Special antibacterial coating with nano silicon dioxide core-shell structure for medical equipment
The composite antibacterial coating with a nano-silica core-shell structure solves the contradiction between cytotoxicity, adhesion and thickness of silver-based antibacterial coatings, achieving highly efficient broad-spectrum antibacterial properties and excellent biocompatibility, making it suitable for medical devices.
Patent Information
- Application Number
- CN202511979647.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-25
- Publication Date
- 2026-05-08
AI Technical Summary
Existing silver-based antibacterial coatings suffer from problems such as high silver loading leading to cytotoxicity, contradiction between adhesion and coating thickness, limited antibacterial spectrum, difficulty in balancing long-term effectiveness and safety, and single function.
By employing a nano-silica core-shell structure, silver nanoparticles and ZnO quantum dots are loaded in situ onto a medical-grade nano-silica carrier, and combined with a PLGA polymer matrix and heparin, a composite antibacterial coating is constructed. Using microwave-assisted in situ reduction and gradient curing processes, ultra-high broad-spectrum antibacterial properties, excellent biocompatibility, and strong adhesion are achieved.
It achieves high antibacterial rate, low cytotoxicity, ultra-thin thickness, broad spectrum coverage and long-lasting sustained release. The coating maintains excellent adhesion under humid and hot conditions, has a high cell survival rate, and releases silver ions safely, making it suitable for precision medical devices.
Abstract
Description
Technical Field
[0001] This invention relates to the field of antibacterial coating technology, specifically to an antibacterial coating for medical devices with a nano-silica core-shell structure. Background Technology
[0002] Medical device-associated infections (HAIs) pose a significant challenge in clinical treatment, and applying antimicrobial coatings to the surfaces of medical devices is an effective means of preventing such infections. Silver nanoparticles are widely used in antimicrobial coatings due to their broad-spectrum antimicrobial properties. However, existing silver-based antimicrobial coatings generally suffer from the following drawbacks:
[0003] 1. The contradiction between antibacterial spectrum and toxicity: To achieve a high antibacterial rate (e.g., above 99.995%), a high silver loading is often required, but this can easily lead to an initial burst release of silver ions, causing cytotoxicity and reducing biosafety (low cell survival rate). At the same time, single silver antibacterial components have limited inhibitory effects on fungi and their antibacterial spectrum is not broad enough.
[0004] 2. Conflict between adhesion and coating design: In order to obtain strong adhesion that meets the requirements of medical device use (such as 5B grade), more adhesion promoters or increased coating thickness are often required. However, this may affect the uniformity and flexibility of the coating or lead to an excessively thick coating, which is not suitable for precision or ultra-thin instruments.
[0005] 3. The contradiction between long-lasting effect and safety: How to control the release kinetics of silver ions so that they can take effect quickly and release slowly over a long period of time, avoiding excessive release (burst release) in a short period of time that could cause toxicity, and at the same time avoiding premature depletion of antibacterial ability, is a technical challenge.
[0006] 4. Limited functionality: Most coatings focus on antibacterial properties, with insufficient attention paid to potential inflammatory responses that may be caused by implanted or contact devices, and lack designs that improve anti-inflammatory properties or improve blood compatibility.
[0007] Therefore, developing a composite antibacterial coating that can balance the above contradictions, namely, having ultra-high antibacterial rate, low cytotoxicity, strong adhesion, ultra-thin thickness, broad-spectrum antibacterial (covering bacteria and fungi) and good biocompatibility, is a technical problem that urgently needs to be solved in the field of medical device surface modification. Summary of the Invention
[0008] (I) Technical Issues
[0009] The present invention aims to provide a nano-silica core-shell structure antibacterial coating for medical devices that simultaneously possesses ultra-high broad-spectrum antibacterial properties, excellent biocompatibility, strong adhesion, and ultra-thin structural characteristics, in order to overcome the contradictions between high silver loading and low toxicity, strong adhesion and ultra-thin thickness, and antibacterial spectrum coverage and long-term sustained release in the prior art.
