Synergistic preparation method and application of carboxylated cellulose nanocrystal and regenerated cellulose

By treating cellulose raw materials with Lewis acids and polycarboxylic acids, the synergistic preparation of cellulose nanocrystals and regenerated cellulose was achieved, solving the environmental and economic bottlenecks of existing processes and producing high-performance, biodegradable cellulose materials.

CN121991254APending Publication Date: 2026-05-08GUILIN UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610111980.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-27
Publication Date
2026-05-08

AI Technical Summary

Technical Problem

Existing processes for preparing cellulose nanocrystals and regenerated cellulose are environmentally unfriendly, costly, and difficult to scale up, and traditional solvent systems are prone to causing pollution.

Method used

A synergistic process for preparing carboxylated cellulose nanocrystals and regenerated cellulose was developed by impregnating cellulose raw materials with Lewis acid solution followed by carboxylation modification in a polycarboxylic acid solution. This process simplifies the procedure and achieves a balance between green chemistry and economic benefits.

Benefits of technology

Cellulose materials with high carboxyl group content and regular nanostructure were prepared, exhibiting excellent self-assembly performance and low energy consumption. They can form iridescent films, have excellent material properties, and are completely biodegradable, thus reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121991254A_ABST
    Figure CN121991254A_ABST
Patent Text Reader

Abstract

The invention discloses a synergistic preparation method and application of carboxylated cellulose nanocrystals and regenerated cellulose, and belongs to the technical field of cellulose nanomaterial preparation. The synergistic preparation method of the carboxylated cellulose nanocrystal and the regenerated cellulose comprises the following steps: carrying out dipping treatment on a cellulose raw material in a Lewis acid solution, then carrying out solid-liquid separation, and collecting a solid-phase component to obtain cellulose slurry; dispersing the cellulose slurry in a polycarboxylic acid solution, reacting, and then filtering and collecting a solid product; treating the solid product by a method I or a method II; the method I comprises the following steps: carrying out separation treatment on the solid product to obtain carboxylated cellulose nanocrystals and regenerated cellulose; and the method II comprises the following steps: washing the solid product, and then carrying out suction filtration to obtain the holocellulose composite membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cellulose nanomaterial preparation technology, and in particular to a method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose and its application. Background Technology

[0002] Cellulose nanocrystals (CNCs) have attracted widespread attention due to their excellent mechanical properties, high specific surface area, biodegradability, and renewability, and have significant application potential in polymer composites, biomedical scaffolds, and smart hydrogels. However, to expand their application range, CNC surfaces typically require chemical modification to introduce specific reactive functional groups. Currently, although methods such as TEMPO oxidation or persulfate oxidation can prepare carboxyl-containing CNCs, existing methods generally suffer from insufficient environmental friendliness (e.g., use of toxic reagents, low atom economy, high waste emissions) and high overall production costs (e.g., expensive reagents, high energy consumption, limited yield, and difficulty in continuous production), severely restricting the large-scale and commercial application of carboxylated cellulose nanocrystals. On the other hand, while regenerated cellulose materials possess good processability and biocompatibility, their traditional preparation processes heavily rely on volatile, toxic, or high-cost solvent systems, such as carbon disulfide used in viscose processes, which easily lead to environmental pollution problems and limit their sustainable development, requiring further improvement. Therefore, designing a preparation process that can simultaneously produce cellulose nanocrystals and regenerated cellulose can help solve the bottleneck problem of the difficulty in balancing greenness and economy in existing processes. Summary of the Invention

[0003] The purpose of this invention is to provide a method for the synergistic preparation and application of carboxylated cellulose nanocrystals and regenerated cellulose, in order to solve the aforementioned problems in the background art. The carboxylated cellulose nanocrystals prepared by this invention not only possess a high content of carboxyl groups and a regular nanostructure, but also exhibit excellent self-assembly properties. Their aqueous dispersion can form an ordered film with an iridescent effect through drying even under low concentration conditions, and the resulting regenerated cellulose has a micron-scale.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] One of the technical solutions of this invention is to provide a method for the synergistic preparation of carboxylated cellulose nanocrystals (CNC) and regenerated cellulose (RC), comprising the following steps:

[0006] (1) The cellulose raw material is impregnated in Lewis acid solution, and then the solid phase component is collected by solid-liquid separation to obtain cellulose slurry;

[0007] (2) Disperse the cellulose slurry in a polycarboxylic acid solution, react, and then filter to collect the solid product; process the solid product by method one or method two;

[0008] The method includes the following steps: separating the solid product to obtain carboxylated cellulose nanocrystals and regenerated cellulose;

[0009] Method 2 includes the following steps: washing the solid product and then filtering it to obtain a full cellulose composite membrane.

