Shrinkage-free high-ductility waterproof repair mortar and preparation method thereof
By combining a high-ductility functional system and a controllable early strength system, the problems of easy cracking and poor adhesion of repair mortar in humid environments are solved, achieving rapid repair and leak-stopping effects with non-shrink, high-ductility waterproof repair mortar.
Patent Information
- Application Number
- CN202511976367.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-25
- Publication Date
- 2026-05-05
AI Technical Summary
Existing repair mortars are prone to causing temperature stress cracks when the repair thickness exceeds 50mm, and there are difficulties in controlling the shrinkage rate. Furthermore, the construction effect is poor in humid environments, and it is difficult to effectively bond and seal leaks in humid environments.
Employing a high-ductility functional system and a controllable early strength system, including modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer, and amorphous active silica materials, combined with a specific mixing process, a non-shrink, high-ductility waterproof repair mortar is formed. This mortar can quickly bond in humid environments and maintain its integrity even when damaged by external forces.
It enables rapid repair in humid environments, avoids shrinkage cracks, improves adhesion and impermeability to old concrete, effectively seals leaks, and maintains structural integrity in the event of external damage.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of waterproof mortar technology, specifically to a non-shrink, high-ductility waterproof repair mortar and its preparation method. Background Technology
[0002] During the service life of concrete structures, due to loads and external factors, defects such as porosity and spalling easily develop on their surface, and even micro-cracks may form inside the material. If these defects are not repaired in time, external water and corrosive media will gradually seep in from the surface defects, eventually leading to accelerated deterioration of the concrete's durability. Accidents of concrete structures failing due to cracking, erosion, and porosity occur frequently. Structural failures or building functional failures caused by various reasons not only affect people's normal lives but also cause huge economic losses. In industrialized countries, more than 40% of total construction investment is used for building repair and reinforcement, while less than 60% is used for new building construction. In the United States, 40% of bridges are severely damaged, while in my country, about 30% of cement concrete pavements are damaged. Obviously, completely replacing or rebuilding damaged facilities is economically infeasible; the only solution is repair. Repairing concrete structures is of great practical significance in preventing environmental erosion of concrete, maintaining its performance, and ensuring and improving the durability and service life of concrete structures.
[0003] Repair mortar is a specialized cement-based polymer mortar used for repairing and reinforcing surface defects in concrete structures. It possesses high compressive strength, adhesion, crack resistance, and waterproofing properties. It can be used to repair cracked concrete surfaces in industrial and civil buildings, or to repair damaged industrial and civil buildings that do not meet design requirements. Cement-based repair mortar is a mixture of cement, fine aggregate (particle size less than 4.75mm), water, and, as needed, lime and additives.
[0004] Applications include surface repair of reinforced concrete buildings in industrial and civil facilities, repair of defects such as honeycomb and holes in concrete, repair of damaged concrete floors, overall repair and protection of concrete and masonry structures, maintenance of underground pipelines requiring corrosion resistance, power plant cooling towers, chimneys, chemical plant structures, and various factory buildings exposed to corrosive gases, ultra-fast repair of civil buildings, bridges, and roads, and emergency road repair in military engineering projects. It is also used in rapid road surface repair in frigid winter regions, rapid repair of bridge expansion joints, rapid tunnel repair, crash barrier repair, and rapid installation of anchors and guardrails.
[0005] Cracking is the most significant technical problem with existing repair mortars. When the thickness of a single repair exceeds 50mm, the heat of hydration inside the material is difficult to dissipate, easily leading to temperature stress cracks. Controlling the material's shrinkage rate also presents a challenge. The 28-day shrinkage rate of ordinary repair mortar is typically between 0.08% and 0.12%, and shrinkage cracks are highly likely to occur when the bond strength with the old concrete interface is insufficient. Secondly, the setting and hardening time of the repair mortar needs to be strictly controlled, requiring sufficient working time while also ensuring rapid curing and high early strength after application. Furthermore, it must be flexible in its working state, yet viscous enough to prevent slippage and deformation.
