Low-stacking-fault-energy micro-twin-crystal synergistically-deformed cobalt-based alloy and preparation method thereof
By adding Ti and Ta elements to cobalt-based superalloys and controlling the stacking fault energy to a negative value, the microtwin deformation mechanism is activated, which solves the problem of insufficient high-temperature plasticity of traditional cobalt-based alloys and achieves a synergistic improvement in high-temperature strength and plasticity, exhibiting excellent high-temperature mechanical properties.
Patent Information
- Application Number
- CN202610073409.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-20
- Publication Date
- 2026-05-05
AI Technical Summary
Traditional cobalt-based superalloys have insufficient grain boundary strength in the high-temperature region, are easily affected by diffusion-controlled reordering, resulting in decreased plasticity, and rely on a single dislocation slip deformation mechanism.
By precisely controlling the electronic structure of the Co-Al-W alloy through first-principles calculations and adding Ti and Ta elements, the stacking fault energy is controlled in the negative range of -95 mJ/m² to -89 mJ/m², thereby activating the microtwin deformation mechanism and realizing the synergistic effect of dislocation slip and microtwins.
The high-temperature strength and plasticity are simultaneously improved at high temperatures, which significantly enhances the overall performance of the alloy. In particular, it exhibits a uniform elongation of up to 48% and a yield strength of over 480 MPa at 850℃.
Smart Images

Figure CN121976093A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a low-layer fault energy microtwin synergistic deformation cobalt-based alloy and its preparation method, belonging to the field of cobalt-based high-temperature alloy technology. Background Technology
[0002] Scientists have discovered a coherent L12-type γ'-Co3(Al, W) intermetallic compound phase in Co-Al-W ternary alloys, similar to that found in nickel-based superalloys. This discovery is a milestone in the development of cobalt-based superalloys, meaning that cobalt-based alloys, like advanced nickel-based alloys, can undergo highly effective precipitation strengthening through a coherent, ordered γ' phase. This significantly improves their high-temperature strength and heat resistance while maintaining the original excellent properties of cobalt-based alloys. Based on this novel strengthening mechanism, researchers are developing a series of new cobalt-based superalloys.
[0003] The invention patent with authorization announcement number CN 115161517 B discloses a rhenium-containing, high-temperature oxidation-resistant, γ'-phase-strengthened cobalt-based superalloy. The alloy's chemical composition by weight percentage is: Ni 20~39%, Al 4.2~7%, Ti 0~3%, W 2~9%, Ta 1~15%, Cr 2~9%, Re 0.1~5%, Nb 0~3%, Mo 0~3%, Hf 0~1%, Y 0~1%, with the balance being Co. The alloy's γ'-phase dissolution temperature is greater than 1180℃, Ni:Co = 0.6~0.95, W+Ta+Re+Mo+Nb+Hf ≤ 25%, Al+Ti+Cr ≥ 8%, Al+Cr ≥ 7.5%, and the alloy's density is not higher than 9 g / cm³. 3 After isothermal oxidation at 1100℃ for 100 hours, the total thickness of the oxide layer formed on the alloy surface was 8.6±0.7μm, forming a continuous and dense alumina protective layer, with an oxidation weight gain of less than 1 mg / cm³. 2The oxidation resistance rating reaches the fully oxidation-resistant level; after solution treatment and aging heat treatment at 1100℃, the microstructure of the high-temperature alloy is a two-phase structure of γ and γ', with the volume fraction of γ' phase ≥50%, the size of γ' phase ≤550nm, and the γ' phase has a cubic morphology. The specific preparation process includes the following steps: (1) weigh high-purity Co, Ni, Al, Ti, W, Ta, Cr, and Re elemental materials according to the component ratio; (2) place the weighed high-purity elemental raw materials in a vacuum arc melting furnace and perform alloy melting in a high-purity Ar protective atmosphere. After the alloy is completely melted, keep it for 1-2 minutes, then turn off the power and cool it to room temperature. Repeat the above melting steps 8-10 times to finally obtain a cobalt-based high-temperature alloy ingot; (3) in a protective atmosphere, keep the prepared cobalt-based high-temperature alloy ingot at a solid solution temperature of 1220-1240℃ for 18-24 hours and air cool it; then keep it at an aging temperature of 900℃-1150℃ for 1-2000 hours and air cool it to obtain a γ' phase strengthened cobalt-based high-temperature alloy.
