Hard and tough alternately-laminated light-weight corrosion-resistant composite material and preparation method thereof
By combining a hard and tough alternating laminate structure with a conductive polymer coating, the shortcomings of lightweight materials in terms of corrosion resistance and impact resistance are solved, resulting in a high-strength, low-density composite material with excellent comprehensive performance.
Patent Information
- Application Number
- CN202610360778.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-24
- Publication Date
- 2026-05-08
AI Technical Summary
Existing lightweight materials face the challenge of balancing comprehensive performance in aerospace, transportation, and marine engineering, especially in terms of corrosion resistance and impact resistance. Traditional connection methods are prone to interfacial strength attenuation and galvanic corrosion.
It adopts a hard and tough alternating layered structure, which is formed by plasma activation treatment on the aluminum alloy surface to create a nanoscale rough structure and carbon fiber reinforced thermoplastic resin layer, and combined with a conductive polymer anti-corrosion coating to form an interface that combines mechanical interlocking and chemical bonding, and provides active electrochemical protection.
A high-impact, low-density composite material has been developed, which possesses excellent corrosion resistance and interfacial strength, effectively inhibits galvanic corrosion, and improves the material's overall mechanical properties and protective capabilities.
Smart Images

Figure CN121989522A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of composite materials, and in particular relates to a lightweight corrosion-resistant composite material with alternating hard and tough layers and its preparation method. Background Technology
[0002] Lightweight materials are increasingly used in aerospace, transportation, and marine engineering, but existing lightweight material systems often face the technical challenge of balancing overall performance. While lightweight metals such as aluminum alloys have low density and good processability, their impact and wear resistance and environmental corrosion resistance are insufficient, especially in corrosive environments such as the marine atmosphere, where pitting corrosion and intergranular corrosion are prominent problems. Carbon fiber reinforced resin matrix composites have the advantages of high specific strength and high specific modulus, but their interlaminar impact resistance is weak, making them prone to delamination damage under impact loads, and they are susceptible to galvanic corrosion when connected to metal components.
[0003] In existing technologies, adhesive bonding or mechanical joining methods are commonly used to address the bonding issues between metals and composite materials. Adhesive bonding interfaces are susceptible to environmental aging, resulting in significant weakening of interface strength. Mechanical joining disrupts fiber continuity and introduces stress concentration points, while the connecting pores become channels for corrosive media intrusion. For corrosion protection, the traditional method involves applying anti-corrosion coatings to the material surface. However, these coatings are mostly passive physical barriers; their protective effect fails once mechanical damage occurs, and they cannot effectively suppress galvanic corrosion that occurs when dissimilar materials come into contact.
[0004] Although some studies in recent years have attempted to laminate metals and composite materials to achieve complementary properties, insufficient interfacial bonding strength and lack of system corrosion resistance remain key factors restricting their engineering applications. Summary of the Invention
[0005] One object of the present invention is to provide a lightweight corrosion-resistant composite material with alternating hard and tough layers, and another object of the present invention is to provide a method for preparing the lightweight corrosion-resistant composite material with alternating hard and tough layers.
[0006] To achieve the first objective of this invention, the following technical solution is adopted: A lightweight, corrosion-resistant composite material with alternating layers of hard and tough materials, comprising: The laminated matrix is composed of alternating layers of high-strength aluminum alloy and carbon fiber reinforced thermoplastic resin. The metallurgical-mechanical composite interface is located between the high-strength aluminum alloy layer and the carbon fiber reinforced thermoplastic resin layer. A nanoscale rough structure is formed on the surface of the aluminum alloy through plasma activation treatment, and it is combined with the thermoplastic resin matrix to form a transition region that has both mechanical interlocking and chemical bonding. A conductive polymer anti-corrosion coating is applied to the outermost surface of the laminated matrix.
