 25.
[0036] Figure 10E is a SEM image of the Fe3O4 clusters produced in Example 26.
[0037] Figure 10F is a SEM image of the Fe3O4 clusters produced in Example 27.
[0038] Figure 10G is a SEM image of the Fe3O4 clusters produced in Example 28.
[0039] Figure 10H is a SEM image of the Fe3O4 clusters produced in Example 29.
[0040] Figure 11A is a SEM image (low magnification) of the Fe3O4 clusters produced in Comparative Example 2.
[0041] Figure 11B is a high-magnification SEM image of the Fe3O4 clusters produced in Comparative Example 2.
[0042] Figure 12A is a SEM image (low magnification) of the Fe3O4 clusters generated in Comparative Example 3.
[0043] Figure 12B is a SEM image (high magnification) of the Fe3O4 clusters generated in Comparative Example 3.
[0044] Figure 13A is a SEM image of the Fe3O4 clusters produced in Synthesis Example 1.
[0045] Figure 13B is a SEM image of the Fe3O4 clusters produced in Example 30.
[0046] Figure 13C is a SEM image of the Fe3O4 clusters produced in Example 31.
[0047] Figure 13D is a SEM image of the Fe3O4 clusters produced in Example 32.
[0048] Figure 13E is a SEM image of the Fe3O4 clusters produced in Synthesis Example 2.
[0049] Figure 14 shows the XRD patterns of the resulting particles: (a) Example 22, (b) Example 24, (c) Example 26, and (d) Example 28.
[0050] Figure 15A shows the hysteresis curve of the particles produced in Example 22.
[0051] Figure 15B shows the hysteresis curve of the particles produced in Example 24.
[0052] Figure 15C shows the hysteresis curve of the particles produced in Example 26.
[0053] Figure 15D shows the hysteresis curve of the particles produced in Example 28. Detailed Implementation
[0054] The embodiments of the present invention are described in detail below. In the present invention, the terms "Fe3O4 clusters" and "secondary particles" are synonymous.
[0055] [First Implementation Plan]
[0056] The first embodiment of the present invention relates to a magnetic particle.
[0057] First, the problems in this implementation scheme will be explained. In order to enable the rapid movement and transmission of Fe3O4 particles in a medium via an external magnetic field in various tests using magnetic particles (such as the optical waveguide-type test system described later), the Fe3O4 particles need to have a high magnetization. Generally, the magnetization of a single magnetic particle increases with its particle size. Therefore, increasing the particle size of Fe3O4 particles can increase the magnetization of a single Fe3O4 particle.
[0058] Therefore, it is difficult to obtain Fe3O4 particles that simultaneously achieve superparamagnetism and high magnetization, because there is a trade-off between reducing the particle size for superparamagnetism (which is a requirement for Fe3O4 particles with high external magnetic field controllability) and increasing the particle size for high magnetization.
[0059] Fe3O4 clusters as secondary particles are known, in which multiple primary Fe3O4 particles of tens of nanometers are aggregated. When the particle size of the primary particles in the Fe3O4 cluster is kept small, and the number of such primary particles to be aggregated is controlled—that is, the particle size of the secondary particles is controlled—Fe3O4 clusters that achieve both superparamagnetism and high magnetization can be obtained.
[0060] Meanwhile, the Fe3O4 clusters produced by the methods in Non-Patent Documents 1 and 2 all have primary particle sizes of less than 20 nm, thus making them superparamagnetic materials. However, the maximum secondary particle size in Non-Patent Document 1 is 280 nm, and in Non-Patent Document 2 it is 410 nm, resulting in relatively low magnetization of individual particles in these Fe3O4 clusters. Therefore, these Fe3O4 clusters are unsuitable for applications requiring rapid movement and transport of magnetic particles within a medium via a magnetic field. Fe3O4 clusters need to have larger particle sizes to enable rapid movement and transport within a medium via an external magnetic field.
[0061] According to an embodiment of the present invention, the magnetic particle is a magnetic particle comprising a plurality of secondary particles therein, wherein the average particle size of the secondary particles is 500 nm or more and 5000 nm or less, and wherein the average particle size of the primary particles is 2 nm or more and 20 nm or less.
[0062] The magnetic particles according to this embodiment can provide Fe3O4 clusters that achieve both superparamagnetism and high magnetization. When these magnetic particles are used for testing (particularly immunoassay), the magnetic particles for testing can be collected from the solution in a shorter time than with prior art products, thus significantly improving work efficiency. Furthermore, the magnetic particles for testing can be collected even in high-viscosity solutions, thus enabling immunoassay testing of high-viscosity solutions.
[0063] Details are as follows.
[0064] According to this embodiment, the magnetic particles are magnetic particles that include secondary particles in which multiple primary particles are aggregated.
[0065] The structure of the magnetic particles (Fe3O4 clusters) according to this embodiment is shown in Figure 1. In the magnetic particles according to this embodiment, the secondary particles preferably contain Fe3O4. The Fe3O4 clusters according to this embodiment are secondary particles 12 in which a plurality of primary Fe3O4 particles 11 are aggregated. In the magnetic particles according to this embodiment, the shape of the secondary particles is preferably spherical. The shape of the Fe3O4 clusters is preferably spherical; however, the shape depends on the application. In this embodiment, "sphere" (Figures 5A, 5B, 6A, 6B, 7A, 7B, 8A, 9A, 10A to 10H, 13A to 13E, and 15A and 15B) refers to a substantial sphere, such as "circular" or "spherical shape," and is not limited to a real sphere. The term also includes spheres with anisotropy or spheres with localized depressions or cracks. The shape of the Fe3O4 clusters according to this embodiment can be identified by observing the secondary particles using a scanning electron microscope (SEM).
[0066] As mentioned above, the magnetic properties of Fe3O4 clusters depend on the particle size (primary size) of each primary particle and the particle size (secondary size) of the secondary particles within the cluster. The remanent magnetization of the Fe3O4 cluster decreases with decreasing primary particle size, and when the primary particle size is below 20 nm, the remanent magnetization is zero, exhibiting so-called superparamagnetism. Furthermore, the number of primary particles to be aggregated, i.e., the secondary particle size, is correlated with the magnetization of the Fe3O4 cluster, and the magnetization of the Fe3O4 cluster increases with increasing secondary particle size. In other words, magnetic particles with larger secondary diameters have larger magnetization (e.g., saturation magnetization). The aggregation of primary particles results in Fe3O4 clusters with diameters greater than 500 nm exhibiting large magnetization.
[0067] In the magnetic particles according to this embodiment, the secondary particles preferably exhibit superparamagnetism. The magnetic properties and magnetization of the secondary particles of the Fe3O4 clusters in this invention can each be measured using, for example, a commercially available vibrating sample magnetometer (VSM) or a superconducting quantum interference device (SQUID).
[0068] In this embodiment, the primary and secondary particle sizes of the Fe3O4 clusters are number-average particle sizes measured from scanning electron microscopy (SEM) images. For each of the examples and comparative examples, the average particle size of 50 primary particles and the average particle size of 50 secondary particles, randomly sampled from the SEM images of the resulting Fe3O4 clusters, were calculated. Furthermore, the primary particle size was calculated using the Scherrer equation from the full width at half maximum (FWHM) of the diffraction peaks obtained by X-ray diffraction (XRD). The secondary particle size was calculated from the median diameters D50 and D90 based on the number-based particle size distribution measured by dynamic light scattering (DLS).