[0010] Preferably, the solid content of the cellulose raw material in the Lewis acid solution is 1-15 wt%.

[0011] Preferably, the cellulose raw material is one or more of microcrystalline cellulose, bacterial cellulose, refined cotton, defatted cotton, dry bleached bagasse, and dry bleached wood pulp.

[0012] Preferably, the immersion treatment is performed at a temperature of 20-80°C for a time of 30-240 minutes.

[0013] Preferably, the active ingredient in the Lewis acid solution is one or more of aluminum trichloride (AlCl3), ferric trichloride (FeCl3), copper dichloride (CuCl2), chromium chloride (CrCl3), zinc chloride (ZnCl2), and lithium bromide (LiBr); the proportion of the active ingredient in the Lewis acid solution is 30-90 wt%.

[0014] Preferably, the solid content of the cellulose slurry in the polycarboxylic acid solution is 1-15 wt%.

[0015] Preferably, the carboxylic acid concentration in the polycarboxylic acid solution is 40-80 wt%; the carboxylic acid in the polycarboxylic acid solution is at least two of citric acid, oxalic acid, succinic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, medoconic acid, and aconitic acid.

[0016] Preferably, the reaction temperature is 20-60℃ and the reaction time is 2-10h.

[0017] Preferably, the separation process includes the following steps: centrifuging the solid product, then collecting the supernatant to obtain carboxylated cellulose nanocrystals; collecting the remaining solid after centrifugation to obtain regenerated cellulose.

[0018] The technical principle of this invention is as follows:

[0019] This invention uses Lewis acid solution to impregnate cellulose raw materials, and then uses polycarboxylic acids to perform carboxylation modification and structural dissociation, thereby obtaining a mixed system containing carboxylated cellulose nanocrystals (CNC) and regenerated cellulose (RC).

[0020] Compared to traditional cellulose material preparation methods, the CNC prepared in this invention not only possesses a high content of carboxyl groups and a well-ordered nanostructure, but also exhibits excellent self-assembly properties. It is nanoscale with controllable aspect ratio and surface groups. Its aqueous dispersion can form an ordered film with an iridescent effect through drying even at low concentrations, and the resulting RC has a micron-scale. From a production perspective, this technology highlights the core advantages of low energy consumption and low cost. This technology not only successfully prepares high-performance functionalized cellulose nanocrystals and regenerated cellulose simultaneously, but also incorporates green chemistry principles throughout the entire process chain, achieving a balance between environmental and economic benefits.

[0021] The carboxylated CNCs prepared by the above method can be stably dispersed in water and various polar organic solvents, facilitating processing through various techniques such as casting and electrospinning, and also possessing the potential to serve as a highly reactive nanoplatform. These carboxylated cellulose nanocrystals can form stronger interfacial interactions with polymer matrices (such as rubber, plastics, and hydrogels), not only enhancing the mechanical properties and thermal stability of composite materials through crosslinking, but also regulating their swelling behavior and degradation rate.

[0022] The beneficial technical effects of the present invention are as follows:

[0023] (1) This invention designs a novel process that can simultaneously prepare carboxylated CNC and RC, which not only greatly simplifies the process, but also realizes the "separable and combinable, on-demand preparation" of carboxylated cellulose nanocrystals and regenerated cellulose from the source, laying a solid foundation for improving material performance.

[0024] (2) The CNC prepared by the present invention not only has a high content of carboxyl groups, but also has excellent self-assembly performance. Its aqueous dispersion can form a film with iridescent phenomenon when dried under conditions that are significantly lower than conventional concentrations.

[0025] (3) The all-cellulose composite membrane of the present invention not only has excellent mechanical properties and transparency, but also can achieve complete bio-based and fully degradable components.

[0026] (4) The reagents used in this invention are all common and readily available chemical raw materials. The reaction conditions are mild, the process is simple, and no complex and expensive special equipment is required, which significantly reduces production energy consumption and production costs.