[0010] (II) Technical Content
[0011] To solve the above-mentioned technical problems, the technical solution of the present invention is: a medical device-specific antibacterial coating with a nano-silica core-shell structure, comprising the following components:
[0012] Medical-grade nano-silicon carrier with a particle size of 5±1 nm, PDI<0.1, and surface hydroxyl density ≥3.5 groups / nm. 2 BET specific surface area ≥ 400m² 2 / g;
[0013] Silver nanoparticles with a particle size of 2-5 nm are in situ loaded on the nano-silicon carrier.
[0014] ZnO quantum dots were coated onto the surface of the nano-silicon carrier using a sol-gel method;
[0015] A PLGA polymer matrix containing heparin grafting density ≥0.6 μg / cm³ 2 ;
[0016] The adhesion enhancer is γ-aminopropyltriethoxysilane;
[0017] Dispersants, crosslinking agents, and defoamers.
[0018] Furthermore, the mass percentages of the components in the antibacterial coating are as follows: 65% medical-grade nano-silicon carrier, 4% silver nanoparticles, 1.5% ZnO quantum dots, 10% PLGA polymer matrix, 0.8% heparin, 12% adhesion enhancer, 2.5% dispersant, 0.8% crosslinking agent, and 0.2% defoamer, wherein the silver nanoparticles are in Ag... + Calculate the content.
[0019] Furthermore, silver nanoparticles were loaded onto the medical-grade nano-silicon carrier using a microwave-assisted in-situ reduction method, with microwave conditions of 50°C, 5 min, and 300 W.
[0020] Furthermore, the heparin is directionally grafted onto the PLGA surface via plasma treatment, with a plasma treatment power of 50W and an Ar atmosphere.
[0021] Furthermore, the molecular weight of the PLGA polymer matrix is 15-30 kDa, and the glass transition temperature is 45-50 °C.
[0022] Furthermore, ZnO quantum dots are coated onto the surface of a medical-grade nano-silicon carrier using a sol-gel method, and the particle size of the ZnO quantum dots is 3-5 nm.
[0023] Furthermore, the crosslinking agent is glutaraldehyde, and the pencil hardness of the cured coating is ≥2H.
[0024] Furthermore, the coating is prepared by a process including electrostatic spraying and gradient curing; the gradient curing involves pre-curing at 80°C followed by UV post-treatment.
[0025] Furthermore, the coating thickness is less than 5 μm, and the surface roughness Ra < 0.5 μm.
[0026] Furthermore, the coating exhibits a 24-hour inhibition rate of ≥99.95% against Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, and Candida albicans, a cell viability rate >96% as measured by ISO10993-5 standard, and an adhesion rating of 5B as measured by ASTMD3359 standard.
[0027] (III) Technical Effects
[0028] The advantages of this invention compared to the prior art are:
[0029] 1. By constructing a "core (nanosilicon-loaded Ag / ZnO)-shell (PLGA / heparin)" composite structure with a medical-grade nanosilicon carrier with excellent monodispersity (PDI<0.1) as the core, the cell survival rate under high silver loading (4%) was successfully increased to over 96%, while the adhesion reached 5B level and the coating thickness was controlled below 5μm. This solved the technical contradiction of the difficulty in achieving both high antibacterial properties, low toxicity, strong adhesion and ultra-thin design.
[0030] 2. Silver nanoparticles (Ag) + The dual antibacterial mechanism of silver ion release (silver ions) and ZnO quantum dots (photocatalytic generation of reactive oxygen species, ROS) produces a synergistic effect, achieving an inhibition rate of over 99.995% against Gram-positive and Gram-negative bacteria, and a significantly improved inhibition rate of 99.95% against fungi such as Candida albicans, achieving true broad-spectrum coverage. Through loading on a nano-silicon carrier and encapsulation on a PLGA matrix, the release kinetics of silver ions are effectively regulated, resulting in a low 24-hour burst release (<0.42 ppm) and a 7-day cumulative release rate of only 47.2%, achieving a long-lasting and mild antibacterial effect while reducing silver waste and the risk of toxic side effects.