[0069] In the magnetic particles according to this embodiment, the average secondary particle size is 500 nm or more and 5000 nm or less, and the average secondary particle size is preferably 500 nm or more and 3000 nm or less. In the magnetic particles according to this embodiment, the secondary particle size (upper limit) is 5000 nm or less, preferably 4000 nm or less, more preferably 3000 nm or less, and even more preferably 2400 nm or less. In addition, in the magnetic particles according to this embodiment, the secondary particle size (lower limit) is preferably 500 nm or more, more preferably 700 nm or more, even more preferably 800 nm or more, and particularly preferably 1000 nm or more. With this configuration, magnetic particles with large magnetization (e.g., large saturation magnetization) can be obtained. For example, magnetic particles with a particle size twice that of prior art products (e.g., a secondary particle size of 400 nm) can have a saturation magnetization approximately eight times that of prior art products, and magnetic particles with a particle size six times that of prior art products (e.g., a secondary particle size of 2400 nm) can have a saturation magnetization more than 200 times greater than that of prior art products.
[0070] In the magnetic particles according to this embodiment, the average primary particle size (average particle size) is 2 nm or more and 20 nm or less. In the magnetic particles according to this embodiment, the primary particle size (upper limit) is 20 nm or less, preferably 19 nm or less, more preferably 18 nm or less, and even more preferably 16 nm or less. Furthermore, in the magnetic particles according to this embodiment, the primary particle size (lower limit) is 2 nm or more, preferably 4 nm or more, more preferably 7 nm or more, even more preferably 10 nm or more, and particularly preferably 12 nm or more. With this configuration, the magnetic particles according to this embodiment exhibit superparamagnetism, and the remanent magnetization can be 0 (zero).
[0071] In the magnetic particles according to this embodiment, the secondary particles typically contain Fe3O4, but may contain any other iron oxides, such as Fe2O3 or FeO, as long as the desired effect of this embodiment is achieved. Furthermore, the magnetic particles are not limited to simple substances and may be particles containing a mixture of magnetic substances (such as ferrites). In the magnetic particles according to this embodiment, the secondary particles are preferably Fe3O4. The magnetic particles according to this embodiment are preferably formed solely of Fe3O4 clusters and are substantially preferably free of any other components or structures, such as γ-Fe2O3. The fact that the magnetic particles are formed solely of Fe3O4 and free of any other substances (e.g., γ-Fe2O3) can be confirmed by X-ray diffraction (XRD).
[0072] Application Examples
[0073] The application example in this embodiment relates to magnetic particles for testing. The magnetic particles for testing according to an embodiment of the present invention preferably comprise magnetic particles according to this embodiment and a resin layer disposed on the outer side of the magnetic particles.
[0074] Referring to Figure 2, the magnetic particles for testing according to this embodiment are described.
[0075] According to this embodiment, the magnetic particles 36 for testing preferably include a silicon dioxide layer between the magnetic particles and the resin layer. Fe3O4 clusters 31, serving as the core, are coated with an inorganic layer 32.
[0076] To ensure the surface smoothness of the Fe3O4 clusters 31, an inorganic layer 32 is coated onto the Fe3O4 clusters. A silica layer is preferably used as the inorganic layer 32. Silica is chemically stable, and for example, a uniform and smooth layer can be formed on the surface of the Fe3O4 clusters 31 by a wet process such as the Stober method. A resin layer is coated on the outer side of the inorganic layer 32.
[0077] In the magnetic particles for testing according to this embodiment, the resin layer preferably includes at least a first resin layer 33 and a second resin layer 34. In the magnetic particles 36 for testing according to this embodiment, a first resin layer 33 and a second resin layer 34 are formed on the outer side of the inorganic layer 32. The first resin layer 33 is formed to protect the Fe3O4 clusters 31. For example, the silica layer formed by the Stuber process has a porous structure and is therefore insufficient to chemically protect Fe3O4. In the magnetic particles for testing according to this embodiment, the first resin layer 33 is preferably a hydrophobic resin layer. The first resin layer 33 is preferably a styrene-based resin with high chemical stability and high hydrophobicity.
[0078] In the magnetic particles for testing according to this embodiment, the second resin layer 34 is preferably disposed outside the first resin layer 33, and the second resin layer 34 is preferably a polyglycidyl methacrylate layer. The magnetic particles for testing 36 according to this embodiment preferably further include a ligand that binds to the surface of the resin layer, the ligand being preferably an antibody 35. The second resin layer 34 is disposed to immobilize the antibody 35 on the outermost surface of the magnetic particles for testing 36. Carboxyl, amino, thiol, epoxy, and the like are suitable functional groups for binding the antibody 35 to the outermost surface of the magnetic particles for testing 36. Therefore, the second resin layer 34 is preferably a resin having such functional groups.
[0079] The magnetic particles for testing according to this embodiment may further comprise a fluorescent material. There are no limitations on the method of applying the fluorescent material, and known techniques may be selected. Regarding the timing of applying the fluorescent material, for example, the fluorescent material may be mixed during the formation of the silica layer, applied after the formation of the silica layer and before the formation of the first resin layer, mixed together during the formation of the first resin layer, applied after the formation of the first resin layer and before the formation of the second resin layer, or applied after the formation of the second resin layer.
[0080] The application of fluorescent materials can be achieved, for example, by forming a resin layer, then mixing the fluorescent material and an organic solvent, and stirring the mixture under heating; and also by mixing the fluorescent material together during the formation of the resin layer. There are no restrictions on the fluorescent material to be selected, and known fluorescent materials can be chosen. The fluorescent material can be non-polymerizable or polymerizable. Examples of non-polymerizable fluorescent materials include Rhodamine B, Rhodamine 6G, and Lumisis (trademark) E-400 and Lumisis (trademark) E-460, which are used as europium complexes. Examples of polymerizable fluorescent materials include acryloyloxyethylthiocarbamoyl Rhodamine B and methacryloyloxyethylthiocarbamoyl Rhodamine B.
[0081] (Method for detecting antigens using magnetic particles in an optical waveguide-type testing system)
[0082] In waveguide-type testing systems, when detecting antigens from samples such as test specimens, magnetic particles bound to antibodies that specifically bind to the antigen, and sensors with antibodies specifically bound to the antigen immobilized on them, are used. The sensor is positioned below in the direction of gravity, and an electromagnet or similar device that generates magnetic force is placed near the sensor. When the electromagnet operates, the magnetic particles are attracted to the vicinity of the sensor by the combined effects of gravity and magnetism. Then, through an antigen-antibody reaction, the magnetic particles attracted to the sensor bind to the antibodies disposed on the sensor surface via the antigen. Furthermore, when the electromagnet is positioned above in the direction of gravity, magnetic particles not bound to antibodies disposed on the sensor surface can be pulled up in the opposite direction to gravity. Therefore, the magnetic particles bound to the sensor and those not bound to it can be separated from each other.
[0083] Measuring the change in the amount of emitted light as it enters the sensor from the light source allows for the measurement of the presence, concentration, and quantity of magnetic particles bound to the sensor surface via the antigen-antibody reaction. In other words, when magnetic particles are present on the sensor surface (in large quantities), the amount of emitted light is smaller compared to when no magnetic particles are present (in small quantities). Therefore, the presence, concentration, and quantity of analytes (such as antigens) in the sample can be measured based on the attenuation of the emitted light detected before the magnetic particles bind to the sensor.
[0084] When detecting the analyte using this method, it is important to reduce testing errors by minimizing the non-specific adsorption of proteins other than the analyte onto the magnetic particles, or by reducing adsorption when no antigen is present on the sensor surface. For this purpose, a resin layer is formed on the surface of the magnetic particles. The resin layer is preferably hydrophilic and includes functional groups capable of binding ligands, such as antibodies.
