Plating film for metal sintering bonding, method for producing same, and semiconductor mounting substrate
By controlling the phosphorus content of the electroless nickel-phosphorus plating film and adding an electroless silver or gold plating film and a barrier metal layer, the heat resistance and thermal shock resistance of the plating film under high temperature environment are solved, making it suitable for metal sintering bonding of next-generation power modules.
Patent Information
- Application Number
- CN202480065098.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-13
- Filing Date
- 2024-07-03
- Publication Date
- 2026-05-12
AI Technical Summary
Existing electroless nickel-phosphorus plating films have poor heat resistance and thermal shock resistance in high-temperature environments, which cannot meet the requirements of next-generation power modules.
By controlling the phosphorus content of the electroless nickel-phosphorus plating film to below 4% by mass, and optionally adding an electroless silver or gold plating film and a barrier metal layer, a plating film with excellent heat resistance and resistance to thermal shock can be formed.
It improves the heat resistance and thermal shock resistance of the coated film in high-temperature environments, making it suitable for metal sintering bonding of next-generation power modules.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a coated film and its manufacturing method, as well as a semiconductor mounting substrate. Background Technology
[0002] In recent years, next-generation power modules using wide-bandgap power semiconductor devices such as SiC and GaN have emerged. These next-generation power modules can operate in high-temperature environments, such as above 200°C, thus requiring high heat resistance from peripheral components.
[0003] In the past, solder was used to bond semiconductor components to substrates, but it had problems such as poor heat resistance and resistance to thermal shock.
[0004] As a bonding technology to replace solder, the focus is on metal sintering bonding using silver and copper particles. However, in order to perform metal sintering bonding, the components to be bonded, such as substrates, need to undergo surface treatment, and the film formed by this surface treatment also requires heat resistance.
[0005] The inventors of this invention have discovered that electroless nickel alloy plating is suitable as a surface treatment for silver sintering or copper sintering. Electroless nickel alloy plating includes electroless nickel-phosphorus plating, electroless nickel-boron plating, etc., and in particular, electroless nickel-phosphorus plating films have been practically applied in a wide range of fields.
[0006] However, the electroless nickel-phosphorus plating film with a phosphorus content of 6-12% by mass (see Patent Document 1) that is commonly used has poor heat resistance and thermal shock resistance, and cracks will occur when used in high temperature environments. Therefore, it is not suitable as a peripheral component of the next generation of power modules.
[0007] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2023-090169 Summary of the Invention
[0008] The problem that the invention aims to solve The purpose of this invention is to provide a coating film with excellent heat resistance and resistance to thermal shock, suitable for metal sintering bonding.
[0009] Technical solutions for solving the problem In order to solve the above-mentioned problems, the inventors of the present invention have repeatedly conducted in-depth research and found that in a plating film having an electroless nickel-phosphorus plating film (A), if the phosphorus content of the (A) electroless nickel-phosphorus plating film is within a specific range, the above-mentioned objective can be achieved, thereby completing the present invention.
[0010] That is, the present invention relates to the following coated film and its manufacturing method, as well as semiconductor mounting substrate.
[0011] 1. A coating film for metal sintering bonding, characterized in that: It is a metal sintering bonding coating with (A) an electroless nickel-phosphorus plating film. The phosphorus content of the electroless nickel-phosphorus plating film (A) is less than 4% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.
[0012] 2. The metal sintering bonding coating as described in item 1, wherein the sulfur content of the electroless nickel-phosphorus coating (A) is less than 0.0005% by mass when the electroless nickel-phosphorus coating is set to 100% by mass.
[0013] 3. The metal sintering bonding coating as described in item 1 or 2, wherein the sulfur content of the electroless nickel-phosphorus coating described in (A) is 0.0001% by mass or less when the electroless nickel-phosphorus coating is set to 100% by mass.
[0014] 4. The plating film for metal sintering bonding as described in any one of items 1 to 3, wherein the thickness of the electroless nickel-phosphorus plating film (A) is 0.1 to 20 μm or less.
[0015] 5. The metal sintering bonding coating as described in any one of items 1 to 4, wherein the (A) electroless nickel-phosphorus coating is further provided with (B) an electroless silver coating or an electroless gold coating.
[0016] 6. The plating film for metal sintering bonding as described in item 5, wherein the thickness of the electroless silver plating film or the electroless gold plating film of (B) is 0.02 to 2 μm.
[0017] 7. The metal sintering bonding coating as described in item 5 or 6, wherein a barrier metal layer (C) is further provided between the above-mentioned (A) electroless nickel-phosphorus plating coating and the above-mentioned (B) electroless silver plating coating or electroless gold plating coating.
[0018] 8. The metal sintering bonding coating as described in item 7, wherein the barrier metal layer (C) is an electroless palladium coating or an electroless palladium-phosphorus coating.
[0019] 9. The coating film for metal sintering bonding as described in any one of items 1 to 9, which is used for metal sintering materials containing silver and / or copper.
[0020] 10. A method for manufacturing a plating film for metal sintering bonding, comprising forming a plating film for metal sintering bonding on a substrate, characterized in that: Step 1 comprises: (1) contacting an electroless nickel-phosphorus plating solution with the surface of a substrate to form an (A) electroless nickel-phosphorus plating film on the substrate. The phosphorus content of the electroless nickel-phosphorus plating film (A) is less than 4% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.
[0021] 11. The manufacturing method as described in item 10, further comprising step 2 of (2) contacting the electroless silver plating solution or the electroless gold plating solution with the surface of the electroless nickel-phosphorus plating film to form (B) the electroless silver plating film or the electroless gold plating film on the (A) electroless nickel-phosphorus plating film.
[0022] 12. A semiconductor mounting substrate, characterized in that: A metal sintering bonding coating having an electroless nickel-phosphorus plating film (A) is laminated on the substrate. A semiconductor element is formed on the aforementioned metal sintering bonding coating through a metal sintering material layer. The phosphorus content of the electroless nickel-phosphorus plating film (A) is less than 4% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.
[0023] Invention Effects The metal sintering bonding coating of the present invention exhibits excellent heat resistance and thermal shock resistance. Therefore, it can be suitably used in metal sintering bonding applications used in next-generation power modules. Furthermore, the manufacturing method of the coating coating of the present invention can produce a coating coating with excellent heat resistance and thermal shock resistance, suitable for use in metal sintering bonding applications. Moreover, the semiconductor mounting substrate of the present invention exhibits excellent heat resistance and thermal shock resistance. Detailed Implementation
[0024] The present invention will now be described in detail.
[0025] In the metal sintering bonding coating of the present invention, when the (A) electroless nickel-phosphorus coating is stacked on the substrate, the direction of the side opposite to the side in contact with the substrate is called "upper" or "surface", and the direction of the opposite side, that is, the side of the (A) electroless nickel-phosphorus coating in contact with the substrate, is called "lower" or "back side".
[0026] 1. Coated film for metal sintering bonding The metal sintering bonding coating (hereinafter, simply referred to as "coating coating") of the present invention is a coating having an electroless nickel-phosphorus coating (hereinafter, also referred to as "(A) layer"), wherein the phosphorus content of the aforementioned electroless nickel-phosphorus coating is 4% by mass or less when the electroless nickel-phosphorus coating is set to 100% by mass. Because the coating of the present invention has the aforementioned (A) layer, the (A) layer can suppress the oxidation of the substrate, can fix the semiconductor element via the metal sintering material, and release the heat generated from the semiconductor element, thus making it suitable for the actual mounting of the semiconductor element. Furthermore, by making the phosphorus content of the (A) layer 4% by mass or less when the electroless nickel-phosphorus coating is 100% by mass, the coating of the present invention exhibits excellent heat resistance and resistance to thermal shock, making it suitable for metal sintering bonding.
[0027] Hereinafter, each of the plating films constituting the metal sintering bonding coating of the present invention will be described in detail.
[0028] (A) Electroless nickel-phosphorus plating film) The metal sintering bonding coating of the present invention has (A) an electroless nickel-phosphorus plating coating.
[0029] The phosphorus content of the electroless nickel-phosphorus plating film is 4% by mass or less when the electroless nickel-phosphorus plating film is set to 100% by mass. When the phosphorus content exceeds 4% by mass, the heat resistance and thermal shock resistance are poor, and cracks will occur in the plating film. Therefore, the bonding with the metal sintering material is insufficient, making it unsuitable for the mounting of semiconductor devices. The phosphorus content is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less. In addition, the lower limit of the phosphorus content is not particularly limited and can be 0.1% by mass, 0.2% by mass, or 0.5% by mass. The phosphorus content of the electroless nickel-phosphorus plating film can be reduced by changing the composition and plating conditions of the electroless nickel-phosphorus plating.
[0030] In layer (A), the sulfur content is preferably less than 0.0005% by mass when the electroless nickel-phosphorus plating film of layer (A) is set to 100% by mass, more preferably less than 0.0002% by mass, even more preferably less than 0.0001% by mass, and particularly preferably sulfur-free, at 0% by mass. By keeping the sulfur content of layer (A) within the above range, the heat resistance and thermal shock resistance of the plating film of the present invention are further improved, and the generation of cracks can be suppressed. Therefore, it is suitable for mounting semiconductor devices via metal sintering materials. The sulfur content can be reduced by decreasing the amount of divalent sulfur in the composition of the electroless nickel-phosphorus plating solution used to form layer (A).
[0031] The thickness of layer (A) is not particularly limited, but is preferably 0.1 to 20 μm, more preferably 0.2 to 10 μm, and even more preferably 0.5 to 5 μm.
[0032] (B) Electroless silver plating film or electroless gold plating film) The metal sintering bonding coating of the present invention may have an electroless silver plating coating or an electroless gold plating coating (hereinafter also referred to as "(B) layer") on top of the (A) layer. By having the metal sintering bonding coating of the present invention have the (B) layer, the bonding with the metal sintering material can be further improved, the semiconductor element can be fixed through the metal sintering material and the heat generated from the semiconductor element can be released, making it more suitable for the mounting of the semiconductor element.