[0004] These cobalt-based superalloys primarily rely on dislocation slip for plastic deformation. Although the γ' phase strengthens the matrix, the high-temperature strength at the grain boundaries is insufficient and susceptible to diffusion-controlled reordering, leading to grain boundary failure and decreased plasticity in the high-temperature region. Summary of the Invention
[0005] To solve the above-mentioned problems, the present invention provides, in a first aspect, a cobalt-based alloy with low stacking fault energy and microtwin-coordinated deformation.
[0006] The technical solution of the present invention to solve the above problems is as follows:
[0007] A low-stacking-energy microtwin-coordinated deformation cobalt-based alloy, wherein the cobalt-based alloy is based on a Co-Al-W alloy, and after first-principles calculations, no more than 4 wt% of the first optimized element Ti and no more than 4 wt% of the second optimized element Ta are added, so that the stacking fault energy of the cobalt-based alloy is controlled at -95 mJ / m at 0 K. 2 ~ -89 mJ / m 2 .
[0008] This invention provides a systematic solution to the insufficient high-temperature plasticity of γ′ phase-strengthened cobalt-based superalloys. Instead of being limited to traditional γ′ phase precipitation strengthening, this invention uses first-principles calculations to precisely control the electronic structure of the alloy, designing the intrinsic stacking fault energy (0K) within the negative range of -95 to -89 mJ / m². This activates the microtwinning deformation mechanism during high-temperature deformation, achieving a synergistic effect between dislocation slip and microtwins. This fundamentally solves the problem of a sharp decline in plasticity caused by the single deformation mechanism (dislocation slip-dominated) and grain boundary weakening during high-temperature deformation of traditional cobalt-based alloys, aiming to achieve a simultaneous improvement in high-temperature strength and plasticity.
[0009] Guided by first-principles calculations, Ti and Ta were selected as key elements for controlling low stacking fault energy, with each added at no more than 4 wt%. The calculations focused on the effects of Ti and Ta on the electronic density of states (especially d electrons) near the Fermi level of the Co-Al-W matrix. Utilizing their specific electronic structure control capabilities, the stacking fault energy of the alloy was precisely and controllably reduced from the positive or near-zero values of conventional alloys to the target negative range, providing the necessary thermodynamic driving force for the nucleation and propagation of microtwins.
[0010] As a preferred embodiment of the above technical solution, the first-principles calculations were performed using the Vienna ab initio simulation software VASP; the generalized gradient approximation proposed by Perdew-Burke-Ernzerhof was used to describe the exchange-correlation functional; the ion-electron interaction was handled using a projected fused plane wave model; the cutoff energy of the plane wave expansion was set to 450 eV; geometric optimization used a 3×3×3 Monkhorst-Pack k-point grid; and the energy convergence criterion for the electron self-consistent field cycle was 10 eV. -6 eV / atom, in geometry optimization, the convergence criterion for the force on each atom is 10. -2 eV / Å.
[0011] Using first-principles calculations, the electronic structure of a Co-Al-W-based supercell model containing Ti and Ta is calculated, enabling reliable prediction of its generalized stacking fault energy surface, particularly the intrinsic stacking fault energy. This computational framework ensures computational accuracy and repeatability at the quantum mechanical level; for example, the high cutoff energy of 450 eV guarantees the completeness of the wave function expansion, and strict convergence criteria eliminate computational errors. This invention elevates material design from macroscopic experience to the electronic scale, providing a direct and reliable theoretical basis for the precise addition of Ti and Ta elements and their quantitative control over stacking fault energy.
[0012] As a preferred embodiment of the above technical solution, the Co-Al-W alloy as the basis specifically comprises Al 4~6wt%, W 8~12wt%, with the balance being Co or containing conventional optimized elements with a total amount not exceeding 15wt%.
[0013] Using a Co-Al-W ternary system as the matrix, the Al content is precisely controlled at 4~6 wt%, and the W content at 8~12 wt%. This composition range ensures that the alloy is stably located in the γ+γ′ two-phase region, and can obtain an L12-type γ′-Co3(Al, W) ordered strengthening phase with a volume fraction of not less than 50%, laying the microstructure foundation for high-temperature strength.
[0014] As a preferred embodiment of the above technical solution, the conventional optimization element is selected from at least one of Ni, Cr, Nb, Mo, Re, and B.