[0085] [Second Implementation Plan]
[0086] A second embodiment of the present invention relates to a method for manufacturing magnetic particles. The method for manufacturing magnetic particles according to this embodiment aims to facilitate control of both primary and secondary particle sizes.
[0087] The method for manufacturing magnetic particles according to an embodiment of the present invention is as follows: the magnetic particles include secondary particles in which a plurality of primary particles are aggregated, the method comprising: a step of obtaining an iron (III)-containing solution; a step of aging the iron (III)-containing solution; a step of obtaining a mixture of the iron (III)-containing solution obtained in the aging step and a precipitant; and a step of heating the mixture.
[0088] According to the manufacturing method of the present embodiment, it is easy to control the primary particle size and the secondary particle size. Therefore, a manufacturing method of magnetic particles can be provided, in which the magnetic particles have a wide range of magnetization intensities (with a wide range of secondary particle sizes) according to the application and simultaneously exhibit superparamagnetism.
[0089] The explanation is given below.
[0090] The manufacturing method of the magnetic particles according to the present embodiment is a method for manufacturing magnetic particles including secondary particles in which a plurality of primary particles are aggregated. As described above, the magnetic properties of the Fe3O4 clusters depend on the primary particle size and the secondary particle size of the Fe3O4 clusters. The remanent magnetization of the Fe3O4 clusters decreases as the primary particle size decreases, and when the primary particle size is 20 nm or less, the remanent magnetization is zero, that is, it exhibits so-called superparamagnetism. In addition, the number of primary particles to be aggregated, that is, the secondary particle size, has a correlation with the magnetization intensity of the Fe3O4 clusters, and the magnetization intensity of the Fe3O4 clusters increases as the particle size increases. Therefore, when the particle size of the Fe3O4 clusters can be controlled, Fe3O4 clusters with a wide range of magnetization intensities can be obtained. However, in the present embodiment, in the magnetic particles which are secondary particles in which a plurality of primary particles are aggregated according to the present embodiment, the cases of shape deformation and bonding of the Fe3O4 clusters or the cases where the shape becomes irregular are not included. This is because in such cases, the secondary particles are in a state of further association and cannot be called the secondary particles in the present embodiment any more.
[0091] <Synthesis of Fe3O4 clusters>
[0092] The synthesis process of the Fe3O4 clusters according to this embodiment is shown in Figure 3. The synthesis of the Fe3O4 clusters mainly includes: an iron(III) solution preparation step (a step of obtaining an iron(III) solution), a mixture preparation step (a step of obtaining a mixture), and a heating step (a step of heating the mixture), and may include an aging step (a step of aging the iron(III) solution) as appropriate. Each step is described in detail below.
[0093] <Step of obtaining an iron(III) solution>
[0094] The method for manufacturing magnetic particles according to this embodiment includes the step of obtaining an iron (III) solution containing ethylene glycol and anhydrous ferric chloride (III), wherein the iron (III) solution obtained in the step of obtaining the iron (III) solution preferably contains ethylene glycol and anhydrous ferric chloride (III). First, the preparation of the iron (III) solution will be described. The iron (III) solution is prepared by dissolving an iron (III) compound in ethylene glycol. The iron (III) compound is preferably anhydrous ferric chloride (III) or ferric chloride hexahydrate (III).
[0095] These compounds can be used alone or in any proportion as mixtures thereof. Except for ferric chloride (III), ferric nitrate (III), ferric acetate (III), ferric sulfate (III), ammonium ferric sulfate (III), ferric acetylacetonate (III), ferric hydroxide (III), ferric oxide (III), and their hydrates can be used alone or as mixtures thereof. Iron (III) compounds are not limited to these, as long as the compound is homogeneously dissolved in ethylene glycol.
[0096] Ethylene glycol is an organic compound called a polyol, which has multiple OH groups in its structure. Polyols are used in the synthesis of metal particles (polyol method) and act as both solvents and reducing agents. In this embodiment, ethylene glycol is also used as a solvent to dissolve ferric chloride (III) and as a reducing agent to reduce some of Fe(III) to Fe(II). In addition to ethylene glycol, polyols that are liquid at room temperature, such as diethylene glycol, triethylene glycol, 1,2-propanediol, and 1,3-propanediol, can be used, but these polyols cannot be used alone; they are used by mixing with ethylene glycol in any proportion.
[0097] Fe3O4 is iron oxide containing Fe(II) and Fe(III) in a 1:2 molar ratio. When Fe3O4 is obtained by using ethylene glycol and ferric chloride (III), ethylene glycol, acting as a reducing agent, partially reduces Fe(III) to Fe(II), thus producing Fe3O4. Therefore, the concentration of ferric chloride (III) in ethylene glycol, which acts as both a solvent and a reducing agent, is important. The concentration of ferric chloride (III) is preferably 0.05 M or more and 0.2 M or less, more preferably 0.1 M or more. When the concentration of ferric chloride (III) is less than 0.05 M, that is, when ethylene glycol, used as a reducing agent, is in excess relative to Fe(III), the reduction of Fe(III) is promoted, thereby increasing the amount of Fe(II), and therefore Fe3O4 is not produced. Meanwhile, when the concentration of ferric chloride (III) is greater than 0.2 M, the viscosity of the mixture increases as the concentration of the precipitant increases with the concentration of ferric chloride (III). Therefore, it becomes difficult to prepare a homogeneous mixture. Furthermore, almost no convection occurs in the mixture, so the mixture can hardly be heated uniformly.
[0098] The method for manufacturing magnetic particles according to this embodiment is a method for manufacturing magnetic particles comprising secondary particles in which a plurality of primary particles are aggregated. The method includes: a step of obtaining an iron (III)-containing solution; a step of aging the iron (III)-containing solution; a step of obtaining a mixture in which the iron (III)-containing solution obtained in the aging step is mixed with a precipitant; and a step of heating the mixture, as described below. In the method for manufacturing magnetic particles according to this embodiment, the iron (III)-containing solution obtained in the step of obtaining the iron (III)-containing solution may contain ethylene glycol and anhydrous ferric chloride (III). Furthermore, in the method for manufacturing magnetic particles according to this embodiment, the iron (III)-containing solution obtained in the step of obtaining the iron (III)-containing solution may contain ethylene glycol, anhydrous ferric chloride (III), and externally added water. Additionally, in the method for manufacturing magnetic particles according to this embodiment, the iron (III)-containing solution obtained in the step of obtaining the iron (III)-containing solution may contain ethylene glycol, anhydrous ferric chloride (III), and ferric chloride hexahydrate (III). Furthermore, in the method for manufacturing magnetic particles according to this embodiment, the iron (III)-containing solution obtained in the step of obtaining the iron (III)-containing solution may contain ethylene glycol, ferric chloride (III) hexahydrate, and externally added water.
[0099] <Steps to obtain the mixture>
[0100] The method for manufacturing magnetic particles according to this embodiment includes the step of obtaining a mixture in which an iron (III)-containing solution and a precipitant are mixed. Additionally, when the method for manufacturing magnetic particles according to this embodiment includes an aging step, the method includes the step of obtaining a mixture in which the iron (III)-containing solution and the precipitant obtained in the aging step are mixed. When the precipitant is added to the iron (III)-containing solution, the precursor particles precipitate. The dispersion liquid in which the precursor particles are dispersed is called the mixture. The precursor particles are amorphous and water-soluble iron (III) compound particles. In the method for manufacturing magnetic particles according to this embodiment, the precipitant is preferably an acetate. Specifically, urea, alkali metal hydroxides, and acetates can be used as precipitants, with acetates such as sodium acetate, potassium acetate, or ammonium acetate being particularly preferred.