[0033] The thickness of layer (B) is not particularly limited, but from the viewpoint that the semiconductor element can be further fixed by the metal sintering material and the heat generated from the semiconductor element can be easily released in the fixed semiconductor element state, it is preferably 0.02 to 2 μm.
[0034] When layer (B) is an electroless silver plating film, the thickness of layer (B) is preferably 0.02 to 1 μm, more preferably 0.05 to 0.5 μm. Furthermore, when layer (B) is an electroless gold plating film, the thickness of layer (B) is preferably 0.02 to 1 μm, more preferably 0.03 to 0.2 μm.
[0035] (C) Barrier metal layer) The metal sintering bonding coating of the present invention may further include a barrier metal layer (hereinafter also referred to as "(C) layer") between layer (A) and layer (B). By including layer (C) in the metal sintering bonding coating of the present invention, surface diffusion of the base metal and corrosion of the nickel-phosphorus plating coating caused by electroless silver plating or electroless gold plating can be further suppressed, thus further improving the bonding with the metal sintering material.
[0036] There is no particular limitation on layer (C), and known plating films can be cited as examples. Examples of layer (C) include electroless palladium plating films, electroless palladium-phosphorus plating films, electroless platinum plating films, electroless cobalt-phosphorus plating films, and electroless cobalt-boron plating films. Among these, from the viewpoint of further suppressing surface diffusion of the substrate metal and corrosion of the nickel-phosphorus plating film caused by electroless silver or gold plating, electroless palladium plating films and electroless palladium-phosphorus plating films are preferred.
[0037] When layer (C) contains phosphorus, such as in an electroless palladium-phosphorus plating film, the phosphorus content in layer (C) is preferably 0.1 to 2.0% by mass when layer (C) is set to 100% by mass, more preferably 0.5 to 1.5% by mass. By keeping the phosphorus content in layer (C) within the above range, surface diffusion of the base metal and corrosion of the nickel-phosphorus plating film caused by electroless silver or electroless gold plating can be further suppressed.
[0038] (Characteristics of coating film for metal sintering) The thickness of the plating film for metal sintering bonding of the present invention is not particularly limited, but is preferably 1 to 10 μm, more preferably 1.5 to 8 μm, and even more preferably 2 to 5 μm. By keeping the thickness of the plating film for metal sintering bonding within the above range, the semiconductor to be mounted can be more firmly fixed, and oxidation can be further suppressed.
[0039] The plating film for metal sintering bonding of the present invention, as described above, has the aforementioned configuration and therefore exhibits excellent heat resistance and resistance to thermal shock. Consequently, it is suitable for use in metal sintering bonding in next-generation power modules. The plating film for metal sintering bonding of the present invention is particularly suitable for silver sintering bonding or copper sintering bonding. That is, the plating film for metal sintering bonding of the present invention is suitable for use as a metal sintering material containing silver and / or copper.
[0040] 2. Method for manufacturing a coating film for metal sintering bonding The manufacturing method of the metal sintering bonding coating of the present invention is a method for forming a metal sintering bonding coating on a substrate, characterized by comprising: (1) a step 1 in which an electroless nickel-phosphorus plating solution is brought into contact with the surface of a substrate to form an (A) electroless nickel-phosphorus plating coating on the substrate, wherein the phosphorus content of the (A) electroless nickel-phosphorus plating coating is 4% by mass or less when the electroless nickel-phosphorus plating coating is set to 100% by mass. Using the manufacturing method of the present invention, it is possible to manufacture a metal sintering bonding coating of the present invention that exhibits excellent heat resistance and resistance to thermal shock, and is suitable for applications involving metal sintering bonding.
[0041] The following is a description of each process.
[0042] (Process 1) Step 1 is a process of bringing an electroless nickel-phosphorus plating solution into contact with the surface of a substrate to form an (A) electroless nickel-phosphorus plating film on the substrate.
[0043] As for the substrate (the object to be plated) used in process 1, examples include substrates used in electronic components such as semiconductors and circuits. Examples of such substrates include printed wiring substrates, ceramic substrates, silicon substrates, and metal substrates. Specifically, examples include semiconductor chips (mainly back electrodes) made of SiC, GaN, Si, etc., metal lead frames, or insulating and heat-dissipating circuit substrates (ceramic substrates) such as DBC (Direct Bonded Copper), DBA (Direct Bonded Aluminum), and AMB (Active Metal Brazing), and heat dissipation substrates such as heat sinks. As for the material of the plated portion of the object to be plated, examples include copper, copper alloys, aluminum, and aluminum alloys.
[0044] The electroless nickel-phosphorus plating solution used in step 1 is not particularly limited as long as it can adjust the phosphorus content of the electroless nickel-phosphorus plating film produced in step 1 to 4% by mass or less when the electroless nickel-phosphorus plating film is set to 100% by mass. Examples of such electroless nickel-phosphorus plating solutions include those containing water-soluble nickel compounds, reducing agents, and complexing agents, and, if necessary, other additives. Hereinafter, such an electroless nickel-phosphorus plating solution will be described by way of example.
[0045] (Water-soluble nickel compounds) The water-soluble nickel compound contained in the electroless nickel-phosphorus plating solution used in the manufacturing method of the present invention is not particularly limited, and any known nickel compound used in electroless nickel-phosphorus plating solutions can be used. The water-soluble nickel compound is preferably, for example, a water-soluble inorganic nickel salt such as nickel sulfate, nickel chloride, nickel hypophosphite, or nickel carbonate; a water-soluble organic nickel salt such as nickel acetate or nickel malate; or its hydrates.
[0046] Water-soluble nickel compounds can be used alone or in combination of two or more.
[0047] The concentration of water-soluble nickel compounds in the electroless nickel-phosphorus plating solution is not particularly limited as long as it is within the range sufficient to form an electroless nickel-phosphorus plating film, and can be adjusted appropriately. The concentration of water-soluble nickel compounds, calculated in nickel metal, is preferably set to, for example, about 0.01 g / L to 100 g / L, more preferably 0.5 to 50 g / L, and even more preferably 1 g / L to 10 g / L. When the concentration of water-soluble nickel compounds, calculated in nickel metal, is below 0.01 g / L, the precipitation rate may sometimes slow down; when it exceeds 100 g / L, the stability of the plating bath may sometimes decrease. Therefore, the above-mentioned ranges are preferred.
[0048] (reducing agent) The reducing agent is preferably at least one selected from hypophosphorous acid and hypophosphite (e.g., sodium salt, potassium salt, ammonium salt, etc.).
[0049] A reducing agent can be used alone or in combination of two or more.
[0050] The concentration of the reducing agent (hypophosphoric acid, hypophosphite, and its hydrate, etc.) in the electroless nickel-phosphorus plating solution is preferably about 0.5 g / L to 40 g / L, more preferably about 1 g / L to 20 g / L, and even more preferably about 2 g / L to 15 g / L. By setting the upper limit of the concentration to the above range, it is easy to adjust the phosphorus content of the formed electroless nickel-phosphorus plating film to 4% by mass or less. In addition, by setting the lower limit of the concentration to the above range, the precipitation properties of the electroless nickel-phosphorus plating can be made more stable.
[0051] (Complexing agent) Electroless nickel-phosphorus plating solutions preferably contain glycine, gluconate, or similar complexing agents. Gluconate is preferably, for example, a sodium salt, potassium salt, or ammonium salt.
[0052] Other complexing agents are preferably: monocarboxylic acids such as formic acid and acetic acid, or their salts (e.g., sodium, potassium, ammonium salts, etc.); dicarboxylic acids such as malonic acid, succinic acid, adipic acid, maleic acid, and fumaric acid, or their salts (e.g., sodium, potassium, ammonium salts, etc.); hydroxycarboxylic acids such as malic acid, lactic acid, glycolic acid, and citric acid, or their salts (e.g., sodium, potassium, ammonium salts, etc.); ethylenediaminediacetic acid, ethylenediaminetetraacetic acid, or their salts (e.g., sodium, potassium, ammonium salts, etc.); and amino acids such as alanine and arginine.
[0053] Complexing agents can be used alone or in combination of two or more.
[0054] The concentration of the complexing agent in the electroless nickel-phosphorus plating bath is not particularly limited and can be adjusted appropriately. The electroless nickel-phosphorus plating bath preferably contains approximately 1 g / L to 100 g / L, more preferably approximately 2 g / L to 50 g / L, and even more preferably approximately 5 g / L to 30 g / L of complexing agent. When the concentration of the complexing agent is below 1 g / L, the stability of the plating bath may decrease; when it exceeds 100 g / L, the precipitation rate may decrease. Therefore, the concentrations within the above ranges are preferred.
[0055] (Stabilizers, sulfur-based additives, pH adjusters, surfactants, etc.) In addition to the components mentioned above, the electroless nickel-phosphorus plating solution may also contain known additives used in electroless nickel-phosphorus plating solutions, as needed. Examples of such additives include stabilizers, sulfur-based additives, pH adjusters, and surfactants.
[0056] Stabilizers can be categorized as follows: lead compounds (e.g., lead nitrate, lead acetate), cadmium compounds (e.g., cadmium nitrate, cadmium acetate), thallium compounds (e.g., thallium sulfate, thallium nitrate), antimony compounds (e.g., antimony chloride, potassium antimony tartrate), tellurium compounds (e.g., telluric acid, tellurium chloride), chromium compounds (e.g., chromium oxide, chromium sulfate), iron compounds (e.g., ferric sulfate, ferric chloride), manganese compounds (e.g., manganese sulfate, manganese nitrate), bismuth compounds (e.g., bismuth nitrate, bismuth acetate), tin compounds (e.g., tin sulfate, tin chloride), selenium compounds (e.g., selenic acid, selenite), cyanides (e.g., methyl cyanide, isopropyl cyanide), and iodine compounds (e.g., potassium iodide).