[0006] In some application scenarios, such as rapid repair of bridge expansion joints and rapid tunnel repair, it is necessary to work with water or even move water. Ordinary cement-based repair mortar will be affected by the water in the scene during construction, the water-material ratio will change, and some (all) components may even be washed away by water, resulting in the quality of the repair project not being guaranteed. Summary of the Invention
[0007] The purpose of this application is to provide a non-shrink, high-ductility waterproof repair mortar and its preparation method. This waterproof repair mortar has a controllable early strength system that can quickly repair damaged structures. It can also effectively bond in adverse environments such as dampness and vertical surfaces. When subjected to external force damage, the system can remain intact even when cracked and can effectively stop leaks.
[0008] To achieve the above objectives, this application provides the following technical solution: A non-shrink, high-ductility waterproof repair mortar comprises a high-ductility functional system and a controllable early strength system. The high-ductility functional system includes modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer (Wanwei 8020), amorphous active silica material (purchased from Xuzhou Mingrui Materials Co., Ltd.), defoamer, lithium carbonate, cellulose ether, thixotropic agent, L-tartaric acid, and sodium gluconate. The controllable early strength system includes ordinary silicate cement, rapid-hardening sulfoaluminate cement, 20-40 mesh river sand, and 40-70 mesh river sand. The mass ratio of the high-ductility functional system to the controllable early strength system is 1-10:70-100.
[0009] Preferably, the high ductility functional system comprises the following raw materials in parts by weight: 0.2-0.4 parts modified sisal fiber, 1-5 parts anhydrous calcium sulfate, 1-3 parts ethylene-vinyl acetate copolymer, 1-5 parts amorphous active silica material, 0.04-0.1 parts defoamer, 0.01-0.05 parts lithium carbonate, 0.01-0.05 parts 400 viscosity cellulose ether, 0.1-0.2 parts thixotropic agent, 0.1-0.2 parts L-tartaric acid, and 0.1-0.2 parts sodium gluconate. The controllable early strength system comprises the following raw materials in parts by weight: 10-30 parts ordinary silicate cement, 10-30 parts rapid-hardening sulfoaluminate cement, 22-35 parts 20-40 mesh river sand, and 20-30 parts 40-70 mesh river sand.
[0010] Preferably, the modified sisal fiber is obtained by sequentially treating natural sisal fiber with alkali, plasma, and grafting.
[0011] More preferably, natural sisal fibers are treated in an alkaline solution with a mass concentration of 0.1–2%, and then dried at 40–70°C to obtain alkali-treated natural sisal fibers. The alkali-treated natural sisal fibers are then subjected to plasma treatment at 80–100W power in an oxygen atmosphere to obtain surface-active natural sisal fibers. Modified sisal fibers are obtained by premixing the surface-active natural sisal fibers with maleic anhydride, dimethylformamide, and dicumyl peroxide, followed by extrusion. Alkali treatment removes the hemicellulose, lignin, and wax layer from the surface of natural sisal fibers, increasing the surface roughness and hydroxyl active sites. Plasma treatment introduces oxygen-containing polar groups, significantly enhancing the surface energy of the natural sisal fibers, giving the natural sisal fiber surface both a rough structure and hydrophilic groups.
[0012] More preferably, the mass ratio of the surface-active natural sisal fiber, maleic anhydride, dimethylformamide and dicumyl peroxide is 100:5-10:0.01-0.05:0.5-0.8.
[0013] More preferably, the premixing sequence is to add surface-active natural sisal fiber, maleic anhydride, dimethylformamide and dicumyl peroxide in sequence, and the extrusion temperature is 175-180°C. The surface-active natural sisal fiber is premixed with maleic anhydride, dimethylformamide and dicumyl peroxide before extrusion to prevent the decomposition of dicumyl peroxide.