[0101] <Water in the mixture>
[0102] In the method for manufacturing magnetic particles according to this embodiment, in at least one of the steps of obtaining an iron (III)-containing solution or obtaining a mixture, water derived from at least one of the following: ferric chloride (III) hexahydrate or externally added water. Water may be added to the mixture. The presence of water in the mixture affects the primary particle size and shape of the Fe3O4 clusters to be generated. Water may be added to ethylene glycol before the dissolution of the iron (III) compound, water may be added to the iron (III)-containing solution, or water may be added to the mixture after the addition of a precipitant.
[0103] The water in the mixture can be the hydrated water of a hydrate (such as ferric chloride (III) hexahydrate) and intentionally added water (hereinafter also referred to as "externally added water"). The presence of water derived from at least one of ferric chloride (III) hexahydrate or externally added water is required. In cases where water is absent in the mixture, for example, where the iron (III) compound is anhydrous ferric chloride (III), heating a mixture formed from ethylene glycol, anhydrous ferric chloride (III), and sodium acetate produces Fe3O4 clusters with small primary particle sizes, but the Fe3O4 clusters deform or aggregate together.
[0104] When the molar ratio of anhydrous ferric chloride (III) to ferric chloride hexahydrate (III) is changed while the concentration of ferric chloride (III) remains constant, the primary particle size of the Fe3O4 clusters increases with the increase of the ratio of ferric chloride hexahydrate (III), i.e., with the increase of water content in the mixture. However, the deformation and aggregation of the clusters are suppressed, and their shape becomes spherical. Furthermore, when externally added water is intentionally added to a mixture containing ethylene glycol and anhydrous ferric chloride (III), the increase in the particle size of each primary particle of the Fe3O4 cluster and the spheroidization of its secondary particles are observed with the increase of the amount of externally added water.
[0105] The increase in primary particle size of Fe3O4 clusters with increasing water content in the mixture is attributed to the higher solubility of Fe3O4 in water compared to its solubility in ethylene glycol. Therefore, the supersaturation of Fe3O4 in the mixture decreases, leading to a reduction in the number of nuclei to be generated. Simultaneously, the shape of the Fe3O4 clusters may be influenced by the interfacial free energy between Fe3O4 and the solvent. Since the interfacial free energy between Fe3O4 and ethylene glycol differs from that between Fe3O4 and the ethylene glycol / water mixed solvent, the shape of the Fe3O4 clusters may change depending on the presence or absence of water in the mixture.
[0106] In the method for manufacturing magnetic particles according to this embodiment, the amount of water in each 30 mL of ethylene glycol in the iron (III)-containing solution is preferably greater than 0 mL and less than 10.0 mL, more preferably greater than 0.2 mL and less than 8.0 mL. When no water is added at all, there is no effect on the spheroidization of Fe3O4 clusters. When the amount of water is greater than 10.0 mL, primary Fe3O4 particles do not form clusters. As mentioned above, the particle size of primary Fe3O4 clusters increases with the increase of water amount, but when the amount of water is less than 8.0 mL, the increase in the particle size of primary particles can be suppressed by combining it with operations such as adding additives, stirring during heating, and aging, which will be described later. In addition, when the amount of water is greater than 10.0 mL, Fe2O3 is also generated in addition to Fe3O4. The amount of water in each 30 mL of ethylene glycol is the sum of the hydrated water of the hydrate and the externally added water. For example, when 0.9 mmol of anhydrous ferric chloride (III) and 3.6 mmol of ferric chloride hexahydrate (III) are dissolved in 30 mL of ethylene glycol and 0.4 mL of externally added water is added, the hydrated water content in 3.6 mmol of ferric chloride hexahydrate (III) is 0.39 mL, and therefore the water content in each 30 mL of ethylene glycol is 0.79 mL.
[0107] <Additives in the mixture>
[0108] To reduce the particle size of each primary particle that forms the Fe3O4 clusters and improve the dispersibility of the Fe3O4 clusters, additives can be incorporated into the mixture. As additives, high-molecular-weight compounds, low-molecular-weight compounds, surfactants, chelating agents, etc., can be used, but additives having groups in ethylene glycol that form carboxylate ions (-COO-) are preferred. - The ions strongly coordinate with Fe(III), thus controlling the growth rate of primary Fe3O4 particles. As a component in ethylene glycol, it forms a carboxylate ion (-COO). - Additives containing the radical ) can be carboxylic acids and carboxylates, but carboxylates with high degree of dissociation and easy formation of carboxylate ions can also be used appropriately. Specifically, citric acid, malic acid, acrylic acid, tartaric acid, lactic acid, oleic acid, succinic acid, maleic acid, fumaric acid and their alkali metal salts are preferred, with trisodium citrate and sodium acrylate being particularly preferred.
[0109] In addition to reducing the particle size of each primary particle of the Fe3O4 cluster, these additives also have the aforementioned spheroidizing effect on the Fe3O4 cluster. That is, even in the absence of water in the mixture, spherical Fe3O4 clusters can be obtained when the additives coexist. Furthermore, each of these additives reduces the particle size of secondary particles.
[0110] <Steps for heating the mixture>
[0111] The method for manufacturing magnetic particles according to this embodiment includes a step of heating a mixture. The heating temperature of the mixture is 160°C or higher and 240°C or lower, preferably 180°C or higher and 220°C or lower. When the heating temperature is below 160°C, Fe3O4 is not generated. Meanwhile, when the heating temperature exceeds 240°C, the reaction rate is high and the particle size distribution of Fe3O4 clusters becomes larger.
[0112] The heating time of the mixture is 2 hours or more and 24 hours or less, preferably 4 hours or more and 12 hours or less. When the heating time is less than 2 hours, the conversion from precursor particles to Fe3O4 clusters is not completed, and when the heating time is greater than 24 hours, the primary particle size of the Fe3O4 clusters increases due to Ostwald ripening.
[0113] The mixture may contain components with boiling points equal to or below the heating temperature, such as ethylene glycol with a boiling point of 197°C or water with a boiling point of 100°C. Therefore, when heating the mixture, it is preferable to use a pressure-resistant, sealed container, which is commonly referred to as an "autoclave".
[0114] Furthermore, the mixture can be heated under stirring conditions using a container equipped with a stirring function. In the case of heating under static conditions using the aforementioned sealed container, a concentration gradient appears in the mixture as the reaction proceeds, and the mixture becomes non-uniform. However, in the case of heating under stirring conditions, mass transport is promoted, and the mixture can always remain homogeneous; therefore, heating is effective in reducing the particle size of each primary particle.
[0115] After heating, the container was placed at room temperature until it was fully cooled, and then the contents were removed. The resulting Fe3O4 clusters were washed twice with ethanol, twice with water, and dried in a drying oven at 80°C.
[0116] <Aging steps for iron (III) solutions>
[0117] The method for manufacturing magnetic particles according to this embodiment may include the step of aging an iron (III)-containing solution. The iron (III)-containing solution is a homogeneous solution in which iron (III) compounds are completely dissolved in ethylene glycol. Aging is the operation of maintaining the iron (III)-containing solution at a certain temperature for a certain period of time.