[0057] Stabilizers can be used alone or in combination of two or more.
[0058] The concentration of the stabilizer in the electroless nickel-phosphorus plating solution is not particularly limited, and can be set to approximately 0.1 mg / L to 500 mg / L. However, to improve the stability of the electroless nickel-phosphorus plating solution, it is preferable to set the stabilizer concentration to approximately 0.1 mg / L or higher. When the stabilizer concentration exceeds 500 mg / L, areas where a plating film cannot form (unprecipitated areas) may occur; therefore, it is preferable to set it within the above-mentioned range.
[0059] The preferred sulfur-based additives are divalent sulfur compounds such as thiourea. From the viewpoint of further reducing the sulfur content of the electroless nickel-phosphorus plating film, it is preferable to set it to the minimum required level or not add it at all.
[0060] pH adjusters are preferably acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; and bases such as sodium hydroxide, potassium hydroxide, and ammonia.
[0061] The pH of the electroless nickel-phosphorus plating bath is preferably around 3 to 12, and more preferably around 4 to 9. The pH of the plating bath can be adjusted using the pH adjuster described above. When the pH is below 3, precipitation may sometimes occur, and when it exceeds 12, the stability of the plating bath may sometimes decrease. Therefore, it is preferable to set it within the range described above.
[0062] As surfactants, various surfactants, including nonionic, anionic, cationic, and amphoteric surfactants, can be used. Examples include aromatic or aliphatic sulfonic acid base salts and aromatic or aliphatic sulfonic acid alkali metal salts. Surfactants can be used alone or in mixtures of two or more. When mixing two or more surfactants, the mixing ratio is not particularly limited and can be appropriately determined.
[0063] The concentration of the surfactant in the electroless nickel-phosphorus plating solution is not particularly limited and can be set to, for example, around 0.01 mg / L to 1000 mg / L. For the purpose of further improving the anti-pitting effect of the electroless nickel-phosphorus plating solution, it is preferable to set the surfactant concentration to around 0.01 mg / L or higher. When the surfactant concentration is below 1000 mg / L, the reduction in precipitation caused by foaming is further suppressed.
[0064] (Electrolytic nickel-phosphorus plating method) In step 1, the electroless nickel-phosphorus plating solution is brought into contact with the surface of the substrate.
[0065] There are no particular limitations on the method of bringing the surface of the substrate into contact with the electroless plating solution, and it can be performed according to conventional methods. In step 1, a preferred example is immersing the substrate, which is to be plated, in an electroless nickel-phosphorus plating solution.
[0066] Regarding the plating conditions (e.g., liquid temperature, plating time, etc.), there are no special restrictions as long as the conditions can form an electroless nickel-phosphorus plating film, and they can be appropriately determined.
[0067] The temperature of the electroless nickel-phosphorus plating solution in step 1 can be appropriately determined based on its composition. For example, the temperature of the electroless nickel-phosphorus plating solution in the plating process can preferably be set to around 25°C or higher, more preferably around 40°C to 100°C, and even more preferably around 45°C to 95°C. When the temperature is below 25°C, the deposition rate of the plating film may slow down, reducing production efficiency; therefore, it is preferable to set it within the above-mentioned range.
[0068] The processing time in step 1 is not particularly limited and can be set to the time until an electroless plating film of the required thickness is formed on the object to be plated. Specifically, the processing time in the plating process can be appropriately determined according to the composition of the plating bath, the type of object to be plated, etc. For example, it is preferably set to about 1 minute to 120 minutes, and more preferably to 3 minutes to 60 minutes.
[0069] The electroless nickel-phosphorus plating film formed on the substrate by process 1 is the (A) electroless nickel-phosphorus plating film of the metal sintering bonding plating film of the present invention described above, wherein the phosphorus content is 4% by mass or less when the electroless nickel-phosphorus plating film is set to 100% by mass. The characteristics of the (A) electroless nickel-phosphorus plating film formed on the substrate by process 1 are the same as those described for the (A) electroless nickel-phosphorus plating film in the metal sintering bonding plating film of the present invention.
[0070] As a method to adjust the phosphorus content in the electroless nickel-phosphorus plating film (A) to below 4% by mass, one method can be listed as (i) adjusting the content of the reducing agent in the electroless nickel-phosphorus plating solution. If the content of the reducing agent in the electroless nickel-phosphorus plating solution increases, the phosphorus content of the formed electroless nickel-phosphorus plating film increases; if the content of the reducing agent in the electroless nickel-phosphorus plating solution decreases, the phosphorus content of the electroless nickel-phosphorus plating film decreases. Additionally, as a method of adjustment as described above, one method can be listed as (ii) adjusting the pH of the electroless nickel-phosphorus plating solution in step 1. If the pH decreases, the phosphorus content of the formed electroless nickel-phosphorus plating film increases; if the pH increases, the phosphorus content of the electroless nickel-phosphorus plating film decreases. Additionally, as a method of adjustment as described above, (iii) adjusting the liquid temperature of the electroless nickel-phosphorus plating solution in step 1 can be listed. As the liquid temperature increases, the phosphorus content of the electroless nickel-phosphorus plating film decreases; as the liquid temperature decreases, the phosphorus content of the electroless nickel-phosphorus plating film increases.
[0071] As a method for adjusting the sulfur content in the electroless nickel-phosphorus plating film (A), one method is to adjust the content of divalent sulfur compounds, such as thiourea, in the electroless nickel-phosphorus plating solution. If the content of divalent sulfur compounds in the electroless nickel-phosphorus plating solution increases, the sulfur content of the formed electroless nickel-phosphorus plating film increases; if the content of divalent sulfur compounds in the electroless nickel-phosphorus plating solution decreases, the sulfur content of the electroless nickel-phosphorus plating film decreases.
[0072] Through process 1 described above, an electroless nickel-phosphorus plating film (A) is formed on the substrate.
[0073] (Process 2) The manufacturing method of the present invention may further include step 2 after step 1, which involves (2) bringing an electroless silver plating solution or an electroless gold plating solution into contact with the surface of the electroless nickel-phosphorus plating film to form an (B) electroless silver plating film or an electroless gold plating film on the (A) electroless nickel-phosphorus plating film.
[0074] There are no particular limitations on the electroless silver plating solution or electroless gold plating solution used in step 2; any existing known plating solution can be used. The electroless silver plating solution and electroless gold plating solution used in step 2 will be described below.
[0075] Electroless silver plating solution There are no particular limitations on the electroless silver plating solution; for example, reduction-deposition type, displacement-reduction type, and displacement-deposition type electroless silver plating solutions can be used. As reduction-deposition type or displacement-reduction type electroless silver plating solutions, solutions containing silver compounds, reducing agents, and complexing agents, and other additives as needed, can be used. Furthermore, as displacement-deposition type electroless silver plating, solutions containing silver compounds, complexing agents, and other additives as needed can be used. The following provides an exemplary description of such electroless silver plating solutions.
[0076] (Silver compound) As for the silver compound, any water-soluble silver compound is acceptable; there are no particular limitations, and known silver compounds used in electroless silver plating solutions can be used. Examples of silver compounds include inorganic salts such as silver nitrate, silver sulfate, and silver iodide; and organic acid salts such as silver acetate and silver methanesulfonate.
[0077] Silver compounds can be used alone or in combination of two or more.
[0078] The concentration of silver compounds in the electroless silver plating solution is not particularly limited as long as it is within the range sufficient to form an electroless silver plating film, and can be adjusted appropriately. The concentration of silver compounds, calculated in terms of silver metal, is preferably set to, for example, about 0.01 g / L to 20 g / L, more preferably 0.1 to 10 g / L, and even more preferably 0.2 g / L to 5 g / L. When the concentration of silver compounds, calculated in terms of silver metal, is below 0.01 g / L, the precipitation rate may slow down; when it exceeds 20 g / L, the stability of the plating bath may decrease. Therefore, the above-mentioned ranges are preferred.
[0079] (reducing agent) The reducing agent is preferably selected from at least one of water-soluble aldehyde compounds, water-soluble hydrazine derivatives, borohydrides, hypophosphorous acid, phosphorous acid, ascorbic acid, and their salts (e.g., sodium salts, potassium salts, ammonium salts, etc.). Alternatively, when using a displacement-precipitation type electroless silver plating solution, the reducing agent may be omitted.
[0080] A reducing agent can be used alone or in combination of two or more. Additionally, when using a displacement-precipitation type electroless silver plating solution, a reducing agent may not be required.
[0081] The concentration of the reducing agent in the electroless silver plating solution is preferably about 0.5 g / L to 15 g / L, more preferably about 1 g / L to 13 g / L, and even more preferably about 1.5 g / L to 10 g / L.
[0082] (Complexing agent) Electroless silver plating solutions preferably contain amide compounds, imide compounds, thiosulfate compounds, sulfite compounds, sulfur-containing compounds (sulfide-containing compounds other than thiosulfate compounds and sulfite compounds), and nitrogen-containing compounds (nitrogen-containing compounds other than amide compounds and imide compounds) as complexing agents, and more preferably contain amide compounds and imide compounds.
[0083] Examples of amide compounds include cyclic amide compounds such as benzamide, N-methylpyrrolidone, N-ethylpyrrolidone, N-vinylpyrrolidone, pyrrolidone, N-butylpyrrolidone, 5-methylpyrrolidone, and N-methylpiperidone; and chain amide compounds such as acetamide, formamide, N,N-dimethylformamide, N-methyl-N-phenylformamide, and N,N-diphenylformamide. These can be used alone or in combination of two or more. Chain amide compounds are preferred, and acetamide and formamide are more preferred.
[0084] The imide compound is not particularly limited, but cyclic imide compounds such as hydantoin, 5,5-dimethylhydantoin, 1-methylhydantoin, 1,3-dimethylhydantoin, glutarimide, and succinimide are preferred. Hydantoin, 5,5-dimethylhydantoin, 1-methylhydantoin, succinimide, 1,3-methylhydantoin, and glutarimide are more preferred. 1-methylhydantoin and succinimide are even more preferred.