[0027] (5) The Lewis acids and polycarboxylic acid reagents used in the entire preparation process can be recycled, which is in line with green and sustainable development. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0029] Figure 1 A photograph of the carboxylated cellulose nanocrystal aqueous dispersion prepared in Example 1 of this invention;

[0030] Figure 2 This is a photograph of the all-cellulose composite film prepared in Example 1 of the present invention;

[0031] Figure 3 The stress-strain diagram is shown for the all-cellulose composite film prepared in Example 1 of this invention.

[0032] Figure 4 A photograph of a thin film exhibiting iridescence prepared by carboxylated cellulose nanocrystals in Example 1;

[0033] Figure 5 This is a scanning electron microscope image of the carboxylated cellulose nanocrystals prepared in Example 1 of the present invention;

[0034] Figure 6 This is a transmission electron microscope image of the carboxylated cellulose nanocrystals prepared in Example 1 of the present invention;

[0035] Figure 7 The conductivity titration diagram is shown for the carboxylated cellulose nanocrystals prepared in Example 1 of this invention.

[0036] Figure 8 The image shows the XRD pattern of the carboxylated cellulose nanocrystals prepared in Example 1 of this invention.

[0037] Figure 9 The XRD pattern of the regenerated cellulose prepared in Example 1 of this invention;

[0038] Figure 10 This is a particle size distribution of the regenerated cellulose prepared in Example 1 of the present invention. Detailed Implementation

[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention.

[0040] Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, are also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0041] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. It should be noted that any aspects of this invention not described in detail are conventional practices in the art and are not the focus of this invention.

[0042] The terms “comprising,” “including,” “having,” “containing,” etc., used in this invention are all open-ended terms, meaning that they include but are not limited to.

[0043] This invention discloses a method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, comprising the following steps:

[0044] (1) The cellulose raw material is impregnated in Lewis acid solution and then the solid and liquid phases are separated; the solid phase after separation is cellulose slurry; the liquid phase after separation is Lewis acid solution, which is recycled.

[0045] (2) Disperse the cellulose slurry obtained in step (1) in a polycarboxylic acid solution, react, and then filter to collect the solid product; process the solid product by method one or method two;

[0046] Method 1 includes the following steps: separating the solid product to obtain carboxylated cellulose nanocrystals (CNC) and regenerated cellulose (RC).

[0047] Method 2 includes the following steps: washing the solid product and then filtering it to obtain a full cellulose composite membrane.

[0048] Furthermore, the solid content of the cellulose raw material in the Lewis acid solution is 1-15 wt%; the impregnation treatment temperature is 20-80℃ and the time is 30-240 min.

[0049] Furthermore, the cellulose raw material is one or more of microcrystalline cellulose, bacterial cellulose, refined cotton, defatted cotton, dry bleached bagasse, and dry bleached wood pulp.

[0050] Furthermore, the active ingredient in the Lewis acid solution is one or more of aluminum trichloride (AlCl3), ferric trichloride (FeCl3), copper dichloride (CuCl2), chromium chloride (CrCl3), zinc chloride (ZnCl2), and lithium bromide (LiBr).

[0051] Furthermore, the active ingredient in the Lewis acid solution accounts for 30-90 wt%.

[0052] Furthermore, the washing method described in step (1) is water washing: after water washing, the following steps are also included: the active ingredients in the obtained liquid phase are separated by rotary evaporation and concentrated to the initial concentration of Lewis acid solution for recycling.

[0053] Furthermore, the solid content of the cellulose slurry in the polycarboxylic acid solution is 1-15 wt%.

[0054] Furthermore, the carboxylic acid concentration in the polycarboxylic acid solution is 40-80 wt%.

[0055] Furthermore, the reaction temperature is 20-60℃, and the reaction time is 2-10h.

[0056] Furthermore, the carboxylic acid in the polycarboxylic acid solution is at least two of citric acid, oxalic acid, succinic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, medoconic acid, and aconitic acid.

[0057] Further, the separation process includes the following steps: the solid product is first washed with water and then centrifuged until the supernatant is turbid, and then the turbid supernatant is collected to obtain carboxylated cellulose nanocrystals (CNC); the solid remaining after centrifugation is collected as regenerated cellulose (RC).

[0058] Furthermore, the carboxyl group content of the carboxylated cellulose nanocrystals is 0.58-0.72 mmol / g; the average particle size of the regenerated cellulose is in the micrometer range.