[0031] 3. Using a specific amount of APTES as an adhesion enhancer, combined with a gradient curing process of 80℃ pre-curing + UV post-treatment, the coating maintains excellent adhesion (4B grade or higher) even under humid and hot conditions. Taber abrasion resistance testing shows high silver retention (>86%) after 1000 cycles, indicating good physical durability of the coating. The PLGA polymer matrix provides a good biocompatibility basis, and the surface-grafted heparin effectively inhibits the release of inflammatory factors (such as IL-6), thereby minimizing cytotoxicity (cell survival rate >96%), with a hemolysis rate of less than 0.5%, negative intradermal irritation test, and high overall biocompatibility.
[0032] 4. The functions of each component in the formula are clearly defined, and the proportions have been optimized. The process parameters of the microwave-assisted in-situ reduction method, electrostatic spraying, and gradient curing are clear, with good repeatability and high production yield (up to 95%), which is conducive to large-scale production and quality control. Detailed Implementation
[0033] The present invention will be further described in detail below with reference to the embodiments. The following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, all percentages are mass percentages (wt%).
[0034] Example 1: Preparation of a coating with high antibacterial and biocompatible properties
[0035] Step 1: Preparation of the core antibacterial material (nano-silicon supported Ag / ZnO)
[0036] 1. Pretreatment of nano-silica carrier: Take 65 grams of medical-grade nano-silica powder (particle size: 5±1nm, PDI: 0.08, surface hydroxyl density: 3.8 groups / nm). 2 BET specific surface area: 420m² 2 / g), placed in a 500mL three-necked flask, added 200mL of ethanol / water mixed solvent with a volume ratio of 7:3, and ultrasonically dispersed in an ultrasonic cell disruptor for 30 minutes to form a uniform nano silica sol.
[0037] 2. Loading of silver nanoparticles: A calculated amount of silver nitrate solution (equivalent to 4 grams of Ag) was added to the above sol. + The mixture was stirred thoroughly. Then, it was treated for 5 minutes in a microwave-assisted reactor (power set to 300W) under continuous stirring at 50℃, while freshly prepared sodium borohydride reducing agent solution was added dropwise. After the reaction, the nano-silicon carrier (Ag@SiO2) loaded with silver nanoparticles was obtained by high-speed centrifugation and washing three times with ethanol. TEM analysis showed that the silver nanoparticles had a particle size of 3±1nm and were uniformly distributed. ICP-MS determined the loading efficiency to be 99.1%.
[0038] 3. ZnO quantum dot composite: The above Ag@SiO2 material was redispersed in ethanol. Zinc nitrate and urea were added at a Zn / Si molar ratio of 1:20, and the reaction was carried out using the sol-gel method at 60°C with stirring for 6 hours. After the reaction, the mixture was centrifuged and dried to obtain the final core material (Ag / ZnO@SiO2) composited with ZnO quantum dots. TEM showed that the ZnO quantum dots had a particle size of approximately 4 nm and were uniformly coated on the surface of the silicon support.
[0039] Step 2: Preparation of coating solution
[0040] Prepare the coating mixture solution according to the following mass percentages:
[0041] Ag / ZnO@SiO2 core material (from step 1): 65%
[0042] PLGA polymer (molecular weight: 20 kDa, Tg: 48℃): 10%
[0043] Adhesion enhancer γ-aminopropyltriethoxysilane (APTES): 12%
[0044] Dispersant: Polyethylene glycol 400 (PEG400): 2.5%
[0045] Crosslinking agent glutaraldehyde (50% aqueous solution): 0.8%
[0046] Organosilicon defoamer: 0.2%
[0047] Deionized water / ethanol mixed solvent (7:3 v / v): bring to 100% to adjust the solution viscosity to 18 mPa·s (25°C).
[0048] Add all the above components in sequence and stir on a magnetic stirrer in the dark for 12 hours to form a uniform and stable coating precursor solution.
[0049] Step 3: Coating preparation and curing
[0050] 1. Substrate treatment: The medical-grade 316L stainless steel test piece (50mm×50mm) was ultrasonically cleaned with acetone and ethanol in sequence, and then dried with nitrogen.
[0051] 2. Electrostatic spraying: Load the solution prepared in step 2 into the electrostatic spraying equipment. Set the parameters: spraying voltage 30kV, liquid flow rate 0.8mL / min, spray gun distance from the substrate 15cm, and moving speed 10cm / s. Spray for a total of 3 cycles, and after each cycle, dry for 10 minutes at 40℃ and 30% relative humidity.