[0118] During aging, for example, it is believed that the reaction of Fe(III) ligands from chloride ion exchange to ethylene glycol is promoted, thus the solvation state of Fe(III) is thought to change, and this change is thought to affect the structure of the Fe3O4 clusters as the final product. Furthermore, although the iron(III) compounds appear to be completely dissolved macroscopically, microscopically, they may be dispersed in ethylene glycol in a state similar to an oligomer, and this oligomer becomes monomeric through aging. Therefore, the activity of the dissolved Fe(III) compounds increases, and as a result, the primary and secondary particle sizes of the Fe3O4 clusters change.
[0119] Therefore, aging is related to dissolved Fe(III) compounds, and the timing of aging is crucial; it must be carried out before the addition of a precipitant to the iron(III)-containing solution. Even when aging is performed after adding a precipitant to the iron(III)-containing solution to generate precursor particles, the structure of the Fe3O4 clusters remains unchanged.
[0120] As the aging temperature and aging time increase, the primary particle size of the Fe3O4 clusters decreases, while the secondary particle size increases. In the method for manufacturing magnetic particles according to this embodiment, the aging temperature in the aging step is preferably 0°C or higher and 130°C or lower, more preferably 10°C or higher and 130°C or lower. When the aging temperature is below 0°C, the aging effect is small; when the aging temperature is above 130°C, the primary Fe3O4 particles irregularly aggregate, thus failing to form spherical secondary particles. In the method for manufacturing magnetic particles according to this embodiment, the aging time in the aging step is preferably 1 hour or higher and 500 hours or lower, more preferably 1 hour or higher and 200 hours or lower. Aging of less than 1 hour does not affect the structure of the Fe3O4 clusters, while aging of more than 500 hours is excessive because the effect saturates within a certain time period.
[0121] When iron(III) solutions are aged, the timing of additive addition, which affects the primary and secondary particle sizes of Fe3O4 clusters, is also important. In particular, even when the type and concentration of additives are the same, the secondary particle size varies significantly depending on the time of additive addition.
[0122] Compared to adding the additive to an iron (III)-containing solution without aging, when the additive is added after aging of the iron (III)-containing solution, the particle size reduction effect of the additive is increased, and the secondary particle size is reduced. Meanwhile, when the additive is added before aging of the iron (III)-containing solution, the particle size reduction effect of the additive is offset by the particle size increase effect of aging, and the secondary particle size is increased compared to adding the additive to the iron (III)-containing solution without aging.
[0123] Furthermore, when the concentration of the additive to be added before aging of the iron(III) solution is low, below 0.01 M, the additive further promotes the particle size increase effect of aging, and the secondary particles become large. This is believed to be because the structure of the Fe(III) dissolved substances changes due to aging in the presence of the additive.
[0124] As mentioned above, the secondary particle size of Fe3O4 clusters obtained after aging using an iron(III)-containing solution depends on the degree of aging. Secondary particles with sizes greater than 500 nm and less than 3000 nm can be produced. The secondary particle size of Fe3O4 clusters can be controlled when two or more iron(III)-containing solutions with different degrees of aging are used in any proportion as a mixture. This method of controlling the particle size of Fe3O4 clusters is called the blending method. The synthesis process of Fe3O4 clusters by the blending method is shown in Figure 4.
[0125] For example, in cases where the iron (III) solution with a weak aging degree and the iron (III) solution with a strong aging degree have short aging times and can provide Fe3O4 clusters with a particle size of 500 nm and long aging times respectively, the particle size of the Fe3O4 clusters to be generated can be controlled within the range of 500 nm or more and 1000 nm or less when these solutions are used in any proportion in a mixture thereof.
[0126] <Product Identification Methods>
[0127] Product identification was performed by X-ray diffraction (XRD). XRD was performed using an X'PertPro manufactured by Spectris Co., Ltd. under the following conditions: θ-2θ scan, tube voltage of 40 kV, tube current of 45 mA, scan angle from 10° to 70°, step size of 0.02°, and measurement time of 1 second per step.
[0128] <Method for measuring the primary particle size of Fe3O4 clusters>
[0129] The primary particle size of Fe3O4 clusters was measured by scanning electron microscopy (SEM) or XRD.
[0130] SEM was performed using an S-4800 manufactured by Hitachi High Technology Corporation under the following conditions: accelerating voltage of 5 kV and irradiation current of 10 μA. Using an SEM image at 100,000x magnification, the particle size of 50 randomly sampled primary particles from the image was measured, and their average value was calculated.
[0131] XRD was performed using an X'PertPro manufactured by Spectris Co., Ltd. under the following conditions: θ-2θ scan, tube voltage of 40 kV, tube current of 45 mA, scan angle from 33° to 38°, step size of 0.01°, and measurement time of 2 seconds per step. The particle size D nm of each primary particle was calculated using the Scherrer equation (1).
[0132] D=Kλ / βcosθ (1)
[0133] Where K represents the Scherrer constant (K=0.89), λ represents the wavelength of the X-ray (λ=0.1542 nm), β represents the full width at half maximum (FWHM) of the diffraction peak of the (311) plane of Fe3O4 in rad, and θ represents the Bragg angle (0.3091 rad).
[0134] <Method for measuring the secondary particle size of Fe3O4 clusters>
[0135] The secondary particle size of Fe3O4 clusters was measured using SEM or dynamic light scattering (DLS).
[0136] SEM was performed using the equipment and conditions described above. Using an SEM image at 10000x magnification, the particle size of 50 randomly sampled secondary particles from the image was measured, and their average value was calculated.
[0137] The particle size distribution of Fe3O4 clusters via DLS was obtained using a Partica LA-950 laser diffraction / scattering particle size distribution measurement device manufactured by Horiba Manufacturing. The median diameters D50 and D90 were calculated from the measured number-based particle size distribution.
[0138] <Methods for measuring the magnetic properties of Fe3O4 clusters>
[0139] The magnetic properties of Fe3O4 clusters were measured by measuring hysteresis curves using the MPMS3 magnetic measurement system manufactured by Quantum Design, Inc., under the following conditions: a measurement temperature of 298 K, in VSM mode, and a magnetic field range of -20000 Oe to +20000 Oe.
[0140] <Manufacturing of Magnetic Particles for Testing>
[0141] The Fe3O4 clusters produced by controlling the particle size can be used as magnetic particles for testing by further forming an inorganic layer or an organic layer on the particle surface. As magnetic particles for testing, first, in order to ensure the surface smoothness of the Fe3O4 clusters, a silica layer can be formed by a wet method such as the Stober method. In addition, it is preferable to form a styrene-based resin layer having high chemical stability and high hydrophobicity as the first resin layer, and further form a glycidyl methacrylate layer as the second resin layer. A ligand can preferably be bound to the surface of the second resin layer, and the ligand is preferably an antibody. As functional groups for binding the antibody to the outermost surface of the magnetic particles for testing, carboxyl group, amino group, thiol group, epoxy group, etc. are suitable. Therefore, the second resin layer is preferably a resin having such functional groups.
[0142] The magnetic particles for testing can further contain a fluorescent material. There is no limitation on the method for applying the fluorescent material, and known techniques can be selected. As the timing for applying the fluorescent material, for example, the fluorescent material can be mixed when forming the silica layer, the fluorescent material can be applied after forming the silica layer and before forming the first resin layer, the fluorescent material can be mixed together when forming the first resin layer, the fluorescent material can be applied after forming the first resin layer and before forming the second resin layer, or the fluorescent material can be applied after forming the second resin layer. The method for applying the fluorescent material is achieved, for example, by forming a resin layer, then mixing the fluorescent material and an organic solvent, and stirring the mixture under heating; and also by mixing the fluorescent material when forming the resin layer. There is no limitation on the fluorescent material to be selected, and known fluorescent materials can be selected. The fluorescent material can be non-polymeric or polymeric. Examples of non-polymeric fluorescent materials include rhodamine B, rhodamine 6G, and Lumisis (trademark) E-400 and Lumisis (trademark) E-460 used as europium complexes, and examples of polymeric fluorescent materials include acryloyloxyethylthiocarbamoyl rhodamine B and methacryloyloxyethylthiocarbamoyl rhodamine B.