[0085] Complexing agents can be used alone or in combination of two or more.
[0086] The concentration of the complexing agent in the electroless silver plating solution is not particularly limited and can be adjusted appropriately. Preferably, the electroless silver plating solution contains approximately 1 g / L to 100 g / L, more preferably 2 g / L to 50 g / L, and even more preferably 5 g / L to 30 g / L of complexing agent. When the concentration of the complexing agent is below 1 g / L, the stability of the plating bath may decrease; when it exceeds 100 g / L, the precipitation rate may decrease. Therefore, the concentrations within the above ranges are preferred.
[0087] (Stabilizers, pH adjusters, surfactants, etc.) In addition to the components mentioned above, the electroless silver plating solution may also contain known additives used in electroless silver plating solutions, as needed. Examples of additives include stabilizers, pH adjusters, and surfactants.
[0088] Stabilizers can be categorized as follows: lead compounds (e.g., lead nitrate, lead acetate), cadmium compounds (e.g., cadmium nitrate, cadmium acetate), thallium compounds (e.g., thallium sulfate, thallium nitrate), antimony compounds (e.g., antimony chloride, potassium antimony tartrate), tellurium compounds (e.g., telluric acid, tellurium chloride), chromium compounds (e.g., chromium oxide, chromium sulfate), iron compounds (e.g., ferric sulfate, ferric chloride), manganese compounds (e.g., manganese sulfate, manganese nitrate), bismuth compounds (e.g., bismuth nitrate, bismuth acetate), tin compounds (e.g., tin sulfate, tin chloride), selenium compounds (e.g., selenic acid, selenite), cyanides (e.g., methyl cyanide, isopropyl cyanide), and iodine compounds (e.g., potassium iodide).
[0089] Stabilizers can be used alone or in combination of two or more.
[0090] The concentration of the stabilizer in the electroless silver plating solution is not particularly limited, and can be set to approximately 0.1 mg / L to 500 mg / L. However, for the purpose of improving the stability of the electroless silver plating solution, it is preferable to set the stabilizer concentration to approximately 0.1 mg / L or higher. When the stabilizer concentration exceeds 500 mg / L, areas where a plating film cannot form (unprecipitated areas) may occur; therefore, the above-mentioned range is preferred.
[0091] pH adjusters are preferably acids such as nitric acid, sulfuric acid, and phosphoric acid; and bases such as sodium hydroxide, potassium hydroxide, and ammonia.
[0092] The pH of the electroless silver plating solution is preferably around 1 to 12, more preferably around 1.5 to 11. The pH of the plating bath can be adjusted using the pH adjuster described above. When the pH is below 1, precipitation may sometimes occur, and when it exceeds 12, the stability of the plating bath may sometimes decrease; therefore, it is preferable to set it within the range described above.
[0093] As surfactants, various surfactants, including nonionic, anionic, cationic, and amphoteric surfactants, can be used. Examples include aromatic or aliphatic sulfonic acid base salts and aromatic or aliphatic sulfonic acid alkali metal salts. Surfactants can be used alone or in mixtures of two or more. When mixing two or more surfactants, the mixing ratio is not particularly limited and can be appropriately determined.
[0094] The concentration of the surfactant in the electroless silver plating solution is not particularly limited and can be set to, for example, around 0.01 mg / L to 1000 mg / L. For the purpose of further improving the anti-pitting effect of the electroless silver plating solution, it is preferable to set the surfactant concentration to around 0.01 mg / L or higher. When the surfactant concentration is below 1000 mg / L, the reduction in precipitation caused by foaming is further suppressed.
[0095] (Method of electroless silver plating) There are no particular limitations on the method for forming an electroless silver plating film on an electroless nickel-phosphorus plating film in step 2. For example, a method can be used to bring the electroless silver plating solution into contact with the surface of the electroless nickel-phosphorus plating film formed in step 1.
[0096] There are no particular limitations on the method for bringing the surface of the electroless nickel-phosphorus plating film into contact with the electroless silver plating solution, and it can be carried out according to conventional methods. In step 2, a preferred example is immersing the substrate with the electroless nickel-phosphorus plating film formed thereon in the electroless silver plating solution.
[0097] Regarding the plating conditions (e.g., liquid temperature, plating time, etc.), there are no special restrictions as long as the conditions are suitable for forming an electroless silver plating film, and they can be appropriately determined.
[0098] The temperature of the electroless silver plating solution in step 2 can be appropriately determined based on its composition. For example, the temperature of the electroless silver plating solution in the plating process can preferably be set to around 25°C or higher, more preferably around 30°C to 80°C, and even more preferably around 40°C to 75°C. When the temperature is below 25°C, the deposition rate of the plating film may slow down, reducing production efficiency; therefore, the above-mentioned range is preferred.
[0099] The processing time in step 2 is not particularly limited and can be set to the time until an electroless silver plating film of the required thickness is formed. Specifically, the processing time in the plating process can be appropriately determined according to the composition of the electroless silver plating solution, for example, preferably set to about 1 minute to 40 minutes, more preferably set to 3 minutes to 20 minutes.
[0100] The electroless silver plating solution formed in step 2 is an electroless silver plating film (B layer) that can be present in the plating film for metal sintering bonding of the present invention. The characteristics of the electroless silver plating film formed on the substrate in step 2 are the same as those described as layer (B) in the plating film for metal sintering bonding of the present invention.
[0101] Electroless gold plating solution There are no particular limitations on the electroless gold plating solution; for example, reduction-deposition type, displacement-reduction type, and displacement-deposition type electroless gold plating solutions can be used. As reduction-deposition type or displacement-reduction type electroless gold plating solutions, solutions containing gold compounds, reducing agents, and complexing agents, and other additives as needed, can be used. Furthermore, as displacement-deposition type electroless gold plating, solutions containing gold compounds, complexing agents, and other additives as needed can be used. The following provides an exemplary description of such electroless gold plating solutions.
[0102] (Gold compounds) As for the gold compound, any water-soluble gold compound is acceptable; there are no particular limitations, and known gold compounds used in electroless gold plating solutions can be used. Examples of gold compounds include potassium gold sulfite, sodium gold sulfite, ammonium gold sulfite, potassium gold cyanide, sodium gold cyanide, and ammonium gold cyanide.
[0103] Gold compounds can be used alone or in combination of two or more.
[0104] The concentration of the gold compound in the electroless gold plating solution is not particularly limited as long as it is within the range sufficient to form an electroless gold plating film, and can be adjusted appropriately. The concentration of the gold compound, calculated in gold metal, is preferably set to, for example, about 0.01 g / L to 10 g / L, more preferably 0.2 to 5 g / L, and even more preferably 0.5 g / L to 2 g / L. When the concentration of the gold compound, calculated in gold metal, is below 0.01 g / L, the deposition rate may slow down; when it exceeds 10 g / L, the cost increases. Therefore, the above-mentioned range is preferred.
[0105] (reducing agent) There are no particular limitations on the reducing agent; the same reducing agents used in known electroless gold plating solutions can be used. For example, hydrazine derivatives such as hydrazine hydrate, hydrazine sulfate, neutral hydrazine sulfate, hydrazine maleate, and their salts can be used; hydroxylamine derivatives and their salts; hydrazine derivatives such as adipic acid dihydrazide, isophthalic acid dihydrazide, and isopropyl hydrazine sulfate; ascorbic acid and its salts (sodium, potassium, ammonium, etc.); borohydrides such as trimethylamine borane (TMAB) and dimethylamine borane (DMAB); thiourea; hypophosphite and its salts (sodium, potassium, ammonium, etc.).
[0106] A reducing agent can be used alone or in combination of two or more. Furthermore, a reducing agent may not be necessary when performing displacement-precipitation electroless gold plating.
[0107] The concentration of the reducing agent in the electroless gold plating solution is preferably about 1 g / L to 15 g / L, more preferably about 2 g / L to 13 g / L, and even more preferably about 3 g / L to 10 g / L. (Complexing agent) There are no particular limitations on the complexing agent; any complexing agent known to be used in electroless gold plating solutions can be used. For example, sulfites such as sodium sulfite, potassium sulfite, and ammonium sulfite can be used; cyanides such as sodium cyanide and potassium cyanide; thiosulfates such as sodium thiosulfate, potassium thiosulfate, and ammonium thiosulfate; inorganic acids such as phosphoric acid and boric acid, and their salts (sodium salts, potassium salts, ammonium salts, etc.); hydroxycarboxylic acids such as citric acid, gluconic acid, tartaric acid, lactic acid, and malic acid, and their salts (sodium salts, potassium salts, ammonium salts, etc.); amine compounds such as ethylenediamine and triethanolamine; aminocarboxylic acids such as glycine, alanine, ethylenediaminetetraacetic acid, and hypozoxytriacetic acid, and their salts (sodium salts, potassium salts, ammonium salts, etc.); phosphonic acids such as aminotrimethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetramethylenephosphonic acid, and diethylenetriaminepenta (methylenephosphonic acid), and their salts (sodium salts, potassium salts, ammonium salts, etc.).
[0108] Complexing agents can be used alone or in combination of two or more.
[0109] The concentration of the complexing agent in the electroless gold plating solution is not particularly limited and can be adjusted appropriately. The electroless gold plating solution preferably contains approximately 1 g / L to 100 g / L, more preferably 2 g / L to 50 g / L, and even more preferably 5 g / L to 30 g / L of complexing agent. When the concentration of the complexing agent is below 1 g / L, the stability of the plating bath may decrease; when it exceeds 100 g / L, the precipitation rate may decrease. Therefore, the concentrations within the above ranges are preferred.
[0110] (Stabilizers, pH adjusters, surfactants, etc.) In addition to the components mentioned above, the electroless gold plating solution may also contain known additives used in electroless gold plating solutions, as needed. Examples of additives include stabilizers, pH adjusters, and surfactants.