[0059] This invention aims to overcome the shortcomings of existing technologies and provide a method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose. By achieving carboxylation and structural regulation of cellulose in this reaction system, the bottleneck problem of balancing greenness and economy in existing processes is effectively solved. The resulting material exhibits excellent dispersibility and self-assembly properties, as well as diverse reactivity and good interfacial bonding ability, which can expand its application scope in composite materials, biomedicine, and other fields.

[0060] Existing technologies for preparing carboxylated cellulose nanocrystals (CNC) and regenerated cellulose (RC) typically require separate steps. While this approach yields both materials individually, it suffers from cumbersome processes and high energy consumption. This invention presents a novel process capable of simultaneously preparing carboxylated CNC and RC, significantly simplifying the process and enabling the "separate and combined, on-demand preparation" of carboxylated cellulose nanocrystals and regenerated cellulose, laying a solid foundation for improving material performance. The all-cellulose composite membrane not only possesses excellent mechanical properties and transparency but also achieves complete bio-based and fully degradable composition, making it a viable alternative to traditional petroleum-based composite materials and demonstrating broad prospects for sustainable material applications.

[0061] The microcrystalline cellulose, refined cotton, and dry bleached sugarcane bagasse used in this invention were purchased from Huzhou Linghu Xinwang Chemical Co., Ltd., Hunan Zhaosheng Cotton Industry Co., Ltd., and Guangxi Guitang Co., Ltd., respectively.

[0062] Unless otherwise specified, "room temperature" in this invention refers to 10-30°C.

[0063] All raw materials used in the following embodiments of the present invention are commercially available products.

[0064] Example 1

[0065] A method for the synergistic preparation of carboxylated cellulose nanocrystals (CNC) and regenerated cellulose (RC) comprises the following steps:

[0066] First, microcrystalline cellulose is pre-impregnated in a Lewis acid solution (70 wt% ZnCl2 solution; the solid content of microcrystalline cellulose in the Lewis acid solution is 5 wt%). After impregnation at 80°C for 30 min, the solid phase component is collected by solid-liquid separation to obtain cellulose slurry. The separated liquid phase component is a Lewis acid solution, which is recycled by rotary evaporation.

[0067] The cellulose slurry was washed and dried, then added to a 65 wt% maleic acid solution (the cellulose slurry comprised 5 wt% of the maleic acid solution), and reacted at 60°C for 9 hours. After the reaction was complete, 200 mL of deionized water was added to terminate the reaction. The resulting mixture was then immediately filtered to separate the solid product from the unreacted solution (the unreacted solution could be recovered by rotary evaporation). The solid product was washed repeatedly with deionized water and then filtered to obtain a full cellulose composite film.

[0068] The solid product was re-prepared by repeating the above steps. It was first washed with deionized water, then water was added, and the mixture was repeatedly centrifuged (5000 rpm for 5 minutes). The supernatant was collected to obtain an aqueous dispersion of carboxylated cellulose nanocrystals (65% yield) (see...). Figure 1 The remaining solids after centrifugation were collected to obtain RC (yield 32%).

[0069] The above-mentioned carboxylated cellulose nanocrystal aqueous dispersion was dried at room temperature to obtain a film exhibiting iridescent properties.

[0070] Figure 1 The image shows the carboxylated cellulose nanocrystal aqueous dispersion prepared in Example 1 of this invention. It can be seen that it is a milky white suspension at room temperature.

[0071] Figure 2 This is a physical image of the all-cellulose composite film prepared in Example 1 of the present invention.

[0072] Figure 3 This is a stress-strain diagram of the all-cellulose composite film prepared in Example 1 of the present invention.

[0073] Figure 4 This is a photograph of a thin film exhibiting iridescence, prepared by carboxylated cellulose nanocrystals in Example 1.

[0074] Figure 5 This is a scanning electron microscope image of the carboxylated cellulose nanocrystals prepared in Example 1 of the present invention.

[0075] Figure 6 This is a transmission electron microscope image of the carboxylated cellulose nanocrystals prepared in Example 1 of the present invention.

[0076] Figure 7 The conductivity titration diagram is shown for the carboxylated cellulose nanocrystals prepared in Example 1 of this invention.

[0077] Figure 8 The image shows the XRD pattern of the carboxylated cellulose nanocrystals prepared in Example 1 of this invention.

[0078] Figure 9 The image shows the XRD pattern of the regenerated cellulose prepared in Example 1 of this invention.

[0079] Figure 10 This is a particle size distribution of the regenerated cellulose prepared in Example 1 of the present invention.