[0014] First, surface-active natural sisal fiber and maleic anhydride are added. This is because the fiber needs to be dispersed in the matrix first, and then grafted with maleic anhydride to improve the interfacial bonding between the fiber and the matrix and reduce agglomeration. If maleic anhydride is added first and then the fiber is added, it may lead to excessively high local concentrations of anhydride, causing side reactions (such as hydrolysis) and reducing grafting efficiency. Next, dimethylformamide is added. As a polar aprotic solvent, dimethylformamide can dissolve maleic anhydride and promote its uniform distribution on the fiber surface. At the same time, it reduces melt viscosity and improves processing fluidity. It should be added after grafting modification to reduce melt viscosity and avoid premature addition to dissolve the fiber, which could lead to agglomeration and inhibit the activity of maleic anhydride. Finally, dicumyl peroxide is added. Dicumyl peroxide decomposes at high temperatures to generate free radicals, which initiate a grafting reaction between maleic anhydride and the matrix polymer. It may also trigger cross-linking to improve material strength. Adding it at the final stage prevents premature decomposition and potential runaway reaction (the half-life of dicumyl peroxide is approximately 1 minute at 175°C).
[0015] Preferably, the amorphous active silicon material has a silicon dioxide content of more than 90%, a particle size of ≤50nm, and an activity index of ≥85% after 7 days.
[0016] Preferably, the defoamer is DF02 defoamer; the thixotropic agent is thixotropic lubricant 602.
[0017] A method for preparing a non-shrink, high-ductility waterproof repair mortar includes the following steps: a high-ductility functional system is prepared by stirring modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer, amorphous active silica material, defoamer, lithium carbonate, cellulose ether, thixotropic agent, L-tartaric acid, and sodium gluconate in a high-pressure hot air environment; a controllable early strength system is prepared by mixing ordinary silicate cement, rapid-hardening sulfoaluminate cement, 20-40 mesh river sand, and 40-70 mesh river sand; and then the high-ductility functional system and the controllable early strength system are transported to a vacuum mixer and stirred evenly.
[0018] Preferably, the temperature in the hot air environment is 60–70°C. The raw materials of the high-ductility functional system are mixed in a high-pressure environment at 60–70°C to fluidize the raw materials. The airflow movement is used to fully mix the raw materials of different components to achieve homogenization, thus solving the problems of easy fiber agglomeration after grafting and the pre-homogenization of trace additives.
[0019] Beneficial effects: 1. The high-ductility functional system of this invention comprises modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer, amorphous active silica material, defoamer, lithium carbonate, cellulose ether, thixotropic agent, L-tartaric acid, and sodium gluconate. Modified sisal fiber improves the bond strength, interfacial adhesion, and pull-out shear force of natural fibers and mortar systems. Furthermore, modified sisal fiber addresses the issues of low fiber grafting rate and easy graft detachment, resulting in a tighter bond between the modified sisal fiber and the cementitious system (such as cement) when dispersed in the mortar system. This provides the tensile strength lacking in the cementitious system under external force, preventing cracking without complete failure. The ethylene-vinyl acetate copolymer reduces the elastic modulus of the system, giving the rigid mortar system high ductility. Simultaneously, the ethylene-vinyl acetate copolymer also improves the adhesion between the repair mortar and the existing substrate. Amorphous active silica materials can combine with calcium hydroxide in cement at the interface to form hydrated calcium silicate crystals, producing insoluble dendritic crystals in the pores and capillaries of concrete. This repeated reaction and propagation mechanism further eliminates the interface between the old and new cementitious systems, not only improving interfacial adhesion but also greatly enhancing the interface's impermeability. Anhydrous calcium sulfate reacts in the cementitious system to form columnar ettringite crystals, compensating for the hydration shrinkage of the cementitious system itself. The combination of L-tartaric acid and sodium gluconate slows down the system's gelation time, providing sufficient working time. 400 viscosity cellulose ether enhances the system's cohesiveness, preventing the mortar from being diluted by water in humid environments. Thixotropic agents control the mortar's fluidity, giving it better workability in vertical construction.
[0020] 2. The controllable early strength system includes ordinary silicate cement, rapid-hardening sulfoaluminate cement, 20-40 mesh river sand, and 40-70 mesh river sand. The combination of ordinary silicate cement and rapid-hardening sulfoaluminate cement, through adjusting their proportions, achieves a cementitious system with controllable working time. River sand of different mesh sizes forms a reasonable aggregate system. The high-ductility functional system and controllable early strength system of this invention, through a specific preparation method, form a high-ductility, non-shrinkage waterproof repair mortar. The controllable early strength system can quickly repair damaged structures, effectively bond even in adverse environments such as dampness and vertical surfaces, and remain intact even when subjected to external forces, effectively sealing leaks.