[0111] Stabilizers can be categorized as follows: lead compounds (e.g., lead nitrate, lead acetate), cadmium compounds (e.g., cadmium nitrate, cadmium acetate), thallium compounds (e.g., thallium sulfate, thallium nitrate), antimony compounds (e.g., antimony chloride, potassium antimony tartrate), tellurium compounds (e.g., telluric acid, tellurium chloride), chromium compounds (e.g., chromium oxide, chromium sulfate), iron compounds (e.g., ferric sulfate, ferric chloride), manganese compounds (e.g., manganese sulfate, manganese nitrate), bismuth compounds (e.g., bismuth nitrate, bismuth acetate), tin compounds (e.g., tin sulfate, tin chloride), selenium compounds (e.g., selenic acid, selenite), cyanides (e.g., methyl cyanide, isopropyl cyanide), and iodine compounds (e.g., potassium iodide).
[0112] Stabilizers can be used alone or in combination of two or more.
[0113] The concentration of the stabilizer in the electroless gold plating solution is not particularly limited, and can be set to approximately 0.1 mg / L to 500 mg / L. However, to improve the stability of the electroless gold plating solution, it is preferable to set the stabilizer concentration to approximately 0.1 mg / L or higher. When the stabilizer concentration exceeds 500 mg / L, areas where a plating film cannot form (unprecipitated areas) may occur; therefore, the above-mentioned range is preferred.
[0114] pH adjusters are preferably acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; and bases such as sodium hydroxide, potassium hydroxide, and ammonia.
[0115] The pH of the electroless gold plating solution is preferably around 3 to 12, more preferably around 4 to 9. The pH of the plating bath can be adjusted using the pH adjuster described above. When the pH is below 3, precipitation may sometimes occur, and when it exceeds 12, the stability of the plating bath may sometimes decrease; therefore, the pH is preferably set within the range described above.
[0116] As surfactants, various surfactants, including nonionic, anionic, cationic, and amphoteric surfactants, can be used. Examples include aromatic or aliphatic sulfonic acid base salts and aromatic or aliphatic sulfonic acid alkali metal salts. Surfactants can be used alone or in mixtures of two or more. When mixing two or more surfactants, the mixing ratio is not particularly limited and can be appropriately determined.
[0117] The concentration of the surfactant in the electroless gold plating solution is not particularly limited and can be set to, for example, around 0.01 mg / L to 1000 mg / L. For the purpose of further improving the anti-pitting effect of the electroless gold plating solution, it is preferable to set the surfactant concentration to around 0.01 mg / L or higher. When the surfactant concentration is below 1000 mg / L, the reduction in precipitation caused by foaming is further suppressed.
[0118] (Method of electroless gold plating) There are no particular limitations on the method for forming an electroless gold plating film on an electroless nickel-phosphorus plating film in step 2. For example, a method can be used to bring the electroless gold plating solution into contact with the surface of the electroless nickel-phosphorus plating film formed in step 1.
[0119] There are no particular limitations on the method for bringing the surface of the electroless nickel-phosphorus plating film into contact with the electroless gold plating solution, and it can be carried out according to conventional methods. In step 2, a preferred example is immersing the substrate with the electroless nickel-phosphorus plating film formed thereon in the electroless gold plating solution.
[0120] Regarding the plating conditions (e.g., liquid temperature, plating time, etc.), there are no special restrictions as long as the conditions are suitable for forming an electroless gold plating film, and they can be appropriately determined.
[0121] The temperature of the electroless gold plating solution in step 2 can be appropriately determined based on its composition. For example, the temperature of the electroless gold plating solution in the plating process can preferably be set to around 25°C or higher, more preferably around 40°C to 90°C, and even more preferably around 45°C to 85°C. When the temperature is below 25°C, the deposition rate of the plating film may slow down, reducing production efficiency; therefore, the above-mentioned range is preferred.
[0122] The processing time in step 2 is not particularly limited and can be set to the time until an electroless gold plating film of the required thickness is formed. Specifically, the processing time in the plating process can be appropriately determined according to the composition of the electroless gold plating solution. For example, it is preferably set to about 1 minute to 40 minutes, and more preferably to 3 minutes to 20 minutes.
[0123] The electroless gold plating film formed by step 2 is an electroless gold plating film that can be included as layer (B) in the plating film for metal sintering bonding of the present invention. The characteristics of the electroless gold plating film formed by step 2 are the same as those described as layer (B) in the plating film for metal sintering bonding of the present invention.
[0124] Through step 2 described above, an electroless silver plating film or an electroless gold plating film is formed on an electroless nickel-phosphorus plating film (A).
[0125] (Barrier metal layer formation process) In the manufacturing method of the present invention, a barrier metal layer forming step may be performed between steps 1 and 2, wherein a plating solution for forming a barrier metal layer is brought into contact with the surface of the electroless nickel-phosphorus plating film, and a barrier metal layer (C) is formed on the electroless nickel-phosphorus plating film (A). By including the barrier metal layer forming step, a barrier metal layer (C) can be formed between layers (A) and (B).
[0126] As the barrier metal layer (C), there is no particular limitation, and known plating films can be cited as examples. Examples of layers (C) include electroless palladium plating films, electroless palladium-phosphorus plating films, electroless platinum plating films, electroless cobalt-phosphorus plating films, and electroless cobalt-boron plating films. Among these, from the viewpoint of further suppressing surface diffusion of the base metal and corrosion of the electroless nickel-phosphorus plating film caused by electroless silver or gold plating, electroless palladium plating films and electroless palladium-phosphorus plating films are preferred.
[0127] The following describes the electroless palladium plating solution and the electroless palladium-phosphorus plating solution used to form an electroless palladium plating film and an electroless palladium-phosphorus plating film as a barrier metal layer.
[0128] [Electrolytic palladium plating solution, electrolytic palladium-phosphorus plating solution] Electroless palladium plating solutions and electroless palladium-phosphorus plating solutions may include, for example, solutions containing palladium compounds, reducing agents, and complexing agents, and may also contain other additives as needed. The following provides exemplary descriptions of electroless palladium plating solutions and electroless palladium-phosphorus plating solutions.
[0129] (Palladium compounds) As for the palladium compound, any water-soluble palladium compound is acceptable; there are no particular limitations. Known palladium compounds used in electroless palladium plating solutions and electroless palladium-phosphorus plating solutions can be used. Examples of palladium compounds include palladium chloride, palladium sulfate, palladium acetate, and tetraamminedichloride.
[0130] Palladium compounds can be used alone or in combination of two or more.
[0131] The concentration of palladium compounds in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is not particularly limited as long as it is within the range that can form these plating films, and can be adjusted appropriately. The concentration of palladium compounds, calculated in palladium metal, is preferably set to approximately 0.01 g / L to 10 g / L, more preferably 0.2 to 5 g / L, and even more preferably 0.5 g / L to 2 g / L. When the concentration of palladium compounds, calculated in palladium metal, is below 0.01 g / L, the precipitation rate may slow down; when it exceeds 10 g / L, the stability of the plating bath may decrease. Therefore, the above-mentioned ranges are preferred.
[0132] (reducing agent) Formic acid, water-soluble aldehyde compounds, water-soluble hydrazine derivatives, and borohydride compounds are preferably used as reducing agents in electroless palladium plating solutions. Furthermore, at least one of hypophosphorous acid and hypophosphite (e.g., sodium, potassium, ammonium salts, etc.), phosphorous acid and phosphite (e.g., sodium, potassium, ammonium salts, etc.) is preferably used as a reducing agent in electroless palladium-phosphorus plating solutions.
[0133] A reducing agent can be used alone or in combination of two or more.
[0134] The concentration of the reducing agent in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is preferably about 1 g / L to 100 g / L, more preferably about 2 g / L to 50 g / L, and even more preferably about 5 g / L to 40 g / L.
[0135] (Complexing agent) There are no particular limitations on the complexing agent; any complexing agent known to be used in electroless palladium plating solutions and electroless palladium-phosphorus plating solutions can be used. As a complexing agent, examples include: amines such as ethylenediamine and diethylenetriamine; amino polycarboxylic acids such as ethylenediaminediacetic acid, ethylenediaminetetraacetic acid, and diethylenetriaminepentaacetic acid, or their salts (e.g., sodium salts, potassium salts, ammonium salts, etc.); amino acids such as glycine, alanine, iminodiacetic acid, hypozinotriacetic acid, L-glutamic acid, L-glutamic acid diacetic acid, L-aspartic acid, and taurine, or their salts (e.g., sodium salts, potassium salts, ammonium salts); and aminotrimethylenephosphonic acid. Monocarboxylic acids such as 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetramethylenephosphonic acid or their salts (e.g., sodium, potassium, ammonium salts), acetic acid, etc.; dicarboxylic acids such as malonic acid, succinic acid, adipic acid, maleic acid, fumaric acid, etc. or their salts (e.g., sodium, potassium, ammonium salts); hydroxycarboxylic acids such as malic acid, lactic acid, glycolic acid, citric acid, etc. or their salts (e.g., sodium, potassium, ammonium salts), etc.
[0136] Complexing agents can be used alone or in combination of two or more.
[0137] The concentration of the complexing agent in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is not particularly limited and can be adjusted appropriately. The electroless palladium plating solution and the electroless palladium-phosphorus plating solution preferably contain about 1 g / L to 100 g / L, more preferably about 2 g / L to 50 g / L, and even more preferably about 5 g / L to 30 g / L of complexing agent. When the concentration of the complexing agent is below 1 g / L, the stability of the plating bath may decrease; when it exceeds 100 g / L, the precipitation rate may decrease. Therefore, the concentrations within the above ranges are preferred.
[0138] (Stabilizers, pH adjusters, surfactants, etc.) In addition to the aforementioned components, the electroless palladium plating solution and the electroless palladium-phosphorus plating solution can also be formulated with known additives used in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution as needed. Examples of additives include, for example, stabilizers, pH adjusters, and surfactants.