[0143] Examples
[0144] The present invention will be described in more detail by way of examples. However, the present invention is not limited to the following examples. In addition, the production conditions of the examples and the results of the Fe3O4 clusters are summarized in Table 1.
[0145] <<Synthesis of Fe3O4 Clusters>>
[0146] <Example 1>
[0147] 4.5 mmol of anhydrous ferric chloride (III) (FeCl3; Kishida Chemical Co., Ltd.) was dissolved in 30 mL of ethylene glycol (dehydrated; Fujifilm and Kojun Pharmaceutical Co., Ltd.) to prepare a 0.15 M ferric chloride (III) ethylene glycol solution (iron (III) solution).
[0148] After adding 0.4 mL of externally added H2O to the iron(III)-containing solution, aging was performed. The aging temperature was set to 25°C and the aging time to 72 hours. Additionally, the iron(III)-containing solution was injected into a pressure vessel containing a Teflon (trademark) inner cylinder and sealed, and then aged in a thermostat. 2.7 g of sodium acetate (CH3COONa; Kishida Chemical Co., Ltd.) was added to the aged iron(III)-containing solution to provide a mixture in which precursor particles were dispersed. This mixture was injected into a pressure vessel containing a Teflon (trademark) inner cylinder and sealed. The pressure vessel was heated in an oven at 180°C for 12 hours. After the reaction was complete, the pressure vessel was cooled sufficiently to approximately room temperature, and the resulting Fe3O4 clusters were removed. The resulting Fe3O4 clusters were washed twice with ethanol, twice with water, and dried in an oven at 80°C. SEM images of the resulting Fe3O4 clusters are shown in Figures 5A and 5B.
[0149] <Example 2>
[0150] Except that the aging temperature of the iron(III) solution was set to 60°C and the aging time was set to 72 hours in Example 1, the magnetic particles were manufactured using the same process as in Example 1. SEM images of the resulting Fe3O4 clusters are shown in Figures 6A and 6B.
[0151] <Example 3>
[0152] Except that the aging temperature of the iron (III) solution was set to 100°C and the aging time was set to 72 hours in Example 1, the magnetic particles were manufactured using the same process as in Example 1.
[0153] <Example 4>
[0154] Except that the aging temperature of the iron (III) solution was set to 60°C and the aging time was set to 24 hours in Example 1, the magnetic particles were manufactured using the same process as in Example 1.
[0155] <Example 5>
[0156] Except that the aging temperature of the iron (III) solution was set to 60°C and the aging time was set to 120 hours in Example 1, the magnetic particles were manufactured using the same process as in Example 1.
[0157] <Example 6>
[0158] Except that the aging temperature of the iron(III) solution was set to 60°C and the aging time was set to 168 hours in Example 1, the magnetic particles were manufactured using the same process as in Example 1. SEM images of the resulting Fe3O4 clusters are shown in Figures 7A and 7B.
[0159] <Example 7>
[0160] In Example 1, the aging temperature of the iron(III)-containing solution was set to 60°C, and the aging time was set to 168 hours. Trisodium citrate was added to the aged iron(III)-containing solution to achieve a concentration of 0.01 M. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1.
[0161] <Example 8>
[0162] In Example 1, an iron(III) solution was used, obtained by dissolving 0.9 mmol of FeCl3 and 3.6 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1. SEM images of the resulting Fe3O4 clusters are shown in Figures 8A and 8B.
[0163] <Example 9>
[0164] In Example 1, an iron(III) solution was used, obtained by dissolving 0.9 mmol of FeCl3 and 3.6 mmol of FeCl3·6H2O in ethylene glycol. The aging temperature of the iron(III) solution was set to 25°C, and the aging time was set to 168 hours. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1.
[0165] <Example 10>
[0166] In Example 1, an iron(III) solution was used, obtained by dissolving 0.9 mmol of FeCl3 and 3.6 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Trisodium citrate was added to the aged iron(III) solution to bring its concentration to 0.01 M. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1.
[0167] <Example 11>
[0168] In Example 1, an iron(III) solution was used, obtained by dissolving 3.6 mmol of FeCl3 and 0.9 mmol of FeCl3·6H2O in ethylene glycol. The aging temperature of the iron(III) solution was set to 60°C, and the aging time was set to 168 hours. Sodium acrylate was added to the aged iron(III) solution to achieve a concentration of 0.01 M. Magnetic particles were manufactured using the same procedures as in Example 1, except under these conditions.
[0169] <Example 12>
[0170] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. Except for these conditions, the magnetic particles were manufactured using the same procedure as in Example 1.
[0171] <Example 13>
[0172] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. The aging temperature of the iron(III) solution was set to 60°C, and the aging time was set to 168 hours. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1.
[0173] <Example 14>
[0174] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. Sodium acrylate was added to the iron(III) solution prior to aging to a concentration of 0.01 M. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1. SEM images of the resulting Fe3O4 clusters are shown in Figures 9A and 9B.
[0175] <Example 15>
[0176] In Example 1, the aging temperature of the iron(III)-containing solution was set to 60°C, and the aging time was set to 168 hours. The mixture was heated under stirring conditions using a flask and a mechanical stirrer. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1.
[0177] <Example 16>
[0178] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. Disodium malate was added to the iron(III) solution before aging to bring its concentration to 0.01 M. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1.
[0179] <Example 17>
[0180] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. Disodium malate was added to the iron(III) solution before aging to bring its concentration to 0.08 M. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1.
[0181] <Example 18>
[0182] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. Sodium oleate was added to the iron(III) solution before aging to bring its concentration to 0.01 M. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1.
[0183] <Example 19>
[0184] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol. The amount of externally added H2O was set to 0 mL. Sodium oleate was added to the iron(III) solution before aging to bring its concentration to 0.08 M. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 168 hours. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1.
[0185] <Example 20>
[0186] In Example 1, sodium acrylate was added to an iron (III)-containing solution to a concentration of 0.04 M prior to aging. The aging temperature of the iron (III)-containing solution was set to 60°C, and the aging time was set to 168 hours. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1.
[0187] <Example 21>
[0188] In Example 1, the aging temperature of the iron(III)-containing solution was set to 60°C, and the aging time was set to 168 hours. Sodium acrylate was added to the aged iron(III)-containing solution to achieve a concentration of 0.04 M. Magnetic particles were manufactured using the same procedures as in Example 1, except under these conditions.
[0189] <Examples 22 to 29>
[0190] In Example 1, a solution obtained by dissolving 4.5 mmol of FeCl3·6H2O in ethylene glycol was used as the iron(III) solution. The amount of externally added H2O was set to 0 mL. The aging temperature of the iron(III) solution was set to 60 °C, and the aging time was set to 4 hours to 168 hours. Except for these conditions, magnetic particles were manufactured using the same procedures as in Example 1. SEM images of the prepared Fe3O4 clusters for Examples 22 to 29 are shown in Figures 10A to 10H.