[0052] 3. Gradient Curing: After spraying, place the sample in a forced-air drying oven and pre-cur it at 80°C for 30 minutes. Then, transfer the sample to a UV curing oven and irradiate it under 365nm UV light for 5 minutes to complete the final curing.
[0053] Example 2: Preparation of a coating with optimized sustained-release and anti-inflammatory properties (two-component system)
[0054] Step 1: Preparation of core antibacterial materials
[0055] 1. Pretreatment of nano-silica carrier: Take 65 grams of medical-grade nano-silica powder (particle size: 5±1nm, PDI: 0.08, surface hydroxyl density: 3.8 groups / nm). 2 BET specific surface area: 420m² 2 / g), placed in a 500mL three-necked flask, added 200mL of ethanol / water mixed solvent with a volume ratio of 7:3, and ultrasonically dispersed in an ultrasonic cell disruptor for 30 minutes to form a uniform nano silica sol.
[0056] 2. Loading of silver nanoparticles: A calculated amount of silver nitrate solution (equivalent to 4 grams of Ag) was added to the above sol. + The mixture was stirred thoroughly. Then, it was treated for 5 minutes in a microwave-assisted reactor (power set to 300W) under continuous stirring at 50℃, while freshly prepared sodium borohydride reducing agent solution was added dropwise. After the reaction, the nano-silicon carrier (Ag@SiO2) loaded with silver nanoparticles was obtained by high-speed centrifugation and washing three times with ethanol. TEM analysis showed that the silver nanoparticles had a particle size of 3±1nm and were uniformly distributed. ICP-MS determined the loading efficiency to be 99.1%.
[0057] 3. ZnO quantum dot composite: The above Ag@SiO2 material was redispersed in ethanol. Zinc nitrate and urea were added at a Zn / Si molar ratio of 1:20, and the reaction was carried out using the sol-gel method at 60°C with stirring for 6 hours. After the reaction, the mixture was centrifuged and dried to obtain the final core material (Ag / ZnO@SiO2) composited with ZnO quantum dots. TEM showed that the ZnO quantum dots had a particle size of approximately 4 nm and were uniformly coated on the surface of the silicon support.
[0058] Step 2: Preparation of coating solution (two-component system)
[0059] To optimize the process, an A / B two-component system is used, which is mixed just before spraying:
[0060] Component A: Contains all of the Ag / ZnO@SiO2 core material (65%). It is uniformly dispersed in a partial ethanol / water (7:3) mixed solvent.
[0061] Component B comprises the entire PLGA polymer matrix (10%), adhesion enhancer APTES (12%), and the amounts of heparin (0.8%), dispersant PEG400 (2.5%), crosslinking agent glutaraldehyde (0.8%), and defoamer (0.2%) as specified in the formulation. Dissolve or disperse the above components in the remaining solvent and stir until homogeneous to form a uniform polymer solution.
[0062] Before spraying, mix components A and B quickly at a volume ratio of 1:1 and stir for 30 minutes to form the final coating liquid.
[0063] Step 3: Coating preparation and curing
[0064] 1. Substrate Treatment and Spraying: Medical-grade 316L stainless steel test pieces (50mm × 50mm) were ultrasonically cleaned sequentially with acetone and ethanol, then dried with nitrogen. The solution prepared in step 2 was loaded into the electrostatic spraying equipment. Parameters were set as follows: spraying voltage 30kV, liquid flow rate 0.8mL / min, spray gun distance from the substrate 15cm, and moving speed 10cm / s. Three spraying cycles were performed, followed by drying at 40℃ and 30% relative humidity for 10 minutes after each cycle.
[0065] 2. Gradient Curing: After spraying, place the sample in a forced-air drying oven and pre-cur at 80°C for 30 minutes. This step allows the coating to initially form a film, and the PLGA substrate is formed.
[0066] 3. Plasma treatment (heparin-directed grafting): The pre-cured sample is placed in the reaction chamber of a plasma cleaner. After evacuation, argon gas (Ar) is introduced to the working pressure and treated at 50W power for a certain time (e.g., 5-10 minutes). This process generates active sites on the surface of the PLGA film, achieving in-situ directional grafting of heparin molecules.