[0007] In this invention, the laminated matrix forms a macroscopically alternating hard and tough structure. Specifically, the laminated matrix uses a high-strength aluminum alloy layer as the outer hard load-bearing and wear-resistant unit, and a carbon fiber reinforced thermoplastic resin layer as the inner tough support and energy absorption unit. Both layers are stacked alternately in a periodic sequence of "aluminum layer-composite layer-aluminum layer" on a macroscopic scale, forming a heterogeneous periodic structure with significant acoustic impedance differences. This spatially ordered alternation of hardness (metal) and toughness (composite material) is not a simple layering of materials, but rather the construction of a novel multi-level energy management and dissipation configuration. Under dynamic impact loads, the outer hard aluminum alloy layer first resists intrusion and cutting; the impact energy is then transferred to the inner tough composite material layer, where it is largely absorbed through micro-cracking of the matrix and plastic deformation of the fiber bundles; simultaneously, stress waves undergo repeated reflection and refraction at the periodically changing heterogeneous interface, further dissipating the energy, thus achieving a level of impact resistance and damage tolerance far exceeding the simple superposition of the properties of individual components.
[0008] In this invention, the metallurgical-mechanical composite interface is a transition region formed in situ by plasma activation treatment of the aluminum alloy layer surface with specific parameters before lamination molding. This treatment process utilizes high-energy particles to physically bombard and chemically modify the aluminum alloy surface, achieving two effects: first, it etches a uniformly distributed nanoscale peak-valley structure on the aluminum alloy surface, significantly increasing surface roughness and specific surface area, providing sufficient mechanical anchoring points for the subsequently molten thermoplastic resin, forming a strong mechanical interlocking effect; second, by introducing oxygen-containing active groups, it greatly enhances the chemical activity and free energy of the aluminum alloy surface, transforming it from a hydrophobic to a superhydrophilic state. This not only promotes complete wetting and spreading of the molten resin but also facilitates the formation of stable chemical bonds or strong physical adsorption between the polar groups in the resin and the active sites on the metal surface. Thus, during the hot-press co-curing process, this region achieves a continuous gradient transition in modulus and properties from the metal to the resin matrix, forming an interface layer with both high strength and high toughness, fundamentally replacing traditional adhesive or mechanical bonding methods.
[0009] In this invention, the conductive polymer anti-corrosion coating provides active electrochemical protection. Specifically, the conductive polymer anti-corrosion coating covers the outermost surface of the laminated substrate. Its function differs from traditional passive isolation coatings; it is an active protection system with anodic passivation capabilities. This coating uses intrinsically conductive polymers such as polyaniline and polypyrrole as functional materials, and their high redox potential characteristics allow them to act as stable cathodes in the electrolyte. When the coating suffers localized damage due to mechanical stress, the exposed aluminum alloy substrate acts as the anode, and the conductive polymer coating acts as the cathode. In the micro-electrochemical environment formed between them, the coating continuously drives a passivation reaction on the aluminum anode surface, promoting the in-situ formation and repair of the alumina protective film. Its active passivation mechanism can suppress the corrosion current density to an extremely low level. Simultaneously, the dense physical structure of the coating itself effectively blocks the penetration of corrosive media such as water, oxygen, and chloride ions. This dual protection mechanism, from physical barriers to electrochemical intervention, provides a systematic solution for galvanic corrosion problems in layered heterostructures.
[0010] Preferably, in the laminated matrix, the total number of high-strength aluminum alloy layers and carbon fiber reinforced thermoplastic resin layers is odd, with the high-strength aluminum alloy layer serving as both the starting and ending layer.
[0011] Preferably, the single-layer thickness of the high-strength aluminum alloy layer is 0.1-0.5 mm; the matrix of the carbon fiber reinforced thermoplastic resin layer is polyetheretherketone, polyphenylene sulfide or polyetherimide, the fiber volume content is 50-65%, and the single-layer thickness is 0.1-0.3 mm.
[0012] Preferably, in the metallurgical-mechanical composite interface, the arithmetic mean roughness Ra of the aluminum alloy surface after plasma activation treatment is 150-300 nm, and the contact angle is less than 10°. This allows the metallurgical-mechanical composite interface to exhibit a superhydrophilic state. This surface state is beneficial for the wetting and spreading of the resin melt, forming a strong interfacial bond.