[0021] 3. In traditional composite mortar production processes, mixing cannot remove moisture from the fibers, causing them to easily agglomerate and become difficult to disperse evenly in the system. This results in reduced strength and crack resistance after hardening. Furthermore, directly mixing the fibers introduces a large amount of gas, leading to increased air content, decreased density, and reduced strength in the mortar system. Traditional planetary mixers also struggle to handle sand and separate particles (sand tends to settle). In contrast, this application first uses hot air to dry the fibers and pre-homogenizes the functional materials with the fibers. Simultaneously, a twin-shaft mixer is used to evenly mix the sand and cementitious materials. Finally, vacuum mixing is used to remove the gas introduced during the pre-mixing of the fibers, effectively controlling the air content within the system and ensuring product performance. Attached Figure Description
[0022] Figure 1 This is a connection diagram of a high-pressure hot air mixer, a twin-shaft groove mixer, and a vacuum mixer. Figure 2 This is a schematic diagram of the internal structure of a high-pressure hot air mixer; Figure 3 This is a schematic diagram of a high-pressure hot air mixer.
[0023] In the diagram: 1. High-pressure hot air mixer; 2. Twin-shaft groove mixer; 3. Spiral auger feeder; 4. Vacuum mixer; 5. Air outlet pipe; 6. High-pressure hot air mixing chamber; 7. Air compressor; 8. Heater; 9. Air pipe. Detailed Implementation
[0024] The present application will now be described in detail with reference to the accompanying drawings and embodiments. Various examples are provided by way of explanation and not by way of limitation. In fact, those skilled in the art will understand that modifications and variations can be made to the present application without departing from the scope or spirit of the present application. For example, a feature shown or described as part of one embodiment may be used in another embodiment to produce yet another embodiment. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention should fall within the scope of protection of the embodiments of the present invention.
[0025] A non-shrink, high-ductility waterproof repair mortar comprises a high-ductility functional system and a controllable early strength system. The high-ductility functional system includes the following raw materials in parts by weight: 0.2–0.4 parts modified sisal fiber, 1–5 parts anhydrous calcium sulfate, 1–3 parts ethylene-vinyl acetate copolymer (Wanwei 8020), 1–5 parts amorphous active silica material (purchased from Xuzhou Mingrui Materials Co., Ltd., with a silica content greater than 90%, particle size ≤50nm, and 7-day activity index ≥85%), and 0.04–0.1 parts defoamer (DF02 defoamer, purchased from [unclear - likely a supplier]). The controlled early strength system comprises the following raw materials by weight: 10-30 parts ordinary silicate cement, 10-30 parts rapid-hardening sulfoaluminate cement, 22-35 parts 20-40 mesh river sand, and 20-30 parts 40-70 mesh river sand. The controlled early strength system also includes: 0.01-0.05 parts lithium carbonate, 0.01-0.05 parts 400 viscosity cellulose ether, 0.1-0.2 parts thixotropic agent (thixotropic lubricant 602, purchased from ROCKWOOD, Germany), 0.1-0.2 parts L-tartaric acid, and 0.1-0.2 parts sodium gluconate.
[0026] Modified sisal fiber is obtained through the following steps: (1) Natural sisal fiber is treated in an alkaline solution with a mass concentration of 0.1-2%, and then dried at 40-70°C to obtain alkali-treated natural sisal fiber. (2) alkali-treated natural sisal fibers are subjected to plasma treatment with 80-100W power in an oxygen atmosphere to obtain surface-active natural sisal fibers; (3) Add surface-active natural sisal fiber, maleic anhydride, dimethylformamide and dicumyl peroxide in sequence, premix and then extrude at 175-180°C to obtain modified sisal fiber. The mass ratio of surface-active natural sisal fiber, maleic anhydride, dimethylformamide and dicumyl peroxide is 100:5-10:0.01-0.05:0.5-0.8.