[0139] Stabilizers can be categorized as follows: lead compounds (e.g., lead nitrate, lead acetate, etc.), cadmium compounds (e.g., cadmium nitrate, cadmium acetate, etc.), thallium compounds (e.g., thallium sulfate, thallium nitrate, etc.), antimony compounds (e.g., antimony chloride, potassium antimony tartrate, etc.), tellurium compounds (e.g., telluric acid, tellurium chloride, etc.), chromium compounds (e.g., chromium oxide, chromium sulfate, etc.), iron compounds (e.g., ferric sulfate, ferric chloride, etc.), manganese compounds (e.g., manganese sulfate, manganese nitrate, etc.), bismuth compounds (e.g., bismuth nitrate, bismuth acetate, etc.), tin compounds (e.g., tin sulfate, tin chloride, etc.), selenium compounds (e.g., selenic acid, selenite, etc.), cyanides (e.g., methyl cyanide, isopropyl cyanide, etc.), iodine compounds (e.g., potassium iodide, etc.), etc.
[0140] Stabilizers can be used alone or in combination of two or more.
[0141] The concentration of the stabilizer in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is not particularly limited, and can be set to approximately 0.1 mg / L to 500 mg / L. For the purpose of improving the stability of the electroless palladium plating solution and the electroless palladium-phosphorus plating solution, it is preferable to set the stabilizer concentration to approximately 0.1 mg / L or higher. When the stabilizer concentration exceeds 500 mg / L, areas where a plating film cannot be formed (unprecipitated areas) may occur; therefore, the above-mentioned range is preferred.
[0142] pH adjusters are preferably acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; and bases such as sodium hydroxide, potassium hydroxide, and ammonia.
[0143] The pH of the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is preferably around 3 to 12, more preferably around 4 to 9. The pH of the plating bath can be adjusted using the pH adjuster described above. When the pH is below 3, precipitation may sometimes occur, and when it exceeds 12, the stability of the plating bath may sometimes decrease; therefore, the pH ranges described above are preferred.
[0144] As surfactants, various surfactants, including nonionic, anionic, cationic, and amphoteric surfactants, can be used. Examples include aromatic or aliphatic sulfonic acid base salts and aromatic or aliphatic sulfonic acid alkali metal salts. Surfactants can be used alone or in mixtures of two or more. When mixing two or more surfactants, the mixing ratio is not particularly limited and can be appropriately determined.
[0145] The concentration of the surfactant in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is not particularly limited, and can be set to approximately 0.01 mg / L to 1000 mg / L. However, to further improve the anti-pitting effect of the electroless palladium plating solution and the electroless palladium-phosphorus plating solution, it is preferable to set the surfactant concentration to approximately 0.01 mg / L or higher. When the surfactant concentration is below 1000 mg / L, the reduction in precipitation caused by foaming is further suppressed.
[0146] (Method for forming barrier metal layer) In the barrier metal layer formation process, there is no particular limitation on the method of forming, for example, an electroless palladium plating solution and an electroless palladium-phosphorus plating solution on an electroless nickel-phosphorus plating film. Examples of methods include contacting the electroless palladium plating solution and the electroless palladium-phosphorus plating solution with the surface of the electroless nickel-phosphorus plating film formed in step 1.
[0147] The method for contacting the surface of the electroless nickel-phosphorus plating film with the electroless palladium plating solution and the electroless palladium-phosphorus plating solution is not particularly limited and can be performed according to conventional methods. In the barrier metal layer formation process, a preferred method is, for example, immersing the substrate with the electroless nickel-phosphorus plating film formed thereon in the electroless palladium plating solution and the electroless palladium-phosphorus plating solution.
[0148] Regarding the plating conditions (e.g., liquid temperature, plating time, etc.), there are no particular restrictions as long as the conditions can form an electroless palladium plating layer and an electroless palladium-phosphorus plating layer, and they can be appropriately determined.
[0149] The temperatures of the electroless palladium plating solution and the electroless palladium-phosphorus plating solution in the barrier metal layer formation process can be appropriately determined based on their composition. For example, the temperatures of the electroless palladium plating solution and the electroless palladium-phosphorus plating solution in the plating process are preferably set to around 25°C or higher, more preferably around 40°C to 90°C, and even more preferably around 45°C to 85°C. When the temperature is below 25°C, the deposition rate of the plating film may slow down, reducing production efficiency; therefore, the above-mentioned ranges are preferred.
[0150] The processing time in the barrier metal layer formation process is not particularly limited and can be set to the time until the desired electroless palladium plating layer or electroless palladium-phosphorus plating layer is formed. Specifically, the processing time in the plating process can be appropriately determined according to the composition of the electroless palladium plating solution or the electroless palladium-phosphorus plating solution, for example, preferably set to about 1 minute to 40 minutes, more preferably set to 3 minutes to 20 minutes.
[0151] Electroless palladium plating film and electroless palladium-phosphorus plating film formed by the barrier metal layer formation process are barrier metal layers that can be present as layer (C) in the plating film for metal sintering bonding of the present invention. The characteristics of the barrier metal layer formed by the barrier metal layer formation process are the same as those described as layer (C) in the plating film for metal sintering bonding of the present invention.
[0152] Through the barrier metal layer formation process described above, barrier metal layer (C) is formed on the above-mentioned electroless nickel-phosphorus plating film (A). By having the barrier metal layer formation process, barrier metal layer (C) can be formed between layer (A) and layer (B).
[0153] 3. Semiconductor mounting substrate The semiconductor mounting substrate of the present invention comprises a metal sintering bonding coating having an electroless nickel-phosphorus plating coating (A) on a substrate, wherein a semiconductor element is provided on the metal sintering bonding coating via a metal sintering material layer, and wherein the phosphorus content of the electroless nickel-phosphorus plating coating (A) is 4% by mass or less when the electroless nickel-phosphorus plating coating is set to 100% by mass.
[0154] In the semiconductor mounting substrate of the present invention, a metal sintering bonding plating film of the present invention is formed on the substrate, and a semiconductor element is bonded to the metal sintering bonding plating film via a metal sintering material layer.
[0155] The characteristics of the coating film for metal sintering bonding are the same as those described in the above description of the coating film for metal sintering bonding of the present invention.
[0156] In the semiconductor mounting substrate of the present invention, semiconductor elements are bonded via a metal sintering material layer.
[0157] As a sintering material for forming a metal sintering material layer, a sintering material paste containing metal powder and organic solvent can be used.
[0158] The metal powder contained in the sintering material paste is not particularly limited, and powders of metals known to be used in existing sintering materials can be used. Examples of such metals include silver, copper, and gold, among which copper and silver powders are preferred, and silver powders are more preferred.
[0159] There is no particular limitation on the average particle size of the metal powder; metal powders of known sizes can be used. The average particle size of the metal powder is preferably on the order of several μm to mm.
[0160] There are no particular limitations on the organic solvents contained in the sintering material paste; any known organic solvents used in existing sintering material pastes can be used. Examples of such organic solvents include methanol, ethanol, 1-propanol, 2-propanol, 2-butanol, 1-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 1-octanol, toluene, diethylene glycol, triethylene glycol, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, diethylene glycol monohexyl ether, terpineol, diethylene glycol methyl ether acetate terpineol, diisopropyl ether, tetrahydrofuran, and 1,4-dioxane. Among these, toluene, diethylene glycol, triethylene glycol, diethylene glycol monomethyl ether, terpineol, and diethylene glycol methyl ether acetate terpineol are suitable choices.
[0161] There is no particular limitation on the heating temperature during metal sintering; any temperature that is commonly used for metal sintering is acceptable, which is around 100 to 450°C.
[0162] The pressure during metal sintering can be either unpressurized or pressurized. When pressurized, the pressure is preferably around 0.1 MPa to 50 MPa, and more preferably around 0.2 MPa to 5 MPa.
[0163] As the configuration of the semiconductor mounting substrate of the present invention, it is sufficient that at least a metal sintering bonding plating film having an electroless nickel-phosphorus plating film (A) is stacked on the substrate, and a semiconductor element is formed on the metal sintering bonding plating film via a metal sintering material layer. That is, as the configuration of the semiconductor mounting substrate of the present invention, it is sufficient that it is formed at least as a substrate / metal sintering bonding plating film / metal sintering material layer / semiconductor element configuration, and it can be formed to have a metal sintering bonding plating film on the semiconductor element side as well. That is, as the configuration of the semiconductor mounting substrate of the present invention, it can be formed as a substrate / metal sintering bonding plating film / metal sintering material layer / metal sintering bonding plating film / semiconductor element configuration, and more specifically, it can be formed as a substrate / (A) layer / metal sintering material layer / (A) layer / semiconductor element configuration.
[0164] The semiconductor mounting substrate of the present invention has a metal sintering bonding coating film formed on the substrate, and semiconductor elements are bonded to the metal sintering bonding coating film via a metal sintering material layer. Therefore, it exhibits excellent heat resistance and resistance to thermal shock. Such a semiconductor mounting substrate of the present invention can be suitable for use as a next-generation power module capable of operating in high-temperature environments.
[0165] The metal sintering bonding coating of the present invention, due to its above-described structure, exhibits excellent heat resistance and resistance to thermal shock. Therefore, it can be suitably used for metal sintering bonding applications, and can also be used to form a bond between a substrate (e.g., an insulating heat-dissipating circuit board such as a DBC substrate or DBA substrate) and a substrate (e.g., a heat sink or heat fin). Examples of such a bond structure include a substrate (e.g., an insulating heat-dissipating circuit board such as a DBC substrate or DBA substrate) / metal sintering bonding coating / metal sintering material layer / metal sintering bonding coating / substrate (e.g., a heat sink or heat fin).
[0166] Example The present invention will be described in more detail below with examples and comparative examples. However, the present invention is not limited to the examples.