[0013] Preferably, the conductive polymer anti-corrosion coating is a coating formed by combining polyaniline, polypyrrole, or polythiophene-based conductive polymers with a resin matrix, and the dry film thickness of the conductive polymer anti-corrosion coating is 20-50 μm. The conductive polymer anti-corrosion coating not only provides a physical barrier but also plays a cathodic protection role at localized damage points in the coating, driving the formation of a passivation film on the metal surface.
[0014] To achieve the second objective of this invention, the following technical solution is adopted: A method for preparing a lightweight corrosion-resistant composite material with alternating hard and tough layers as described above includes the following steps: S1. Surface pretreatment: The surface of the high-strength aluminum alloy sheet is ultrasonically cleaned and degreased using organic solvents. S2. Plasma activation treatment: Atmospheric pressure plasma treatment is applied to the cleaned aluminum alloy surface to form a nanoscale rough structure and improve the surface energy. S3. Laying out layers: The treated aluminum alloy layer and carbon fiber reinforced thermoplastic prepreg are laid alternately in the design sequence to form a preform; S4. Hot pressing curing: The preform is placed in a hot pressing device and hot-pressed at a temperature above the melting temperature of the thermoplastic resin to combine the resin matrix with the activated aluminum alloy surface to form a laminated matrix with a metallurgical-mechanical composite interface. S5. Preparation of anti-corrosion coating: A conductive polymer anti-corrosion coating slurry is applied to the outermost surface of the laminated matrix, and the conductive polymer anti-corrosion coating is formed after curing.
[0015] Preferably, in step S2, the plasma activation treatment uses a mixture of argon and oxygen gas, the plasma activation treatment has an equivalent power of 200-500W, a treatment time of 60-180s, and a distance of 5-15mm between the nozzle and the sample surface.
[0016] Preferably, in step S4, the hot pressing temperature is 350-400℃, the pressure is 1-2MPa, the holding time is 20-40min, and the pressure is released after cooling to below 150℃ under the holding pressure.
[0017] Preferably, in step S5, the conductive polymer anti-corrosion coating slurry is prepared by mixing conductive polymer powder, resin matrix, curing agent and solvent, and is applied by spraying, scraping or dipping.
[0018] Preferably, the time interval between S3 and S2 does not exceed 15 minutes.
[0019] In the S3 layering step of the present invention, a symmetrical layering structure design is adopted. The treated high-strength aluminum alloy layer is used as the bottom layer, and then a layer of carbon fiber reinforced thermoplastic resin prepreg is immediately laid, ensuring that the fiber direction is 0° (along the long side of the board). The above process is repeated several times until the layering is completed. In this step, the total number of layers of the treated aluminum alloy layer and the carbon fiber reinforced thermoplastic prepreg are alternately laid in the design order, which is an odd number of layers, with the high-strength aluminum alloy layer as the starting and ending layer.
[0020] In S5 of the present invention, the specific preparation steps of the anti-corrosion coating are as follows: Prepare a conductive polymer anti-corrosion coating slurry by uniformly dispersing conductive polymer powder in a solvent system containing a resin matrix and a curing agent. Apply the slurry to the surface of the laminated matrix by spraying, scraping, or dipping, controlling the wet film thickness, and curing at an appropriate temperature to form a dense coating. The curing temperature is determined according to the resin system and is generally 60-120℃.
[0021] The beneficial effects of this invention are: The lightweight corrosion-resistant composite material of the present invention is formed by alternating hard and tough layers after plasma-activated treatment of aluminum alloy surface and alternating layering with carbon fiber reinforced thermoplastic prepreg, followed by hot-pressing co-curing to form a hard and tough alternating layer matrix.
[0022] The preparation method of the present invention enables the hard aluminum alloy layer and the tough composite material layer to form nanoscale mechanical interlocking and chemical bonding at the interface, which significantly improves the interfacial bonding strength.