[0080] X-ray diffraction pattern ( Figure 8 , 9 This confirms that the carboxylated CNC prepared in this invention completely retains the cellulose type I crystal structure, while the RC transforms into the cellulose type II crystal structure; conductivity titration data ( Figure 7The conductivity titration (with a titrant concentration of 0.1 M and a sample mass of 0.042 g) showed that the carboxyl content of the carboxylated CNC reached 0.7 mmol / g (0.1*(1.14-0.84) / 0.042=0.71), proving the successful grafting of carboxyl groups; scanning and transmission electron microscopy images ( Figure 5 , 6 The results showed that carboxylated CNC exhibited a regular nanorod morphology with diameters ranging from 10 to 30 nanometers and lengths from 100 to 300 nanometers; mechanical property tests ( Figure 3 The results show that the tensile strength of the obtained composite film is as high as 132 MPa, exhibiting excellent mechanical properties. Based on the above characterization results, this embodiment successfully prepared a cellulose material with a regular crystal structure and surface carboxyl functionalization.

[0081] Example 2

[0082] A method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, comprising the following steps:

[0083] First, microcrystalline cellulose was pre-impregnated in a Lewis acid solution (78 wt% CuCl2 solution; the solid content of microcrystalline cellulose in the Lewis acid solution was 5 wt%). After impregnation at 70°C for 120 min, the solid phase component was collected by solid-liquid separation to obtain cellulose slurry. The separated liquid phase component was a Lewis acid solution, which was recovered and reused after rotary evaporation.

[0084] The cellulose slurry was washed and dried, then added to a 60 wt% itaconic acid solution (the cellulose slurry accounted for 5 wt% of the itaconic acid solution), and reacted at 55°C for 8 hours. After the reaction was completed, 200 mL of deionized water was added to terminate the reaction, and the resulting mixture was immediately filtered to separate the solid product from the unreacted solution (the unreacted solution could be recovered by rotary evaporation). The solid product was taken, washed several times with deionized water, and then filtered to obtain a full cellulose composite film.

[0085] The above solid product was re-prepared by repeating the above steps. It was first washed with deionized water, then water was added, and it was repeatedly centrifuged (centrifugation speed of 5000 rpm, centrifugation time of 5 minutes). The upper liquid was collected to obtain carboxylated cellulose nanocrystal aqueous dispersion (yield of 60%). The remaining solid after centrifugation was collected to obtain RC (yield of 34%).

[0086] The carboxyl group content of the carboxylated CNC obtained in this embodiment was measured to be 0.58 mmol / g. The carboxylated CNC prepared in this embodiment still retains the crystalline structure of cellulose I, while RC transforms into the crystalline structure of cellulose II. The prepared carboxylated CNC has a diameter of approximately tens of nanometers and a length of approximately 100-250 nm. The composite film exhibits a tensile strength as high as 121 MPa, demonstrating excellent mechanical properties.

[0087] Example 3

[0088] A method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, comprising the following steps:

[0089] First, microcrystalline cellulose was pre-impregnated in a Lewis acid solution (65 wt% LiBr solution; the solid content of microcrystalline cellulose in the Lewis acid solution was 5 wt%). After impregnation at 60°C for 40 min, the solid phase component was collected by solid-liquid separation to obtain cellulose slurry. The separated liquid phase component was a Lewis acid solution, which was recycled by rotary evaporation.

[0090] The cellulose slurry was washed and dried, then added to a 60 wt% itaconic acid solution (the cellulose slurry accounted for 5 wt% of the itaconic acid solution), and reacted at 40°C for 6 hours. After the reaction was completed, 200 mL of deionized water was added to terminate the reaction, and the resulting mixture was immediately filtered to separate the solid product from the unreacted solution (the unreacted solution could be recovered by rotary evaporation). The solid product was taken, washed several times with deionized water, and then filtered to obtain a full cellulose composite film.

[0091] The above solid product was re-prepared by repeating the above steps. It was first washed with deionized water, then water was added, and it was repeatedly centrifuged (centrifugation speed of 5000 rpm, centrifugation time of 5 minutes). The upper liquid was collected to obtain carboxylated cellulose nanocrystal aqueous dispersion (yield of 61%). The remaining solid after centrifugation was collected to obtain RC (yield of 35%).