[0015] As a preferred embodiment of the above technical solution, the conventional optimization elements specifically include any combination of the following element contents:
[0016] a) Ni 2~5wt%;
[0017] b) Cr 5~8wt%
[0018] c) Nb 1~3wt%;
[0019] d) Mo 1~3wt%;
[0020] e) Re 0.5~2wt%;
[0021] f), B 0.005~0.02wt%.
[0022] The total amount of conventional optimized elements such as Ni, Cr, Nb, Mo, Re, and B does not exceed 15 wt%. Among them, Ni (2~5 wt%) is used to stabilize and expand the γ / γ′ two-phase region; Cr (5~8 wt%) ensures high-temperature oxidation and corrosion resistance; Nb, Mo, and Re (total amount controlled) provide solid solution strengthening and creep resistance; and B (0.005~0.02 wt%) agglomerates grain boundaries, playing a role in strengthening grain boundaries, inhibiting grain boundary diffusion, and preventing embrittlement. The elements work synergistically within their preferred content ranges, constructing a composition system that combines high thermal strength, excellent oxidation resistance, good creep resistance, and long-term structural stability without excessively increasing density or cost. This overcomes the potential environmental adaptability and grain boundary weakening problems of the pure Co-Al-W-Ti-Ta system, making it closer to the service requirements of actual high-temperature components.
[0023] As a further preferred embodiment of the above technical solution, the low stacking fault energy microtwin synergistic deformation cobalt-based alloy is based on the Co-Al-W alloy, with Ti content added at 3~4wt% and Ta content added at 3~4wt%.
[0024] At the optimal addition level of 3-4 wt%, a perfect balance between "precise control of stacking fault energy" and "γ′ phase strengthening" is achieved. This avoids the risks of insufficient addition leading to a non-negative stacking fault energy, or excessive addition (such as approaching the upper limit of 4 wt%) potentially increasing the tendency for precipitation of brittle Ti / Ta-rich phases, ensuring that the alloy achieves high plasticity without sacrificing strength and thermal stability.
[0025] Secondly, the present invention provides a method for preparing a cobalt-based alloy with low stacking fault energy and microtwin synergistic deformation.
[0026] The technical solution is as follows:
[0027] A method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy includes the following steps:
[0028] (1) Smelting: The cobalt-based alloy is batched and loaded into the furnace according to the above-mentioned method, and then smelted under vacuum and argon atmosphere.
[0029] (2) Casting and forging: The casting temperature is controlled at 1520~1580℃. After casting, the ingot is air-cooled. Before forging, the ingot is heated to 1160~1200℃, the initial forging temperature is 1140~1200℃, the final forging temperature is ≥900℃, and then air-cooled to obtain the forging billet.
[0030] (3) Cold working deformation: The forging billet is first subjected to solution heat treatment, and then subjected to multiple cold rolling deformations. The amount of reduction in each cold rolling pass shall not exceed 0.1 mm, and the total reduction shall be 40%~50%.
[0031] (4) Recrystallization annealing: The recrystallization annealing temperature is 1050℃±10℃, the holding time is not less than 20min, and then water quenching is performed to cool to room temperature;
[0032] (5) Aging heat treatment: The temperature of aging heat treatment is 850℃±10℃, and the aging time is not less than 10h.
[0033] As a preferred embodiment of the above technical solution, in step (2), the forging ratio is ≥3.
[0034] As a preferred embodiment of the above technical solution, in step (3), the forging billet is subjected to solution heat treatment at 1200℃ for 30 minutes.
[0035] As a preferred embodiment of the above technical solution, in step (3), the initial pressing amount is 0.05~0.1mm / pass, and after the total pressing amount reaches 30%, the pressing amount is 0.01~0.05mm / pass.
[0036] As a preferred embodiment of the above technical solution, in step (4), the heat preservation time is 30 minutes.
[0037] As a preferred embodiment of the above technical solution, the effective time in step (5) is 15 hours.
[0038] As a preferred embodiment of the above technical solution, in step (4), after cutting out tensile specimens from the plate after cold working deformation, recrystallization annealing is performed.
[0039] In the above-mentioned technical solution of the present invention, "process control" is transformed from "macro-process" into "quantifiable operation steps", which ensures the composite multi-scale structure of "high-density deformation defects + fine equiaxed crystals + dispersed γ' phase", providing an ideal carrier for the nucleation and growth of microtwins, and ultimately achieving the target performance.