[0167] Furthermore, in all embodiments and comparative examples, a copper block material (30×30×3mm) was used as the substrate (the object to be plated). The substrate was subjected to degreasing and acid activation treatment, and pretreatment was performed by imparting a palladium catalyst.
[0168] (Example 1) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless silver plating film Formation of electroless nickel-phosphorus plating film The object to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the plating conditions described below, thereby forming an electroless nickel-phosphorus plating film on the object to be plated.
[0169] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 20g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0170] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 20 minutes Formation of electroless silver plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless silver plating solution prepared as described below under the plating conditions, thereby forming an electroless silver plating film on the electroless nickel-phosphorus plating film.
[0171] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0172] Conditions for electroless silver plating Liquid temperature: 60℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, on which an electroless nickel-phosphorus plating coating and an electroless silver plating coating are sequentially formed on the object to be plated.
[0173] • Electroless nickel-phosphorus plating film: phosphorus content 4% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless silver plating film: 0.2μm thick (Example 2) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless silver plating film By modifying the combination and plating conditions of the electroless nickel-phosphorus plating in Example 1 as follows, a metal sintering bonding plating film is manufactured on the object to be plated, on which the following electroless nickel-phosphorus plating film and electroless silver plating film are sequentially formed.
[0174] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0175] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless silver plating film: 0.2μm thick (Example 3) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless silver plating film By modifying the combination and plating conditions of the electroless nickel-phosphorus plating in Example 1 as follows, a metal sintering bonding plating film is manufactured on the object to be plated, on which the following electroless nickel-phosphorus plating film and electroless silver plating film are sequentially formed.
[0176] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 8g / L, glycine 20g / L, lead acetate 0.5mg / L, and other trace additives. The pH is then adjusted to 6.5 with sulfuric acid and ammonia.
[0177] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0001% by mass, thickness 4μm • Electroless silver plating film: 0.2μm thick (Example 4) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless silver plating film By modifying the combination and plating conditions of the electroless nickel-phosphorus plating in Example 1 as follows, a metal sintering bonding plating film is manufactured on the object to be plated, on which the following electroless nickel-phosphorus plating film and electroless silver plating film are sequentially formed.
[0178] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 8g / L, glycine 20g / L, lead acetate 0.5mg / L, and other trace additives. The pH is then adjusted to 6.5 with sulfuric acid and ammonia.
[0179] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 3.5 minutes • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0001% by mass, thickness 0.5μm • Electroless silver plating film: 0.2μm thick (Example 5) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless silver plating film By modifying the electroless silver plating process and plating conditions of Example 2 as follows, a metal sintering bonding plating film is manufactured on the object to be plated, on which the following electroless nickel-phosphorus plating film and electroless silver plating film are sequentially formed.
[0180] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0181] Conditions for electroless silver plating Liquid temperature: 60℃ Contact time with plating solution: 10 minutes • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless silver plating film: 0.1μm thickness (Example 6) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless gold plating film Formation of electroless nickel-phosphorus plating film The object to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the plating conditions described below, thereby forming an electroless nickel-phosphorus plating film on the object to be plated.
[0182] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 20g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0183] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 20 minutes Formation of electroless gold plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless gold plating solution prepared as described below under the plating conditions, thereby forming an electroless gold plating film on the electroless nickel-phosphorus plating film.
[0184] Electroless gold plating As a basic component, it is combined with 1.8 g / L potassium gold cyanide and 15 g / L sodium ethylenediaminetetraacetate, and other trace additives are added. The pH is then adjusted to 5.0 with sulfuric acid and ammonia.
[0185] Conditions for electroless gold plating Liquid temperature: 85℃ Contact time with plating solution: 10 minutes Through the above steps, a metal sintering bonding coating is manufactured, on which an electroless nickel-phosphorus plating coating and an electroless gold plating coating are sequentially formed on the object to be plated.
[0186] • Electroless nickel-phosphorus plating film: phosphorus content 4% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless gold plating film: 0.05μm thick (Example 7) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless gold plating film By modifying the combination and plating conditions of the electroless nickel-phosphorus plating in Example 6 as follows, a metal sintering bonding plating film is manufactured on the plated object having the following electroless nickel-phosphorus plating film and electroless gold plating film formed sequentially.
[0187] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0188] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless gold plating film: 0.05μm thick (Example 8) Plated object: Electroless nickel-phosphorus plating film; Electroless palladium plating film - Electroless silver plating membrane Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0189] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0190] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes Formation of electroless palladium plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless palladium plating solution prepared as described below under the following conditions, thereby forming an electroless palladium plating film on the electroless nickel-phosphorus plating film.
[0191] Electroless palladium plating As a basic component, it is combined with palladium chloride 1.5 g / L, sodium formate 10 g / L, ethylenediamine 15 g / L, and other trace additives. The pH is then adjusted to 6.0 with hydrochloric acid and ammonia.
[0192] Electroless palladium plating conditions Liquid temperature: 55℃ Contact time with plating solution: 10 minutes Formation of electroless silver plating film An electroless palladium plating film formed by the above-described operation is brought into contact with an electroless silver plating solution prepared as described below under the following conditions to form an electroless silver plating film on the electroless palladium plating film.
[0193] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0194] Conditions for electroless silver plating Liquid temperature: 70℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, on which the following electroless nickel-phosphorus plating coating, electroless palladium plating coating, and electroless silver plating coating are sequentially formed on the object to be plated.
[0195] • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless palladium plating film: 0.1μm thickness • Electroless silver plating film: 0.2μm thick (Example 9) Plated object: Electroless nickel-phosphorus plating; Electroless palladium plating; Electroless gold plating membrane Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0196] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0197] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes Formation of electroless palladium plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless palladium plating solution prepared as described below under the following conditions, thereby forming an electroless palladium plating film on the electroless nickel-phosphorus plating film.
[0198] Electroless palladium plating As a basic component, it is combined with palladium chloride 1.5 g / L, sodium formate 10 g / L, ethylenediamine 15 g / L, and other trace additives. The pH is then adjusted to 6.0 with hydrochloric acid and ammonia.
[0199] Electroless palladium plating conditions Liquid temperature: 55℃ Contact time with plating solution: 10 minutes Formation of electroless gold plating film An electroless palladium plating film formed by the above-described operation is brought into contact with an electroless gold plating solution prepared as described below under the following conditions to form an electroless gold plating film on the electroless palladium plating film.
[0200] Electroless gold plating As a basic component, it is combined with 1.8 g / L potassium gold cyanide and 15 g / L sodium ethylenediaminetetraacetate, and other trace additives are added. The pH is then adjusted to 5.0 with sulfuric acid and ammonia.
[0201] Conditions for electroless gold plating Liquid temperature: 90℃ Contact time with plating solution: 10 minutes Through the above steps, a metal sintering bonding coating is manufactured, in which the following electroless nickel-phosphorus plating coating, electroless palladium plating coating, and electroless gold plating coating are sequentially formed on the object to be plated.
[0202] • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless palladium plating film: 0.1μm thickness • Electroless gold plating film: 0.05μm thick (Example 10) Substrate to be plated: Electroless nickel-phosphorus plating film: Electroless palladium-phosphorus plating film: Electroless silver plating film Coated film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless Ni-P plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0203] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0204] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes Formation of electroless palladium-phosphorus plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless palladium-phosphorus plating solution prepared as described below under the following conditions, thereby forming an electroless palladium-phosphorus plating film on the electroless nickel-phosphorus plating film.
[0205] Electroless palladium-phosphorus plating As a basic component, it is combined with palladium chloride 1.5 g / L, sodium hypophosphite 10 g / L, and ethylenediamine 15 g / L. After adding other trace additives, the pH is adjusted to 6.0 with hydrochloric acid and ammonia.
[0206] Conditions for electroless palladium-phosphorus plating Liquid temperature: 60℃ Contact time with plating solution: 10 minutes Formation of electroless silver plating film An electroless palladium-phosphorus plating film formed by the above operation is brought into contact with an electroless silver plating solution prepared as described below under the following conditions to form an electroless silver plating film on the electroless palladium-phosphorus plating film.
[0207] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0208] Conditions for electroless silver plating Liquid temperature: 70℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, on which the following electroless nickel-phosphorus plating coating, electroless palladium-phosphorus plating coating, and electroless silver plating coating are sequentially formed on the object to be plated.
[0209] • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless palladium-phosphorus plating film: phosphorus content 1% by mass, thickness 0.1 μm • Electroless silver plating film: 0.2μm thick (Example 11) Substrate to be plated: Electroless nickel-phosphorus plating film: Electroless palladium-phosphorus plating film: Electroless gold plating film Coated film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless Ni-P plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0210] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0211] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes Formation of electroless palladium-phosphorus plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless palladium-phosphorus plating solution prepared as described below under the following conditions, thereby forming an electroless palladium-phosphorus plating film on the electroless nickel-phosphorus plating film.
[0212] Electroless palladium-phosphorus plating As a basic component, it is combined with palladium chloride 1.5 g / L, sodium hypophosphite 10 g / L, and ethylenediamine 15 g / L. After adding other trace additives, the pH is adjusted to 6.0 with hydrochloric acid and ammonia.
[0213] Conditions for electroless palladium-phosphorus plating Liquid temperature: 60℃ Contact time with plating solution: 10 minutes Formation of electroless gold plating film An electroless palladium-phosphorus plating film formed by the above operation is brought into contact with an electroless gold plating solution prepared as described below under the following conditions to form an electroless gold plating film on the electroless palladium-phosphorus plating film.
[0214] Electroless gold plating As a basic component, it is combined with 1.8 g / L potassium gold cyanide and 15 g / L sodium ethylenediaminetetraacetate, and other trace additives are added. The pH is then adjusted to 5.0 with sulfuric acid and ammonia.
[0215] Conditions for electroless gold plating Liquid temperature: 90℃ Contact time with plating solution: 10 minutes Through the above steps, a metal sintering bonding coating is manufactured on the object to be plated, in which the following electroless nickel-phosphorus plating coating, electroless palladium-phosphorus plating coating, and electroless gold plating coating are sequentially formed.