[0092] The carboxyl group content of the carboxylated CNC obtained in this embodiment was measured to be 0.63 mmol / g. The carboxylated CNC prepared in this embodiment still retains the crystalline structure of cellulose I, while RC transforms into the crystalline structure of cellulose II. The prepared carboxylated CNC has a diameter of approximately tens of nanometers and a length of approximately 100-350 nm. The composite film exhibits a tensile strength as high as 119 MPa, demonstrating excellent mechanical properties.

[0093] Example 4

[0094] A method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, comprising the following steps:

[0095] First, refined cotton is pre-impregnated in a Lewis acid solution (composed of a 60wt% FeCl3 solution and a 40wt% ZnCl2 solution in a ratio of 1.2:1; the solid content of the refined cotton in the Lewis acid solution is 7wt%). After impregnation at 40℃ for 45 min, the solid phase component is collected by solid-liquid separation to obtain cellulose pulp. The separated liquid phase component is the Lewis acid solution, which is recycled by rotary evaporation.

[0096] The cellulose slurry was washed and dried, then added to a 68 wt% aconitic acid solution (the cellulose slurry accounted for 5 wt% of the aconitic acid solution), and reacted at 40°C for 6 hours. After the reaction was completed, 200 mL of deionized water was added to terminate the reaction, and the resulting mixture was immediately filtered to separate the solid product from the unreacted solution (the unreacted solution could be recovered by rotary evaporation). The solid product was taken, washed several times with deionized water, and then filtered to obtain a full cellulose composite film.

[0097] The above solid product was re-prepared by repeating the above steps. It was first washed with deionized water, then water was added, and it was repeatedly centrifuged (centrifugation speed of 5000 rpm, centrifugation time of 5 minutes). The upper liquid was collected to obtain carboxylated cellulose nanocrystal aqueous dispersion (yield of 62%). The remaining solid after centrifugation was collected to obtain RC (yield of 33%).

[0098] The carboxyl group content of the carboxylated CNC obtained in this embodiment was measured to be 0.68 mmol / g. The carboxylated CNC prepared in this embodiment retains the crystalline structure of cellulose I, while RC transforms into the cellulose II crystalline structure. The prepared carboxylated CNC has a diameter of approximately tens of nanometers and a length of approximately 150-350 nm. The composite film exhibits a tensile strength as high as 111 MPa, demonstrating excellent mechanical properties.

[0099] Example 5

[0100] A method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, comprising the following steps:

[0101] First, refined cotton is pre-impregnated in a Lewis acid solution (composed of a 40wt% FeCl3 solution and a 20wt% AlCl3 solution in a 1:1 ratio; the solid content of the refined cotton in the Lewis acid solution is 7wt%). After impregnation at 30℃ for 60 min, the solid phase component is collected by solid-liquid separation to obtain cellulose pulp. The separated liquid phase component is the Lewis acid solution, which is recycled by rotary evaporation.

[0102] The cellulose slurry was washed and dried, then added to a 68 wt% aconitic acid solution (the cellulose slurry accounted for 5 wt% of the aconitic acid solution), and reacted at 40°C for 6 hours. After the reaction was completed, 200 mL of deionized water was added to terminate the reaction, and the resulting mixture was immediately filtered to separate the solid product from the unreacted solution (the unreacted solution could be recovered by rotary evaporation). The solid product was taken, washed several times with deionized water, and then filtered to obtain a full cellulose composite film.

[0103] The above solid product was re-prepared by repeating the above steps. It was first washed with deionized water, then water was added, and it was repeatedly centrifuged (centrifugation speed of 5000 rpm, centrifugation time of 5 minutes). The upper liquid was collected to obtain carboxylated cellulose nanocrystal aqueous dispersion (yield of 64%). The remaining solid after centrifugation was collected to obtain RC (yield of 30%).

[0104] The carboxyl group content of the carboxylated CNC obtained in this embodiment was measured to be 0.62 mmol / g. The carboxylated CNC prepared in this embodiment still retains the crystalline structure of cellulose I, while RC transforms into the crystalline structure of cellulose II. The prepared carboxylated CNC has a diameter of approximately tens of nanometers and a length of approximately 140-330 nm. The composite film exhibits a tensile strength as high as 111 MPa, demonstrating excellent mechanical properties.

[0105] Example 6

[0106] A method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, comprising the following steps:

[0107] First, the dried bleached sugarcane bagasse was pre-impregnated in a Lewis acid solution (composed of a 60 wt% FeCl3 solution and a 40 wt% ZnCl2 solution in a ratio of 1.5:1; the solid content of the dried bleached sugarcane bagasse in the Lewis acid solution was 7 wt%). After impregnation at 40°C for 45 min, the solid phase was collected by solid-liquid separation to obtain cellulose pulp. The separated liquid phase was the Lewis acid solution, which was recycled by rotary evaporation.