[0023] In this invention, the alternating hard and tough macroscopic structure enables the material to exhibit high impact and wear resistance under impact loads through a multi-stage energy dissipation mechanism. The process of coating the outermost layer with a conductive polymer coating further endows the material with active corrosion resistance. Furthermore, the conductive polymer coating can drive passivation of the metal surface in the damaged area, effectively inhibiting galvanic corrosion. The composite material obtained by the preparation method of this invention has an average density of 2.1-2.2 g / cm³, maintaining its lightweight advantage while exhibiting superior comprehensive mechanical properties and corrosion resistance compared to traditional metal materials and conventional composite laminate structures. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the structure of a lightweight corrosion-resistant composite material with alternating hard and tough layers according to the present invention.
[0025] Figure label: 1. High-strength aluminum alloy thin layer; 2. Carbon fiber reinforced thermoplastic resin layer; 3. Metallurgical-mechanical composite interface; 4. Conductive polymer anti-corrosion coating. Detailed Implementation
[0026] The invention can be further understood through the specific embodiments given below, but they are not intended to limit the invention. Example 1
[0027] This embodiment 1 presents a lightweight, corrosion-resistant composite material with alternating hard and tough layers, comprising:
[0028] The laminated matrix is composed of alternating layers of high-strength aluminum alloy and carbon fiber reinforced thermoplastic resin. The metallurgical-mechanical composite interface is located between the high-strength aluminum alloy layer and the carbon fiber reinforced thermoplastic resin layer. A nanoscale rough structure is formed on the aluminum alloy surface through plasma activation treatment, and it is combined with the thermoplastic resin matrix to form a transition region that combines mechanical interlocking and chemical bonding. A conductive polymer anti-corrosion coating is applied to the outermost surface of the laminated matrix.
[0029] The preparation method of the lightweight corrosion-resistant composite material with alternating hard and tough layers in Example 1 includes the following steps: S1. Surface pretreatment: Select AA5083-H116 aluminum alloy sheet with a thickness of 0.3mm, and place it in acetone and anhydrous ethanol for ultrasonic cleaning for 15min each, and then blow it dry with nitrogen. S2. Plasma activation treatment: The cleaned aluminum alloy surface is subjected to atmospheric pressure plasma treatment. A mixture of argon and oxygen is used with a gas volume ratio of 95:5. The treatment power is 300W, the distance between the nozzle and the sample surface is 10mm, the treatment time is 120s, and the surface roughness Ra of the aluminum alloy after treatment is 220nm and the contact angle is less than 5°. S3. Lamination: Within 15 minutes after plasma treatment, the treated aluminum alloy layer and carbon fiber reinforced polyether ether ketone prepreg are alternately laid in the order of [Al / CFRP]×10 / Al to form a preform. The fiber volume content of the prepreg is 60% and the thickness of a single layer is 0.2 mm. S4. Hot pressing curing: The preform is placed in a hot press device and heated to 380°C at a heating rate of 5°C / min. When the temperature reaches 350°C, a pressure of 1.5MPa is applied. The preform is held at 380°C for 30 minutes. After cooling to below 150°C under pressure, the pressure is released to obtain a laminated matrix with a metallurgical-mechanical composite interface. S5. Preparation of anti-corrosion coating: Polyaniline powder is dispersed in a solvent containing epoxy curing agent to prepare a coating slurry. The slurry is uniformly coated on the outer surface of the laminated matrix by spraying. The wet film thickness is controlled to be 80μm. The coating is cured at 80℃ for 2h to form a conductive polymer anti-corrosion coating with a dry film thickness of 30μm. Example 2
[0030] This embodiment 2 presents a lightweight corrosion-resistant composite material with alternating hard and tough layers, and its structure and composition are the same as those in embodiment 1.