[0040] Vacuum induction melting is employed under an inert atmosphere to ensure precise composition and low gas content. The casting temperature (1520~1580℃) and air cooling method help reduce segregation. The forging process (heating 1160~1200℃, initial forging 1140~1200℃, final forging ≥900℃, forging ratio ≥3) aims to fully break down the cast dendrites, eliminate porosity, refine the original grains, and provide a uniform billet for subsequent processing.
[0041] The forging billet undergoes solution treatment (e.g., 1200℃ / 30min) to dissolve the non-equilibrium phase and homogenize the composition. Subsequently, it undergoes strictly controlled multi-pass cold rolling with a total deformation of 40%–50%. By combining a relatively large initial reduction (0.05–0.1 mm / pass) with a fine reduction (0.01–0.05 mm / pass), high-density dislocations and deformation twins are introduced as recrystallization nucleation sites while minimizing cracking. Following this, recrystallization annealing is performed at 1050℃ (holding ≥20min, preferably 30min followed by water quenching) to obtain fine and uniform equiaxed recrystallized grains. Finally, long-term aging at 850℃ (≥10h, preferably 15h) promotes the precipitation of fine, dispersed, cubic γ′ phase, achieving peak strengthening. This combined process of "large deformation cold rolling + complete recrystallization + peak aging" is key to obtaining the ideal multi-scale composite microstructure of "high dislocation / twin storage energy + fine equiaxed γ matrix grains + dispersed nano-γ′ phase". Defects introduced by cold rolling drive recrystallization to refine the grains, while precisely controlled aging optimizes the size, morphology, and distribution of the γ′ phase. This microstructure is the ideal carrier for achieving the synergistic effect of "γ′ phase strengthening" and "microtwin toughening". The recrystallization temperature (1050℃) is lower than the complete dissolution temperature of the γ′ phase, preventing excessive grain growth; the aging temperature (850℃) matches the precipitation kinetics of the γ′ phase, facilitating the acquisition of a high volume fraction and thermally stable strengthening phase. A clearly defined process window ensures stable and controllable microstructure and properties.
[0042] In summary, the present invention has the following beneficial effects:
[0043] 1. Pioneering integration of strengthening and toughening mechanisms: This invention is the first to successfully construct a synergistic strengthening and toughening system in cobalt-based superalloys that combines “γ′ phase precipitation strengthening” and “low stacking fault energy-induced microtwin deformation”. This system breaks through the performance bottleneck caused by traditional reliance on a single mechanism, and utilizes microtwins to generate additional strengthening while improving plasticity, thereby achieving simultaneous optimization of high-temperature strength and plasticity.
[0044] 2. Excellent high-temperature mechanical properties: Under typical high-temperature service conditions of 850°C, the alloy of this invention exhibits a uniform elongation of up to 48% and a yield strength of over 480 MPa. This excellent combination of strength and plasticity significantly surpasses the level of existing γ′ phase-strengthened cobalt-based alloys, making it possible to use or reduce the weight of components under more demanding conditions, and directly expanding the application safety boundary.
[0045] 3. Reverse material design based on quantum mechanics calculations: First-principles calculations precisely target the key physical parameter of stacking fault energy, guiding the addition of Ti and Ta elements, achieving reverse and quantitative design from "performance requirements" to "composition design." This marks a paradigm shift in materials development from empirical trial and error to theoretical prediction and intelligent design, greatly improving the predictability and efficiency of R&D.
[0046] 4. Multi-scale, full-chain systematic optimization: This invention embodies full-chain innovation from the electronic scale (stack fault energy design), atomic scale (composition design), micro-nano scale (structure control) to the macro scale (process realization); the high synergy of composition, process, structure and performance ensures the feasibility, stability and repeatability of the excellent performance of the invented alloy, and has a solid industrialization foundation.