[0027] A method for preparing a non-shrink, high-ductility waterproof repair mortar includes the following steps: a high-ductility functional system is prepared by stirring modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer, amorphous active silica material, defoamer, lithium carbonate, cellulose ether, thixotropic agent, L-tartaric acid, and sodium gluconate in a high-pressure hot air environment (60–70°C); a controllable early strength system is prepared by mixing and stirring ordinary silicate cement, rapid-hardening sulfoaluminate cement, 20–40 mesh river sand, and 40–70 mesh river sand; and then the high-ductility functional system and the controllable early strength system are transported to a vacuum mixer and stirred evenly.
[0028] Example 1 A method for preparing a non-shrink, high-ductility waterproof repair mortar includes the following steps: (1) Natural sisal fiber was treated in a sodium hydroxide solution with a mass concentration of 2% for 8 hours. After treatment, it was washed with water until neutral and then pre-dried at 45°C for 2 hours to prevent the surface from drying too quickly and locking in the internal moisture. After most of the free water evaporated, the temperature was gradually increased to 65°C for thorough drying to obtain alkali-treated natural sisal fiber.
[0029] (2) The natural sisal fiber treated with alkali was subjected to plasma treatment with 100W power for 10 minutes in an oxygen atmosphere to obtain surface-active natural sisal fiber; (3) First, mix 100 parts of surface-active natural sisal fiber and 10 parts of maleic anhydride. Then, add 0.05 parts of dimethylformamide and 0.5 parts of dicumyl peroxide. Finally, after premixing, extrude at 178°C to obtain modified sisal fiber.
[0030] (4) 0.3 parts of modified sisal fiber, 3 parts of anhydrous calcium sulfate, 3 parts of vinyl acetate-ethylene copolymer powder, 0.1 parts of amorphous active silicon material, 0.1 parts of DF02 defoamer, 0.05 parts of lithium carbonate, 0.05 parts of 400 viscosity cellulose ether, 0.2 parts of thixotropic lubricant 602, 0.1 parts of L-tartaric acid and 0.1 parts of sodium gluconate were placed in a high-pressure hot air mixer 1 and stirred at 0.6 MPa and 60°C to obtain a high ductility functional system.
[0031] (5) Put 20 parts of ordinary silicate cement, 20 parts of rapid hardening sulfoaluminate cement, 28 parts of 20-40 mesh river sand and 25 parts of 40-70 mesh river sand into a twin-shaft groove mixer 2 and mix evenly to obtain a controllable early strength system. (6) The high ductility functional system and the controllable early strength system are fed into the vacuum mixer 4 through the spiral auger feeder 3 and vacuum mixed to obtain non-shrink high ductility waterproof repair mortar.
[0032] like Figure 1-3 As shown, the high-pressure hot air mixer 1 includes a high-pressure hot air mixing chamber 6. Air outlet pipes 5 are evenly arranged inside the high-pressure hot air mixing chamber 6. One end of the air outlet pipe 5 is located inside the high-pressure hot air mixing chamber 6, and the other end is connected to an air pipe 9. A heater 8 is provided inside the air pipe 9, and an air compressor 7 is connected to the air pipe 9.
[0033] In specific implementation, 0.3 parts of modified sisal fiber, 3 parts of anhydrous calcium sulfate, 3 parts of vinyl acetate-ethylene copolymer powder, 0.1 parts of amorphous active silicon material, 0.1 parts of DF02 defoamer, 0.05 parts of lithium carbonate, 0.05 parts of 400 viscosity cellulose ether, 0.2 parts of thixotropic lubricant 602, 0.1 parts of L-tartaric acid, and 0.1 parts of sodium gluconate are placed in a high-pressure hot air mixing chamber 6. Compressed air is sent into the air pipe 9 by an air compressor 7. The air is heated to 60°C by a heater 8 built into the air pipe 9 and then passes through the air pipe 9 and the air pipe 5, forming a rotating hot air in the high-pressure hot air mixing chamber 6. The high-ductility functional system is obtained by stirring under the conditions of 0.6 MPa and 60°C.
[0034] Twin-shaft groove mixer: Dongguan Qingxi Zhentai General Machinery Equipment; Spiral reamer feeder: Weifang Linqu Baiente Electromechanical; Vacuum mixer: Wuxi Minghai Powder Machinery Equipment Factory Minghai Powder Vacuum Mixer; Air compressor model is GA55VSD, heater model is HRY1-HRY3.