[0031] The preparation method of the lightweight corrosion-resistant composite material with alternating hard and tough layers in Example 2 includes the following steps: S1. Surface pretreatment: AA7075-T6 aluminum alloy sheet with a thickness of 0.2mm is selected and cleaned and degreased. S2. Plasma activation treatment: Atmospheric pressure plasma treatment is performed on the surface of aluminum alloy, using a mixture of argon and oxygen with a gas volume ratio of 98:2, a treatment power of 400W, and a treatment time of 90s. S3. Lamination: The treated aluminum alloy layer and carbon fiber reinforced polyphenylene sulfide prepreg are alternately laid in the order of [Al / CFRP]×8 / Al. The fiber volume content of the prepreg is 55% and the thickness of a single layer is 0.15mm. S4. Hot pressing curing: Heat the preform to 370℃, apply 1.8MPa pressure, hold for 25 minutes, and then cool under pressure. S5. Preparation of anti-corrosion coating: Polypyrrole-polyurethane composite coating slurry is used and applied by scraping. After curing, an anti-corrosion coating with a dry film thickness of 25μm is formed. Example 3
[0032] This embodiment 3 presents a lightweight, corrosion-resistant composite material with alternating hard and tough layers, and its structure and composition are the same as those in embodiment 1.
[0033] The preparation method of the lightweight corrosion-resistant composite material with alternating hard and tough layers in Example 3 includes the following steps: S1. Surface pretreatment: AA5052-H32 aluminum alloy sheet with a thickness of 0.4mm is selected and cleaned and degreased. S2. Plasma activation treatment: Atmospheric pressure plasma treatment is performed on the surface of aluminum alloy, using a mixture of argon and oxygen with a gas volume ratio of 92:8, a treatment power of 250W, and a treatment time of 150s. S3, Lamination: The treated aluminum alloy layer and carbon fiber reinforced polyetherimide prepreg are alternately laid in the order of [Al / CFRP]×12 / Al. The fiber volume content of the prepreg is 62%, and the thickness of a single layer is 0.25mm. S4. Hot pressing curing: Heat the preform to 390℃, apply 1.2MPa pressure, hold for 35 minutes, and then cool under pressure. S5. Preparation of anti-corrosion coating: Polythiophene-epoxy composite coating slurry is used, and the coating is applied by impregnation. After curing, an anti-corrosion coating with a dry film thickness of 40μm is formed. Example 4
[0034] This embodiment 4 presents a lightweight, corrosion-resistant composite material with alternating hard and tough layers, and its structure and composition are the same as those in embodiment 1.
[0035] The preparation method of the lightweight corrosion-resistant composite material with alternating hard and tough layers in Example 4 includes the following steps: S1. Surface pretreatment: AA6061-T6 aluminum alloy sheet with a thickness of 0.25mm is selected and cleaned and degreased. S2. Plasma activation treatment: The aluminum alloy surface is subjected to atmospheric pressure plasma treatment, with parameters the same as in Example 1; S3. Lamination: The treated aluminum alloy layer and carbon fiber reinforced polyether ether ketone prepreg are alternately laid in the order of [Al / CFRP]×6 / Al. The fiber volume content of the prepreg is 58%, and the thickness of a single layer is 0.18mm. S4. Hot pressing curing: Heat the preform to 375℃, apply 1.6MPa pressure, hold for 28 minutes, and then cool under pressure. S5. Preparation of anti-corrosion coating: Polyaniline-polyimide composite coating slurry is used, and after coating and curing, an anti-corrosion coating with a dry film thickness of 35μm is formed.
[0036] Comparative Example 1 This comparative example 1 is a lightweight corrosion-resistant composite material with alternating hard and tough layers. Compared with Example 1, the plasma activation treatment step is omitted, the aluminum alloy surface is only cleaned with conventional acetone, and other materials and process parameters are the same as in Example 1.
[0037] Comparative Example 2 This comparative example 1 is a lightweight composite material with alternating hard and tough layers. Compared with Example 1, the outermost conductive polymer anti-corrosion coating is omitted, while other materials and process parameters are the same as in Example 1.
[0038] Performance testing Performance tests were conducted on the lightweight (corrosion-resistant) composite materials with alternating hard and tough layers prepared in Examples 1-4 and Comparative Examples 1-2, as well as traditional CFRP laminate samples. The tests included: tensile strength and elastic modulus testing, compressive strength after impact (CAI) testing, interlaminar fracture toughness (GIC) testing, friction corrosion wear rate comparison testing, and salt spray corrosion testing, as detailed below: Tensile strength and modulus of elasticity testing: The testing standard is ASTM D3039 / D3039M-17. A standard dumbbell-shaped specimen is prepared and subjected to tension at a constant rate on a universal testing machine. The load-displacement curve is recorded, and the tensile strength and modulus of elasticity are calculated.