[0047] 5. Significant Engineering Application Value and Prospects: This alloy, while inheriting the inherent excellent resistance to hot corrosion and oxidation of cobalt-based alloys, overcomes the limitation of high-temperature plasticity, enabling its comprehensive performance to meet the higher temperature resistance and reliability requirements of hot-end components (such as high-pressure turbine blades and guide vanes) in next-generation high-performance aero-engines, gas turbines, and other power plants. The implementation of this invention is expected to promote the upgrading of related equipment, improve its thrust-to-weight ratio, thermal efficiency, and service life, and has significant strategic and economic benefits. Attached Figure Description
[0048] Figure 1 This is a microstructure image of the sample from Example 1 under a transmission electron microscope;
[0049] Figure 2 This is the tensile stress-strain curve of the sample in Example 1 at a high temperature of 850℃. Detailed Implementation
[0050] The present invention will be further explained and described below with reference to the accompanying drawings.
[0051] This specific embodiment is merely an explanation of the present invention and is not intended to limit the present invention. Any changes made by those skilled in the art after reading the specification of the present invention, as long as they are within the scope of the claims, will be protected by patent law.
[0052] Example 1
[0053] This embodiment provides a low stacking fault energy microtwin synergistic deformation cobalt-based alloy; the alloy is obtained by adding 3.7 wt% Ti and 3.8 wt% Ta to a Co-Al-W alloy.
[0054] Specifically, first-principles calculations were performed using the Vienna ab initio simulation software VASP; the generalized gradient approximation proposed by Perdew-Burke-Ernzerhof was used to describe the exchange-correlation functional; ion-electron interactions were handled using a projected coupled plane wave model; the cutoff energy of the plane wave expansion was set to 450 eV; geometry optimization used a 3×3×3 Monkhorst-Pack k-point grid; and the energy convergence criterion for the electron self-consistent field cycle was 10 eV. -6 eV / atom, in geometry optimization, the convergence criterion for the force on each atom is 10. -2 eV / Å; the stacking fault energy of this alloy at 0K is -93 mJ / m 2 .
[0055] Specifically, the composition of the Co-Al-W alloy is as follows:
[0056] Al 5.2 wt%, W 9.7 wt%, Ti 3.7 wt%, Ta 3.8 wt%, the balance is Co.
[0057] The preparation method of the above-mentioned low-layer fault energy microtwin synergistic deformation cobalt-based alloy is as follows:
[0058] Step 1: According to the above ingredient distribution, place the refractory and large pieces of material in the lower part of the crucible; fill the gaps between the large pieces with small pieces of material; place the small pieces of material loosely in the upper part; place the long rod-shaped materials vertically, with the bottom tightly packed and the top loose; add the components with low melting points last; after evacuating the vacuum induction furnace, fill it with the protective gas argon to start the melting process, with an initial power of 12KW; after melting is completed, proceed with casting, and control the casting temperature at 1550℃;
[0059] Step 2: Use wire electrical discharge machining to cut the ingot into metal plates with a thickness of 20mm each, perform solution treatment (temperature 1200℃, hold for 2h), and then water quench to cool to room temperature;
[0060] Step 3: Cold roll the metal sheet at room temperature. To prevent cracking during rolling, the initial reduction is controlled within the range of 0.05~0.08 mm / pass. After the total reduction reaches 30%, the reduction is controlled within the range of 0.02~0.04 mm / pass, and the final total reduction is controlled at about 40%.
[0061] Step 4: Perform recrystallization annealing on the rolled plate at a temperature of 1050℃ for 30 minutes, followed by water quenching to room temperature;
[0062] Step 5: Perform aging heat treatment (temperature 850℃, aging time 15h), and finally cut tensile specimens from the rolled plate for mechanical property testing.
[0063] like Figure 1 As shown, the novel cobalt-based superalloy prepared by this invention, after being subjected to high-temperature stretching, was found to contain microtwins and a strengthening phase γ' by transmission electron microscopy.
[0064] like Figure 2 As shown, the tensile yield strength, tensile strength and uniform elongation at 850℃ are 484MPa, 366MPa and 48%, respectively, exhibiting excellent strong and ductile properties at both room temperature and high temperature.
[0065] Experimental results show that this invention proposes a method for designing cobalt-based alloy composition based on first-principles control of stacking fault energy. By introducing elements with low stacking fault energy to construct a cobalt-based alloy system, the stacking fault energy threshold of the alloy is effectively reduced, and the new shear deformation mechanism of microtwins is successfully activated. This mechanism realizes the synergistic effect of dislocation slip and microtwin deformation at high temperature, thereby endowing the material with excellent comprehensive strength and plasticity.