[0067] 4. UV post-curing: After plasma treatment, the sample is immediately transferred to a UV curing chamber and irradiated under UV light at a wavelength of 365nm for 5 minutes to complete the final cross-linking and curing, and fix the coating structure.
[0068] Performance Tests and Results
[0069] The coating samples obtained in Examples 1 and 2 were subjected to key performance tests according to the standard methods described in international or relevant national standards. The results are shown in the table below:
[0070] Test Project Test standards / methods Example 1 Example 2 Coating thickness White light interferometer 4.1±0.2μm 4.3±0.2μm Surface roughness Ra White light interferometer 0.42μm 0.38μm Adhesion (after wet heat) ASTM D3359 4B level 5B level Pencil hardness ISO15184 2H 2H Antibacterial rate (24h, Escherichia coli) ISO20743 99.997% 99.998% Antibacterial rate (24h, Candida albicans) ISO20743 99.95% 99.96% Cell viability ISO 10993-5 (MTT Method) 97.2±1.2% 97.5±1.0% hemolysis rate YY / T0616 0.38% 0.35% Silver ion burst release 24 hours AAS method (PBS, 37℃) 0.42ppm 0.40ppm 7-day cumulative release rate AAS method (PBS, 37℃) 47.2% 46.8% Abrasion resistance (Ag retention rate after 1000 cycles) Taber abrasion tester 86.5% 87.0%
[0071] The present invention and its embodiments have been described above. This description is not restrictive, and the embodiments shown are only one of the embodiments of the present invention. The actual structure is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar structures and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.
Claims
1. A nano-silica core-shell structured antibacterial coating for medical devices, characterized in that, It contains the following components: Medical-grade nano-silicon carrier with a particle size of 5±1 nm, PDI<0.1, and surface hydroxyl density ≥3.5 groups / nm. 2 BET specific surface area ≥ 400m² 2 / g; Silver nanoparticles with a particle size of 2-5 nm are in situ loaded on the nano-silicon carrier. ZnO quantum dots were coated onto the surface of the nano-silicon carrier using a sol-gel method; A PLGA polymer matrix containing heparin grafting density ≥0.6 μg / cm³ 2 ; The adhesion enhancer is γ-aminopropyltriethoxysilane; Dispersants, crosslinking agents, and defoamers.
2. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, The antibacterial coating comprises the following components by mass percentage: 65% medical-grade nano-silicon carrier, 4% silver nanoparticles, 1.5% ZnO quantum dots, 10% PLGA polymer matrix, 0.8% heparin, 12% adhesion enhancer, 2.5% dispersant, 0.8% crosslinking agent, and 0.2% defoamer. The silver nanoparticles are in Ag... + Calculate the content.
3. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, Silver nanoparticles were loaded onto the medical-grade nano-silicon carrier using a microwave-assisted in-situ reduction method. The microwave conditions were 50°C, 5 min, and 300 W.
4. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, The heparin was directionally grafted onto the PLGA surface via plasma treatment at a power of 50W in an Ar atmosphere.
5. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, The PLGA polymer matrix has a molecular weight of 15-30 kDa and a glass transition temperature of 45-50℃.
6. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, ZnO quantum dots are coated onto the surface of a medical-grade nano-silicon carrier using a sol-gel method, and the particle size of the ZnO quantum dots is 3-5 nm.
7. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, The crosslinking agent used is glutaraldehyde, and the hardness of the coated pencil after curing is ≥2H.
8. The antibacterial coating for medical devices with a nano-silica core-shell structure according to claim 1, characterized in that, The coating is prepared by a process including electrostatic spraying and gradient curing; the gradient curing involves pre-curing at 80°C followed by UV post-treatment.
9. A medical device-specific antibacterial coating with a nano-silica core-shell structure according to any one of claims 1-8, characterized in that, The coating has a thickness of less than 5 μm and a surface roughness Ra < 0.5 μm.
10. A nano-silica core-shell structured antibacterial coating for medical devices according to any one of claims 1-8, characterized in that, The coating exhibits a 24-hour inhibition rate of ≥99.95% against Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, and Candida albicans, a cell viability rate >96% as measured by ISO10993-5, and an adhesion rating of 5B as measured by ASTMD3359.