[0039] Compressive strength after impact (CAI) test: The test standards refer to ASTM D7136 / D7136M-15 (impact) and ASTM D7137 / D7137M-17 (compression). First, the specimen is subjected to a drop hammer impact with a specified energy (e.g., 30J) to introduce damage. Then, the impacted specimen is installed in a compression fixture and subjected to a compression test until failure. The maximum compressive load is recorded and the compressive strength (CAI value) is calculated.
[0040] Interlaminar fracture toughness (GIC) test: The test standard is based on ASTM D5528-13. A double cantilever beam (DCB) specimen is used. The energy release rate during crack propagation is measured by pre-existing cracks under type I loading, and the type I interlaminar fracture toughness (GIC) value is calculated.
[0041] Frictional corrosion wear rate comparison test: The test standards refer to ASTM G65-16e1 and ASTM G119-09. Rubber wheel wear tests were conducted in dry air and simulated salt spray corrosion environments (such as dripping or spraying of 5% NaCl solution). The volume loss of the sample after a specified number of revolutions was measured, the wear rate was calculated, and the increase in wear rate under the two environments was compared.
[0042] Salt spray corrosion test: The test standard is based on ASTM B117-19. The sample is placed in a salt spray chamber and continuously exposed to a neutral salt spray environment of 5% sodium chloride (35°C). After 1000 hours, the sample is removed, and the corrosion penetration of the cross-section (e.g., metallographic cross-sectional analysis) and the surface corrosion grade are observed and recorded (refer to ASTM D610-08(2019)). The test results are shown in Table 1:
[0043] As can be seen from the test results in Table 1, the composite material samples prepared in Examples 1-4 of the present invention exhibit excellent comprehensive performance.
[0044] Improved mechanical properties: The tensile strength (315-330 MPa) and elastic modulus (77.8-81.2 GPa) of the samples in each embodiment were significantly improved compared with Comparative Example 1 (310 MPa, 70.3 GPa) without plasma treatment, indicating that plasma activation treatment effectively improved interfacial bonding and promoted load transfer. The compressive strength after impact (CAI value 328-348 MPa) was much higher than that of aluminum plate of equal thickness (210 MPa) and traditional CFRP laminate (185 MPa), demonstrating the advantages of the hard-tough alternating laminate structure in multi-stage energy dissipation.
[0045] Significant interface toughening effect: The interlaminar fracture toughness GIC values (485-535 J / m²) of the samples in each embodiment are more than 300% higher than those of Comparative Example 1 (130 J / m²), and far higher than those of traditional CFRP laminates (160 J / m²), which fully demonstrates the key role of the "metallurgical-mechanical composite interface" formed by plasma activation in inhibiting crack propagation and improving interface toughness and bonding strength.
[0046] Excellent synergistic effect between wear resistance and corrosion resistance: In the tribological wear test under salt spray corrosion environment, the wear rate of the sample in the example was (4.0-4.8×10). -6The wear rate (mm³ / N·m) is lower than that of Comparative Example 1, the aluminum plate of equal thickness, and the conventional CFRP laminate, and the increase in wear rate relative to the dry air environment is less than 50%. In contrast, the increase in wear rate of Comparative Example 1 and the aluminum plate of equal thickness exceeds 120%, and that of the conventional CFRP laminate exceeds 80%. This indicates that the structure of the present invention can still maintain good wear resistance in a corrosive environment, which is attributed to the active anti-corrosion effect of the outer conductive polymer coating protecting the base material.
[0047] Outstanding long-term corrosion resistance: After 1000 hours of salt spray testing, no signs of corrosive medium penetration were observed in the cross-sections of all the sample examples, while Comparative Example 1 and Comparative Example 2 showed varying degrees of penetration. This directly demonstrates that the "active passivation" capability provided by the outermost conductive polymer coating is crucial for achieving long-term corrosion resistance, especially for suppressing galvanic corrosion.