[0066] Example 2
[0067] This embodiment provides a low stacking fault energy microtwin synergistic deformation cobalt-based alloy; the alloy is obtained by adding 3.7 wt% Ti and 3.8 wt% Ta to a Co-Al-W alloy.
[0068] Specifically, first-principles calculations were performed using the Vienna ab initio simulation software VASP; the generalized gradient approximation proposed by Perdew-Burke-Ernzerhof was used to describe the exchange-correlation functional; ion-electron interactions were handled using a projected coupled plane wave model; the cutoff energy of the plane wave expansion was set to 450 eV; geometry optimization used a 3×3×3 Monkhorst-Pack k-point grid; and the energy convergence criterion for the electron self-consistent field cycle was 10 eV. -6 eV / atom, in geometry optimization, the convergence criterion for the force on each atom is 10. -2 eV / Å; the stacking fault energy of this alloy at 0K is -92 mJ / m 2 .
[0069] Specifically, the composition of the Co-Al-W alloy is as follows:
[0070] Al 5.2 wt%, W 9.7 wt%, Ti 3.7 wt%, Ta 3.8 wt%, Ni 4.7wt%, Cr 5.6wt%, Nb2wt%, B 0.01wt%, and the balance is Co.
[0071] The preparation method of the above-mentioned low-layer fault energy microtwin synergistic deformation cobalt-based alloy is as follows:
[0072] Step 1: According to the above ingredient distribution, place the refractory and large pieces of material in the lower part of the crucible; fill the gaps between the large pieces with small pieces of material; place the small pieces of material loosely in the upper part; place the long rod-shaped materials vertically, with the bottom tightly packed and the top loose; add the components with low melting points last; after evacuating the vacuum induction furnace, fill it with the protective gas argon to start the melting process, with an initial power of 12KW; after melting is completed, proceed with casting, and control the casting temperature at 1550℃;
[0073] Step 2: Use wire electrical discharge machining to cut the ingot into metal plates with a thickness of 20mm each, perform solution treatment (temperature 1200℃, hold for 2h), and then water quench to cool to room temperature;
[0074] Step 3: Cold roll the metal sheet at room temperature. To prevent cracking during rolling, the initial reduction is controlled within the range of 0.05~0.08 mm / pass. After the total reduction reaches 30%, the reduction is controlled within the range of 0.02~0.04 mm / pass, and the final total reduction is controlled at about 40%.
[0075] Step 4: Perform recrystallization annealing on the rolled plate at a temperature of 1050℃ for 30 minutes, followed by water quenching to room temperature;
[0076] Step 5: Perform aging heat treatment (temperature 850℃, aging time 15h).
[0077] Example 3
[0078] This embodiment provides a low stacking fault energy microtwin synergistic deformation cobalt-based alloy; the alloy is obtained by adding 3.7 wt% Ti and 3.8 wt% Ta to a Co-Al-W alloy.
[0079] Specifically, first-principles calculations were performed using the Vienna ab initio simulation software VASP; the generalized gradient approximation proposed by Perdew-Burke-Ernzerhof was used to describe the exchange-correlation functional; ion-electron interactions were handled using a projected coupled plane wave model; the cutoff energy of the plane wave expansion was set to 450 eV; geometry optimization used a 3×3×3 Monkhorst-Pack k-point grid; and the energy convergence criterion for the electron self-consistent field cycle was 10 eV. -6eV / atom, in geometry optimization, the convergence criterion for the force on each atom is 10. -2 eV / Å; the stacking fault energy of this alloy at 0K is -92 mJ / m 2 .
[0080] Specifically, the composition of the Co-Al-W alloy is as follows:
[0081] Al 5.2 wt%, W 9.7 wt%, Ti 3.7 wt%, Ta 3.8 wt%, Ni 4.7wt%, Cr 5.6wt%, Mo2wt%, B 0.01wt%, and the balance is Co.