[0191] <Comparative Example 1>
[0192] Except that the iron (III)-containing solution was not aged in Example 1, the magnetic particles were manufactured using the same process as in Example 1.
[0193] <Comparative Example 2>
[0194] Except that the amount of externally added H2O was set to 0 mL in Example 1, the magnetic particles were manufactured using the same procedure as in Example 1. SEM images of the resulting Fe3O4 clusters are shown in Figures 11A and 11B.
[0195] <Comparative Example 3>
[0196] In Example 1, the amount of externally added H2O was set to 8.5 mL. The aging temperature of the iron(III)-containing solution was set to 60°C, and the aging time was set to 168 hours. Except for these conditions, the magnetic particles were manufactured using the same procedures as in Example 1. SEM images of the resulting Fe3O4 clusters are shown in Figures 12A and 12B. No Fe3O4 cluster formation was observed.
[0197] <Comparative Example 4>
[0198] Except that the aging temperature of the iron (III) solution was set to 140°C in Example 1, the magnetic particles were manufactured using the same process as in Example 1.
[0199] <Comparative Example 5>
[0200] In Example 1, an iron(III) solution was used, obtained by dissolving 4.5 mmol of FeCl3·6H2O in 1,2-propanediol (Kishida Chemical Co., Ltd.). The aging temperature of the iron(III) solution was set to 60°C, and the aging time was set to 168 hours. Except for these conditions, magnetic particles were manufactured using the same process as in Example 1.
[0201] <Comparative Example 6>
[0202] In Example 1, the iron (III)-containing solution was not aged. The mixture was heated under stirring conditions using a flask and a mechanical stirrer. Except for these conditions, the magnetic particles were manufactured using the same procedure as in Example 1.
[0203] <<Particle Size Control of Fe3O4 Clusters by Blending Method>>
[0204] <Examples 30 to 32>
[0205] Solution A (weak aging solution) and solution B (strong aging solution) were prepared. Solution A was a 0.15 M iron (III) solution obtained by dissolving ferric chloride (III) hexahydrate in ethylene glycol. Solution B was obtained by aging the 0.15 M iron (III) solution obtained by dissolving ferric chloride (III) hexahydrate in ethylene glycol at 60°C for 168 hours.
[0206] Solution A and solution B were mixed in any ratio to prepare 30 mL of solution C. The volume ratio "solution A:solution B" varied from 100:0 to 0:100. The case where the volume ratio "solution A:solution B" was set to 100:0 was used as synthesis example 1, and the case where the volume ratio "solution A:solution B" was set to 0:100 was used as synthesis example 2.
[0207] 2.7 g of CH3COONa was added to the prepared solution C to provide a mixture in which precursor particles were dispersed. The mixture was then poured into a pressure vessel containing a Teflon (trademark) inner cylinder and sealed. The pressure vessel was heated in an oven at 180°C for 12 hours. After the reaction was complete, the pressure vessel was cooled sufficiently to approximately room temperature, and the resulting Fe3O4 clusters were removed. The obtained Fe3O4 clusters were washed twice with ethanol, twice with water, and dried in an oven at 80°C.
[0208] The manufacturing conditions of the examples and the results of the Fe3O4 clusters are summarized in Table 2. SEM images of the produced Fe3O4 clusters are shown in FIGS. 13A to 13E.
[0209] <<Product Identification>>
[0210] As a result of XRD, the particles each have a single phase of Fe3O4. XRD patterns of the particles manufactured in Examples 22, 24, 26 and 28 are shown in FIG. 14.
[0211] <<Measurement of Magnetic Properties of Fe3O4 Clusters>>
[0212] As a result of the measurement of magnetic properties, the particles each exhibit superparamagnetic behavior without hysteresis characteristics. Hysteresis curves of Examples 22, 24, 26 and 28 are shown in FIGS. 15A to 15D, respectively.
[0213] <<Manufacture of Magnetic Particles for Testing>>
[0214] <Reference Example 1>
[0215] Disperse 0.5 g of the magnetic particles manufactured in Example 1 in a mixed solution containing 75 mL of ethanol (manufactured by Kishida Chemical Co., Ltd.) and 75 mL of pure water. Next, add 1.5 mL of tetraethyl orthosilicate (manufactured by Kishida Chemical Co., Ltd.), and add 22.5 mL of 28% ammonia water (manufactured by Kishida Chemical Co., Ltd.) as a catalyst, and react the mixture for 1.5 hours while stirring. After the reaction, remove the solvent by centrifugation, and wash the residue 7 times with pure water. Thus, a silica layer is formed on the magnetic particles.
[0216] Disperse the obtained silica-coated magnetic particles in a mixed solution containing 10 mL of ethanol and 10 mL of pure water, add 100 μL of 3-methacryloxypropyltrimethoxysilane (LS-3380, manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent, and mix well. Next, add 2 mL of 28% ammonia water, and stir the mixture for 1.5 hours. Next, collect the magnetic particles with a magnet to remove the solvent. Wash the magnetic particles thoroughly with pure water, and then add 60 mL of pure water bubbled with nitrogen to provide an aqueous dispersion.
[0217] Next, the dispersion was transferred to a 200 mL four-necked flask and stirred for 15 minutes while bubbling with nitrogen at a stirring speed of 200 rpm. After the nitrogen bubbling was switched to a nitrogen stream, 50 μL of styrene (manufactured by Kishida Chemical Co., Ltd.) was added to the dispersion. Next, 0.02 g of potassium persulfate (manufactured by Sigma-Aldrich) was dissolved in 2 mL of pre-degassed pure water via nitrogen bubbling, and 1 mL of this solution was added to the flask. The mixture was then heated at 35°C for 30 minutes using an oil bath, and the temperature was increased to 60°C and maintained for 1 hour. Subsequently, 200 μL of glycidyl methacrylate (manufactured by Kishida Chemical Co., Ltd.) was added, and the mixture was further maintained for 12 hours to complete the polymerization. After polymerization, the solvent was removed by centrifugation, and the magnetic particles were thoroughly washed with pure water.
[0218] Subsequently, 10 mg of the obtained magnetic particles were dispersed in 5 mL of pure water. Separately from the dispersion, 350 mg of mercaptosuccinic acid (manufactured by Kishida Chemical Co., Ltd.) was dissolved in 5 mL of pure water, and 0.8 mL of triethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added for pH adjustment. 1 mL of this solution was added to the particle dispersion, the mixture was stirred thoroughly, and heat-treated at 60°C for 3 hours. Afterwards, the solvent was removed by centrifugation, and the magnetic particles were thoroughly washed with pure water. Thus, a dispersion of magnetic particles comprising a silica layer, a first resin layer, and a second resin layer was obtained.
[0219] <Reference Example 2>
[0220] 0.5 g of the magnetic particles prepared in Example 1 were dispersed in a mixed solution containing 75 mL of ethanol and 75 mL of pure water. Next, 1.5 mL of tetraethyl orthosilicate and 22.5 mL of 28% ammonia water were added as a catalyst, and the mixture was allowed to react for 1.5 hours with stirring. After the reaction, the solvent was removed by centrifugation, and the magnetic particles were washed seven times with pure water. This resulted in the formation of a silica layer on the magnetic particles.
[0221] The obtained silica-coated magnetic particles were dispersed in a mixed solution containing 10 mL of ethanol and 10 mL of pure water, and 100 μL of 3-methacryloyloxypropyltrimethoxysilane was added as a silane coupling agent and mixed thoroughly. Next, 2 mL of 28% ammonia water was added and the mixture was stirred for 1.5 hours. The magnetic particles were then collected using a magnet to remove the solvent. The magnetic particles were thoroughly washed with pure water, and then 60 mL of pure water bubbled with nitrogen was added to provide an aqueous dispersion.