[0048] In summary, the composite material prepared by this invention through macroscopic alternating hard and tough layer design, microscopic plasma-activated interface strengthening, and system-level conductive polymer active anti-corrosion coating has the properties of lightweight, high impact and wear resistance, and ultra-strong electrochemical corrosion resistance.
[0049] The above description is merely an embodiment of the present invention, and the scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A lightweight, corrosion-resistant composite material with alternating layers of hard and tough materials, characterized in that, include: The laminated matrix is composed of alternating layers of high-strength aluminum alloy and carbon fiber reinforced thermoplastic resin. The metallurgical-mechanical composite interface is located between the high-strength aluminum alloy layer and the carbon fiber reinforced thermoplastic resin layer. A nanoscale rough structure is formed on the surface of the aluminum alloy through plasma activation treatment, and it is combined with the thermoplastic resin matrix to form a transition region that has both mechanical interlocking and chemical bonding. A conductive polymer anti-corrosion coating is applied to the outermost surface of the laminated matrix.
2. The lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 1, characterized in that, In the laminated matrix, the total number of high-strength aluminum alloy layers and carbon fiber reinforced thermoplastic resin layers is an odd number.
3. The lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 1, characterized in that, The single-layer thickness of the high-strength aluminum alloy layer is 0.1-0.5 mm; the matrix of the carbon fiber reinforced thermoplastic resin layer is polyetheretherketone, polyphenylene sulfide or polyetherimide, and the single-layer thickness of the carbon fiber reinforced thermoplastic resin layer is 0.1-0.3 mm.
4. The lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 1, characterized in that, In the metallurgical-mechanical composite interface, the arithmetic mean roughness Ra of the aluminum alloy surface after plasma activation treatment is 150-300 nm, and the contact angle is less than 10°.
5. The lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 1, characterized in that, The conductive polymer anti-corrosion coating is a coating formed by combining polyaniline, polypyrrole or polythiophene conductive polymers with a resin matrix, and the dry film thickness of the conductive polymer anti-corrosion coating is 20-50 μm.
6. A method for preparing a lightweight corrosion-resistant composite material with alternating hard and tough layers as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. Surface pretreatment: Cleaning and degreasing the surface of high-strength aluminum alloy sheet; S2. Plasma activation treatment: Atmospheric pressure plasma treatment is applied to the cleaned aluminum alloy surface to form a nanoscale rough structure and improve the surface energy. S3. Laying out layers: The treated aluminum alloy layer and carbon fiber reinforced thermoplastic prepreg are laid alternately in the design sequence to form a preform; S4. Hot pressing curing: The preform is placed in a hot pressing device and hot-pressed at a temperature above the melting temperature of the thermoplastic resin to combine the resin matrix with the activated aluminum alloy surface to form a laminated matrix with a metallurgical-mechanical composite interface. S5. Preparation of anti-corrosion coating: A conductive polymer anti-corrosion coating slurry is applied to the outermost surface of the laminated matrix, and the conductive polymer anti-corrosion coating is formed after curing.
7. The method for preparing the lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 6, characterized in that, In step S2, the plasma activation treatment uses a mixture of argon and oxygen gas, with a power of 200-500W and a treatment time of 60-180s.
8. The method for preparing the lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 6, characterized in that, In step S4, the hot pressing temperature is 350-400℃, the pressure is 1-2MPa, the holding time is 20-40min, and the pressure is released after cooling to below 150℃ under the holding pressure.
9. The method for preparing the lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 6, characterized in that, In step S5, the conductive polymer anti-corrosion coating slurry is prepared by mixing conductive polymer powder, resin matrix, curing agent and solvent, and is applied by spraying, scraping or dipping.
10. The method for preparing the lightweight corrosion-resistant composite material with alternating hard and tough layers according to claim 6, characterized in that, The time interval between S3 and S2 shall not exceed 15 minutes.