[0108] The cellulose slurry was washed and dried, then added to a 68 wt% aconitic acid solution (the cellulose slurry accounted for 5 wt% of the aconitic acid solution), and reacted at 40°C for 6 hours. After the reaction was completed, 200 mL of deionized water was added to terminate the reaction, and the resulting mixture was immediately filtered to separate the solid product from the unreacted solution (the unreacted solution could be recovered by rotary evaporation). The solid product was taken, washed several times with deionized water, and then filtered to obtain a full cellulose composite film.

[0109] The above solid product was re-prepared by repeating the above steps. It was first washed with deionized water, then water was added, and it was repeatedly centrifuged (centrifugation speed of 5000 rpm, centrifugation time of 5 minutes). The upper liquid was collected to obtain carboxylated cellulose nanocrystal aqueous dispersion (yield of 63%). The remaining solid after centrifugation was collected to obtain RC (yield of 34%).

[0110] The carboxyl group content of the carboxylated CNC obtained in this embodiment was measured to be 0.72 mmol / g. The carboxylated CNC prepared in this embodiment retains the crystalline structure of cellulose I, while RC transforms into the cellulose II crystalline structure. The prepared carboxylated CNC has a diameter of approximately tens of nanometers and a length of approximately 240-300 nm. The composite film exhibits a tensile strength as high as 96 MPa, demonstrating excellent mechanical properties.

[0111] In summary, the carboxylated CNCs prepared in Examples 1-6 have a carboxyl content of 0.58-0.72 mmol / g and a nanometer length of 100-350 nm; the tensile strength of the composite films is 96-132 MPa. Compared with existing technologies, the preparation method described in this application does not require the use of other additives (e.g., sulfuric acid, phosphoric acid, hydrochloric acid, etc.), and Lewis acids and polycarboxylic acids can be recycled through simple methods, which is of great significance for industrial production.

[0112] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for the synergistic preparation of carboxylated cellulose nanocrystals and regenerated cellulose, characterized in that, Includes the following steps: (1) The cellulose raw material is impregnated in Lewis acid solution, and then the solid phase component is collected by solid-liquid separation to obtain cellulose slurry; (2) Disperse the cellulose slurry in a polycarboxylic acid solution, react, and then filter to collect the solid product; process the solid product by method one or method two; The method includes the following steps: separating the solid product to obtain carboxylated cellulose nanocrystals and regenerated cellulose; Method 2 includes the following steps: washing the solid product and then filtering it to obtain a full cellulose composite membrane.

2. The synergistic preparation method according to claim 1, characterized in that, The cellulose raw material has a solid content of 1-15 wt% in Lewis acid solution.

3. The synergistic preparation method according to claim 1, characterized in that, The cellulose raw material is one or more of microcrystalline cellulose, bacterial cellulose, refined cotton, defatted cotton, dry bleached sugarcane bagasse, and dry bleached wood pulp.

4. The synergistic preparation method according to claim 1, characterized in that, The immersion treatment is performed at a temperature of 20-80℃ for a time of 30-240 minutes.

5. The synergistic preparation method according to claim 1, characterized in that, The active ingredient in the Lewis acid solution is one or more of aluminum trichloride, ferric trichloride, copper dichloride, chromium chloride, zinc chloride, and lithium bromide; the active ingredient in the Lewis acid solution accounts for 30-90 wt%.

6. The synergistic preparation method according to claim 1, characterized in that, The cellulose slurry has a solid content of 1-15 wt% in the polycarboxylic acid solution.

7. The synergistic preparation method according to claim 1, characterized in that, The carboxylic acid concentration in the polycarboxylic acid solution is 40-80 wt%; the carboxylic acid in the polycarboxylic acid solution is at least two of citric acid, oxalic acid, succinic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, zeaxanthin, and aconitic acid.

8. The synergistic preparation method according to claim 1, characterized in that, The reaction temperature is 20-60℃, and the reaction time is 2-10h.

9. The synergistic preparation method according to claim 1, characterized in that, The separation process includes the following steps: centrifuging the solid product, then collecting the supernatant to obtain carboxylated cellulose nanocrystals; collecting the remaining solid after centrifugation to obtain regenerated cellulose.