[0035] Example 2 Unlike Example 1, this example uses 10 parts of ordinary silicate cement and 30 parts of rapid-hardening sulfoaluminate cement.
[0036] Example 3 Unlike Example 1, this example uses 30 parts of ordinary silicate cement and 10 parts of rapid-hardening sulfoaluminate cement.
[0037] Example 4 Unlike Example 1, there were 53 parts of 20-40 mesh river sand and 0 parts of 40-70 mesh river sand.
[0038] Example 5 Unlike Example 1, there were 0 parts of 20-40 mesh river sand and 53 parts of 40-70 mesh river sand.
[0039] Comparative Example 1 Unlike Example 1, the modified sisal fiber was replaced with ordinary polypropylene fiber.
[0040] Comparative Example 2 Unlike Example 1, the manufacturing process was changed to directly mix all materials using a planetary mixer.
[0041] The repair mortars prepared in Examples 1-5 and Comparative Examples 1-2 were characterized. The flowability of the mortar was determined according to the "Method for Determining the Flowability of Cement Mortar" (GB / T 2419-2005); the initial setting time was determined according to the "Test Method for Standard Consistency Water Requirement, Setting Time and Soundness of Cement" (GB 1346-2011); the compressive strength and tensile bond strength were determined according to the "Repair Mortar" (JC / T2381-2016); the preparation of the wet substrate for tensile bond strength was based on the "Code for Construction and Acceptance of Building Exterior Wall Facing Brick Engineering" (JGJ144-2019); the second impermeability pressure ratio was determined according to the "Technical Specification for Self-Healing Waterproofing Materials Admixtured in Concrete and Construction" (T / SZWA 003-2020) (ordinary repair mortar was used for the blank group); the air content was determined according to the "Test Standard for Performance of Ordinary Concrete Mixtures" (GB / T 50080-2016); and the 28-day equivalent flexural strength was determined according to the "Technical Standard for Application of High Ductility Concrete" (DB62 / T). (3159-2019), the results are shown in Table 1.
[0042] Table 1 Performance characterization results of non-shrink high-ductility waterproof repair mortar As shown in Table 1, the non-shrink, high-ductility waterproof repair mortar prepared in Example 1 has high tensile bond strength, can bond tightly to the substrate, and achieve a repair effect (the tensile bond strength required by "Repair Mortar" (JC / T2381-2016) is ≥1.0MPa). At the same time, the equivalent flexural strength at 28 days far exceeds the requirement of ≥5.0MPa required by "Technical Standard for Application of High-Ductility Concrete" (DB62 / T 3159-2019), exhibiting strain hardening characteristics under stress, significantly improving deformation capacity, and achieving "cracked but not broken". The second anti-seepage pressure ratio exceeds 200% of the requirement of "Technical Specification for Self-Healing Waterproof Materials and Construction of Concrete Admixtures" (T / SZWA003-2020), indicating that it can effectively self-repair after cracking, avoiding the problem of traditional repair mortar failing as soon as it cracks.
[0043] Comparing the data from Examples 1-3, it can be seen that adjusting the ratio of ordinary Portland cement to rapid-hardening sulfoaluminate cement can significantly adjust its initial setting time and early strength; different ratios can be selected for different working conditions. Comparing the data from Examples 1, 4, and 5, it can be seen that a reasonable gravel gradation plays a key role in the final flowability of the system, and an unreasonable gravel gradation will reduce the strength and toughness of the system to some extent.
[0044] Comparing the data from Example 1 and Comparative Example 1, it can be seen that the equivalent flexural strength at 28 days is significantly lower with polypropylene fiber compared to modified sisal fiber, affecting the system's deformation and crack resistance. Comparing the data from Example 1 and Comparative Example 2, it can be seen that the product mixed using a conventional planetary mixer has a significantly higher air content and a significantly lower strength than the product prepared using the method described in this patent. Furthermore, due to uneven fiber dispersion, its flowability on the mixing table is also somewhat reduced, affecting its workability.