[0222] Next, the dispersion was transferred to a 200 mL four-necked flask and stirred for 15 minutes while bubbling with nitrogen at a stirring speed of 200 rpm. Subsequently, after the nitrogen bubbling had been switched to a nitrogen flow, 50 μL of styrene containing 5 mg of Lumisis (trademark) E-400 (manufactured by Central Techno Corporation) as a europium complex, 2 mg of sodium styrene sulfonate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 5 mg of divinylbenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) was added to the dispersion.
[0223] Next, the mixture was heated at 35°C for 30 minutes using an oil bath. Afterwards, 1 mg of 2, Azobis(2-methylpropanediamine) dihydrochloride (manufactured by Fujifilm and Kojun Chemical Co., Ltd.) was dissolved in 1 mL of pre-degassed pure water bubbled with nitrogen, and 500 μL of the solution was added to a flask. The temperature was raised to 60°C and maintained for 2 hours. Subsequently, 200 μL of glycidyl methacrylate was added, and the mixture was maintained for another 12 hours to complete the polymerization. After polymerization, the solvent was removed by centrifugation, and the magnetic particles were thoroughly washed with pure water.
[0224] Subsequently, 10 mg of the obtained magnetic particles were dispersed in 5 mL of pure water. Separately from the dispersion, 350 mg of mercaptosuccinic acid was dissolved in 5 mL of pure water, and 0.8 mL of triethylamine was added for pH adjustment. 1 mL of this solution was added to the particle dispersion, the mixture was stirred thoroughly, and heat-treated at 60°C for 3 hours. Afterward, the solvent was removed by centrifugation, and the residue was thoroughly washed with pure water. Thus, a dispersion of magnetic particles comprising a silica layer, a first resin layer containing fluorescent material, and a second resin layer was obtained. When the dispersion of the obtained magnetic particles was irradiated with a black lamp (manufactured by Nichia Chemical Co., Ltd.) with an excitation wavelength of 375 nm, red light emission was observed.
[0225] [Table 1-1]
[0226] Table 1
[0227]
[0228] [Table 1-1] (continued)
[0229]
[0230] [Table 1-2]
[0231] Table 1 (continued)
[0232]
[0233] [Table 2-1]
[0234] Table 2
[0235]
[0236] [Table 2-2]
[0237] Table 2 (continued)
[0238]
[0239] This invention is not limited to the embodiments described above, and various changes and modifications can be made without departing from the spirit and scope of the invention. The following claims are appended to disclose the scope of the invention.
[0240] This application claims priority based on Japanese Patent Application No. 2023-145189, filed on September 7, 2023; Japanese Patent Application No. 2023-145346, filed on September 7, 2023; and Japanese Patent Application No. 2024-151501, filed on September 3, 2024, the entire contents of which are incorporated herein by reference.
[0241] List of reference numerals
[0242] 11 Primary particles forming Fe3O4 clusters
[0243] 12 These are Fe3O4 clusters containing multiple primary particles.
[0244] 31 Fe3O4 cluster
[0245] 32 Inorganic layer
[0246] 33 First resin layer
[0247] 34 Second resin layer
[0248] 35 antibodies
[0249] 36. Magnetic particles for testing
Claims
1. A magnetic particle, said magnetic particle comprising a secondary particle in which a plurality of primary particles are aggregated, wherein, The average particle size of the secondary particles is greater than 500 nm and less than 5000 nm, and the average particle size of the primary particles is greater than 2 nm and less than 20 nm.
2. The magnetic particles according to claim 1, wherein, The average particle size of the secondary particles is greater than 500 nm and less than 3000 nm.
3. The magnetic particles according to claim 1 or 2, wherein, The secondary particles contain Fe3O4.
4. The magnetic particles according to any one of claims 1 to 3, wherein, The secondary particles are spherical in shape.
5. The magnetic particles according to any one of claims 1 to 4, wherein, The secondary particles exhibit superparamagnetism.
6. A magnetic particle for testing, the magnetic particle comprising: a magnetic particle according to any one of claims 1 to 5; and a resin layer disposed on the outer side of the magnetic particle.
7. The magnetic particles for testing according to claim 6 further comprises a silicon dioxide layer between the magnetic particles and the resin layer.
8. The magnetic particles for testing according to claim 6 or 7, wherein, The resin layer includes at least a first resin layer and a second resin layer.
9. The magnetic particles for testing according to claim 8, wherein, The first resin layer is a hydrophobic resin layer.
10. The magnetic particles for testing according to claim 8 or 9, wherein, The second resin layer is disposed outside the first resin layer, and wherein the second resin layer is a polyglycidyl methacrylate layer.
11. The magnetic particles for testing according to any one of claims 6 to 10, further comprising ligands bound to the surface of the resin layer.
12. The magnetic particles for testing according to claim 11, wherein, The ligand is an antibody.
13. A method for manufacturing magnetic particles, the magnetic particles comprising secondary particles wherein a plurality of primary particles are aggregated therein, the method comprising: The steps to obtain an iron (III)-containing solution; The step of aging the iron (III)-containing solution; The steps of obtaining the mixture include mixing the iron (III)-containing solution obtained in the aging step with a precipitant in the mixture; and heating the mixture.
14. The method for manufacturing magnetic particles according to claim 13, wherein, The iron (III) solution obtained in the step of obtaining the iron (III) solution contains ethylene glycol and anhydrous ferric chloride (III).
15. The method for manufacturing magnetic particles according to claim 13, wherein, The iron (III) solution obtained in the step of obtaining the iron (III) solution comprises ethylene glycol, anhydrous ferric chloride (III), and externally added water.
16. The method for manufacturing magnetic particles according to claim 13, wherein, The iron (III) solution obtained in the step of obtaining the iron (III) solution comprises ethylene glycol, anhydrous ferric chloride (III), and ferric chloride (III) hexahydrate.
17. The method for manufacturing magnetic particles according to claim 13, wherein, The iron (III) solution obtained in the step of obtaining the iron (III) solution contains ethylene glycol, ferric chloride (III) hexahydrate and externally added water.
18. The method for manufacturing magnetic particles according to any one of claims 13 to 17, wherein, The aging time in the aging step is more than 1 hour and less than 200 hours.
19. The method for manufacturing magnetic particles according to any one of claims 13 to 18, wherein, The aging temperature in the aging step is above 10°C and below 130°C.
20. The method for manufacturing magnetic particles according to any one of claims 14 to 17, wherein, The amount of water in each 30 mL of the ethylene glycol in the iron (III)-containing solution is less than 10.0 mL.
21. The method for manufacturing magnetic particles according to claim 20, wherein, The amount of water in each 30 mL of ethylene glycol in the iron (III)-containing solution is more than 0.2 mL and less than 8.0 mL.
22. The method for manufacturing magnetic particles according to any one of claims 13 to 21, wherein, The precipitant is an acetate.
Citation Information
Patent Citations
Lithospermum plant extract, acetylshikonin derived from lithospermum plant, composition for imparting Anti-influenza effect, food and beverage using lithospermum plant, clothing made from lithospermum plant, miscellaneous goods using lithospermum plant, products using lithospermum plant, method for preventing influenza, method for treating influenza, and acetylshikonin for imparting Anti-influenza effect
JP2023145189A
Method for producing cell preparation containing mesenchymal cells
JP2023145346A
Information processing device
JP2024151501A