[0082] The preparation method of the above-mentioned low-layer fault energy microtwin synergistic deformation cobalt-based alloy is as follows:
[0083] Step 1: According to the above ingredient distribution, place the refractory and large pieces of material in the lower part of the crucible; fill the gaps between the large pieces with small pieces of material; place the small pieces of material loosely in the upper part; place the long rod-shaped materials vertically, with the bottom tightly packed and the top loose; add the components with low melting points last; after evacuating the vacuum induction furnace, fill it with the protective gas argon to start the melting process, with an initial power of 12KW; after melting is completed, proceed with casting, and control the casting temperature at 1550℃;
[0084] Step 2: Use wire electrical discharge machining to cut the ingot into metal plates with a thickness of 20mm each, perform solution treatment (temperature 1200℃, hold for 2h), and then water quench to cool to room temperature;
[0085] Step 3: Cold roll the metal sheet at room temperature. To prevent cracking during rolling, the initial reduction is controlled within the range of 0.05~0.08 mm / pass. After the total reduction reaches 30%, the reduction is controlled within the range of 0.02~0.04 mm / pass, and the final total reduction is controlled at about 40%.
[0086] Step 4: Perform recrystallization annealing on the rolled plate at a temperature of 1050℃ for 30 minutes, followed by water quenching to room temperature;
[0087] Step 5: Perform aging heat treatment (temperature 850℃, aging time 15h).
Claims
1. A low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy, characterized in that: The cobalt-based alloy is based on a Co-Al-W alloy. After first-principles calculations, no more than 4 wt% of Ti (a first optimized element) and no more than 4 wt% of Ta (a second optimized element) are added to control the stacking fault energy of the cobalt-based alloy at -95 mJ / m at 0 K. 2 ~ -89 mJ / m 2 .
2. The low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 1, characterized in that: First-principles calculations were performed using the Vienna ab initio simulation software VASP; the generalized gradient approximation proposed by Perdew-Burke-Ernzerhof was used to describe the exchange-correlation functional; ion-electron interactions were handled using a projected fused plane wave model; the cutoff energy of the plane wave expansion was set to 450 eV; geometry optimization used a 3×3×3 Monkhorst-Pack k-point grid; and the energy convergence criterion for the electron self-consistent field cycle was 10 eV. -6 eV / atom, in geometry optimization, the convergence criterion for the force on each atom is 10. -2 eV / Å.
3. The low stacking fault energy microtwin-coordinated deformation cobalt-based alloy according to claim 1, characterized in that: The basic Co-Al-W alloy specifically comprises 4~6wt% Al, 8~12wt% W, with the balance being Co or containing conventionally optimized elements in total not exceeding 15wt%; the conventionally optimized elements are selected from at least one of Ni, Cr, Nb, Mo, Re, and B.
4. A low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 3, characterized in that: Based on the Co-Al-W alloy, the amount of Ti added is 3~4wt%, and the amount of Ta added is 3~4wt%.
5. A method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to any one of claims 1 to 4, comprising the following steps: (1) Smelting: The cobalt-based alloy according to any one of claims 1 to 4 is batched and loaded into a furnace, and then smelted under vacuum and argon atmosphere; (2) Casting and forging: The casting temperature is controlled at 1520~1580℃. After casting, the ingot is air-cooled. Before forging, the ingot is heated to 1160~1200℃, the initial forging temperature is 1140~1200℃, the final forging temperature is ≥900℃, and then air-cooled to obtain the forging billet. (3) Cold working deformation: The forging billet is first subjected to solution heat treatment, and then subjected to multiple cold rolling deformations. The amount of reduction in each cold rolling pass shall not exceed 0.1 mm, and the total reduction shall be 40%~50%. (4) Recrystallization annealing: The recrystallization annealing temperature is 1050℃±10℃, the holding time is not less than 20min, and then water quenching is performed to cool to room temperature; (5) Aging heat treatment: The temperature of aging heat treatment is 850℃±10℃, and the aging time is not less than 10h.
6. The method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 5, characterized in that: In step (2), the forging ratio is ≥3.
7. The method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 5, characterized in that: In step (3), the forging billet is subjected to solution heat treatment at 1200℃ for 30 minutes.
8. The method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 5, characterized in that: In step (3), the initial pressing amount is 0.05~0.1 mm / pass, and after the total pressing amount reaches 30%, the pressing amount is 0.01~0.05 mm / pass.
9. The method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 5, characterized in that: In step (4), the heat preservation time is 30 minutes.
10. The method for preparing a low-stacking-fault-energy microtwin-coordinated deformation cobalt-based alloy according to claim 5, characterized in that: In step (5), the time limit is 15 hours.
Citation Information
Patent Citations
A rhenium-containing, high-temperature oxidation-resistant γ′ phase-strengthened cobalt-based superalloy and its preparation method
CN115161517B