[0045] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0046] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A non-shrink, high-ductility, waterproof repair mortar, characterized in that, The system includes a high-ductility functional system and a controllable early strength system. The high-ductility functional system comprises modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer, amorphous active silicate material, defoamer, lithium carbonate, cellulose ether, thixotropic agent, L-tartaric acid, and sodium gluconate. The controllable early strength system comprises ordinary silicate cement, rapid-hardening sulfoaluminate cement, 20-40 mesh river sand, and 40-70 mesh river sand. The mass ratio of the high-ductility functional system to the controllable early strength system is 1-10:70-100.
2. The non-shrink, high-ductility waterproof repair mortar according to claim 1, characterized in that, The high-ductility functional system comprises the following raw materials in parts by weight: 0.2-0.4 parts modified sisal fiber, 1-5 parts anhydrous calcium sulfate, 1-3 parts ethylene-vinyl acetate copolymer, 1-5 parts amorphous active silica material, 0.04-0.1 parts defoamer, 0.01-0.05 parts lithium carbonate, 0.01-0.05 parts 400 viscosity cellulose ether, 0.1-0.2 parts thixotropic agent, 0.1-0.2 parts L-tartaric acid, and 0.1-0.2 parts sodium gluconate. The controllable early strength system comprises the following raw materials in parts by weight: 10-30 parts ordinary silicate cement, 10-30 parts rapid-hardening sulfoaluminate cement, 22-35 parts 20-40 mesh river sand, and 20-30 parts 40-70 mesh river sand.
3. The non-shrink, high-ductility waterproof repair mortar according to claim 1 or 2, characterized in that, The modified sisal fiber is obtained by sequentially treating natural sisal fiber with alkali, plasma, and grafting.
4. The non-shrink, high-ductility waterproof repair mortar according to claim 3, characterized in that, Natural sisal fibers are treated in an alkaline solution with a mass concentration of 0.1-2%, and then dried at 40-70°C to obtain alkali-treated natural sisal fibers. The alkali-treated natural sisal fibers are then subjected to plasma treatment with a power of 80-110W in an oxygen atmosphere to obtain surface-active natural sisal fibers. Modified sisal fibers are obtained by premixing the surface-active natural sisal fibers with maleic anhydride, dimethylformamide and dicumyl peroxide and then extruding them.
5. The non-shrink, high-ductility waterproof repair mortar according to claim 4, characterized in that, The mass ratio of the surface-active natural sisal fiber, maleic anhydride, dimethylformamide, and dicumyl peroxide is 100:5-10:0.01-0.05:0.5-0.
8.
6. The non-shrink, high-ductility waterproof repair mortar according to claim 4 or 5, characterized in that, The premixing sequence involves sequentially adding surface-active natural sisal fiber, maleic anhydride, dimethylformamide, and diisopropylbenzene peroxide, and the extrusion temperature is 175–180°C.
7. The non-shrink, high-ductility waterproof repair mortar according to claim 1 or 3, characterized in that, The amorphous active silicon material has a silicon dioxide content of greater than 90%, a particle size of ≤50nm, and an activity index of ≥85% after 7 days.
8. The non-shrink, high-ductility waterproof repair mortar according to claim 1, 3, or 7, characterized in that, The defoamer is DF02 defoamer; the thixotropic agent is thixotropic lubricant 602.
9. A method for preparing a non-shrink, high-ductility waterproof repair mortar as described in claim 1, 3, 7, or 8, characterized in that, Includes the following steps: A high-ductility functional system was prepared by stirring modified sisal fiber, anhydrous calcium sulfate, ethylene-vinyl acetate copolymer, amorphous active silica material, defoamer, lithium carbonate, cellulose ether, thixotropic agent, L-tartaric acid, and sodium gluconate in a high-pressure hot air environment. A controllable early strength system was prepared by mixing ordinary silicate cement, rapid-hardening sulfoaluminate cement, 20-40 mesh river sand, and 40-70 mesh river sand. The high-ductility functional system and the controllable early strength system were then transported to a vacuum mixer and stirred evenly.
10. The method for preparing the non-shrink, high-ductility waterproof repair mortar according to claim 9, characterized in that, The temperature in the hot air environment is 60–70°C.