[0216] • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless palladium-phosphorus plating film: phosphorus content 1% by mass, thickness 0.1 μm • Electroless gold plating film: 0.05μm thick (Example 12) Plated object: Electroless nickel-phosphorus plating film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0217] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 20g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0218] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, which forms the following electroless nickel-phosphorus plating coating on the object to be plated.
[0219] • Electroless nickel-phosphorus plating film: phosphorus content 4% by mass, sulfur content 0.0003% by mass, thickness 4μm (Example 13) Plated object: Electroless nickel-phosphorus plating film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0220] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 10g / L, glycine 20g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 6.5 with sulfuric acid and ammonia.
[0221] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes Through the above steps, a metal sintering bonding coating is manufactured, which forms the following electroless nickel-phosphorus plating coating on the object to be plated.
[0222] • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0003% by mass, thickness 4μm (Example 14) Plated object: Electroless nickel-phosphorus plating film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0223] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 8g / L, glycine 20g / L, lead acetate 0.5mg / L, and other trace additives. The pH is then adjusted to 6.5 with sulfuric acid and ammonia.
[0224] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 25 minutes Through the above steps, a metal sintering bonding coating is manufactured, which forms the following electroless nickel-phosphorus plating coating on the object to be plated.
[0225] • Electroless nickel-phosphorus plating film: phosphorus content 2% by mass, sulfur content 0.0001% by mass, thickness 4μm (Comparative Example 1) Substrate to be plated: Electroless nickel-phosphorus plating film; Electroless silver plating film Formation of electroless nickel-phosphorus plating film The object to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the plating conditions described below, thereby forming an electroless nickel-phosphorus plating film on the object to be plated.
[0226] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 25g / L, malic acid 15g / L, lead acetate 0.5mg / L, and other trace additives. The pH is then adjusted to 4.5 with sulfuric acid and ammonia.
[0227] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 20 minutes Formation of electroless silver plating film An electroless nickel-phosphorus plating film formed on the substrate is brought into contact with an electroless silver plating solution prepared as described below under the plating conditions, thereby forming an electroless silver plating film on the electroless nickel-phosphorus plating film.
[0228] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0229] Conditions for electroless silver plating Liquid temperature: 60℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, on which an electroless nickel-phosphorus plating coating and an electroless silver plating coating are sequentially formed on the object to be plated.
[0230] • Electroless nickel-phosphorus plating film: phosphorus content 10% by mass, sulfur content 0.0001% by mass, thickness 4μm • Electroless silver plating film: 0.2μm thick (Comparative Example 2) Plated object: Electroless nickel-phosphorus plating film; Electroless silver plating film By changing the formulation and plating conditions of the electroless nickel-phosphorus plating in Comparative Example 1 as follows, a metal sintering bonding plating film is manufactured on the plated object having the following electroless nickel-phosphorus plating film and electroless silver plating film formed sequentially.
[0231] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 25g / L, malic acid 15g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 4.8 with sulfuric acid and ammonia.
[0232] Electroless nickel-phosphorus plating conditions Liquid temperature: 85℃ Contact time with plating solution: 20 minutes • Electroless nickel-phosphorus plating film: phosphorus content 7% by mass, sulfur content 0.0001% by mass, thickness 4μm • Electroless silver plating film: 0.2μm thick (Comparative Example 3) Plated object: Electroless nickel-phosphorus plating film; Electroless silver plating film By changing the formulation and plating conditions of the electroless nickel-phosphorus plating in Comparative Example 1 as follows, a metal sintering bonding plating film is manufactured in which the following electroless nickel-phosphorus plating film and electroless silver plating film are sequentially formed on the plated object.
[0233] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 25g / L, malic acid 15g / L, lead acetate 0.5mg / L, thiourea 0.2mg / L, and other trace additives. The pH is then adjusted to 4.5 with sulfuric acid and ammonia.
[0234] Electroless nickel-phosphorus plating conditions Liquid temperature: 85℃ Contact time with plating solution: 20 minutes • Electroless nickel-phosphorus plating film: phosphorus content 7% by mass, sulfur content 0.0003% by mass, thickness 4μm • Electroless silver plating film: 0.2μm thick (Comparative Example 4) Plated object: Electroless silver plating film Formation of electroless silver plating film The object to be plated is brought into contact with the electroless silver plating solution described below under the plating conditions described below, thereby forming an electroless silver plating film on the object to be plated.
[0235] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0236] Conditions for electroless silver plating Liquid temperature: 60℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating film is manufactured, which forms the following electroless silver plating film on the object to be plated.
[0237] • Electroless silver plating film: 0.2μm thick (Comparative Example 5) Plated object: Electroless silver plating film Formation of electroless silver plating film The object to be plated is brought into contact with the electroless silver plating solution described below under the plating conditions described below, thereby forming an electroless silver plating film on the object to be plated.
[0238] Electroless silver plating As a basic component, it is combined with 1.7 g / L silver nitrate, 1.5 g / L water-soluble hydrazine derivative, 20 g / L 1-methylhydantoin, and 0.5 mg / L lead acetate. After adding other trace additives, the pH is adjusted to 10 with nitric acid and sodium hydroxide.
[0239] Conditions for electroless silver plating Liquid temperature: 70℃ Contact time with plating solution: 40 minutes Through the above steps, a metal sintering bonding coating film is manufactured, which forms the following electroless silver plating film on the object to be plated.
[0240] • Electroless silver plating film: 1.0μm thick (Comparative Example 6) Plated object: Electroless nickel-phosphorus plating film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0241] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 25g / L, malic acid 15g / L, lead acetate 0.5mg / L, and other trace additives. The pH is then adjusted to 4.5 with sulfuric acid and ammonia.
[0242] Electroless nickel-phosphorus plating conditions Liquid temperature: 90℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, which forms the following electroless nickel-phosphorus plating coating on the object to be plated.
[0243] • Electroless nickel-phosphorus plating film: phosphorus content 10% by mass, sulfur content 0.0001% by mass, thickness 4μm (Comparative Example 7) Plated object: Electroless nickel-phosphorus plating film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0244] Electroless nickel-phosphorus plating combination As the basic components, in combination with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 25g / L, malic acid 15g / L, lead acetate 0.5mg / L, thiourea 0.1mg / L, and other trace additives, the pH is adjusted to 4.8 with sulfuric acid and ammonia.
[0245] Electroless nickel-phosphorus plating conditions Liquid temperature: 85℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, which forms the following electroless nickel-phosphorus plating coating on the object to be plated.
[0246] • Electroless nickel-phosphorus plating film: phosphorus content 7% by mass, sulfur content 0.0001% by mass, thickness 4μm (Comparative Example 8) Plated object: Electroless nickel-phosphorus plating film Formation of electroless nickel-phosphorus plating film The substrate to be plated is brought into contact with the electroless nickel-phosphorus plating solution described below under the following conditions to form an electroless nickel-phosphorus plating film on the substrate.
[0247] Electroless nickel-phosphorus plating combination As a basic component, it is combined with nickel sulfate•6H2O 22.5g / L, sodium hypophosphite 25g / L, malic acid 15g / L, lead acetate 0.5mg / L, thiourea 0.2mg / L, and other trace additives. The pH is then adjusted to 4.5 with sulfuric acid and ammonia.
[0248] Electroless nickel-phosphorus plating conditions Liquid temperature: 85℃ Contact time with plating solution: 20 minutes Through the above steps, a metal sintering bonding coating is manufactured, which forms the following electroless nickel-phosphorus plating coating on the object to be plated.
[0249] • Electroless nickel-phosphorus plating film: phosphorus content 7% by mass, sulfur content 0.0003% by mass, thickness 4μm (Comparative Example 9) The object being plated (copper block material) (Evaluation Method) The following evaluation was performed on the embodiments and comparative examples.
[0250] Sample preparation for determining the bond strength of silver sintered joints In the various embodiments and comparative examples, the metal sintering bonding coatings manufactured were used to mount semiconductor devices using a silver sintering material. Specifically, a paste material containing micron-sized silver flakes (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd.) and an ether solvent (manufactured by DAICL Co., Ltd.) was used as the silver sintering material. A SiC dummy chip (3mm × 3mm × 1mm) with a titanium / silver sputtered film (0.1μm / 1.0μm) was used as the semiconductor device. Evaluation samples of the silver sintering bonding were prepared by bonding the metal sintering bonding coating formed on the substrate to the SiC dummy chip with the titanium / silver sputtered film using the silver sintering material. Furthermore, the bonding conditions for Examples 1-11 and Comparative Examples 1-5 were set to no pressure, atmospheric environment, 250°C, and 30 minutes; the bonding conditions for Examples 12-14 and Comparative Examples 6-9 were set to 1MPa pressure, atmospheric environment, 250°C, and 30 minutes.
[0251] Bond strength measurement For the aforementioned evaluation specimens, shear tests were conducted using a weld strength tester (Nordson DAGE 4000Plus) to determine the bond strength between the metal sintering coating and the silver sintered material. Shear tests were performed immediately after silver sintering and after heat treatment at 300°C for 500 hours. Initial bond strength and bond strength after heat treatment were evaluated according to the following evaluation criteria.
[0252] Above 30MPa: Good bonding strength Below 30 MPa: Insufficient bond strength The results are shown in Table 1.
[0253] [Table 1] According to the results in Table 1, in Examples 1 to 14, the initial bonding and the bonding after heat treatment are excellent. Even if heat treatment is performed, the bonding strength will not decrease drastically. Therefore, the heat resistance and thermal shock resistance are excellent, forming a coating film suitable for metal sintering bonding applications.
[0254] In contrast, in Comparative Examples 1-9, the bonding strength after heat treatment was significantly reduced compared to the initial bonding strength, and the heat resistance and thermal shock resistance were poor compared to Examples 1-14.
Claims
1. A coating film for metal sintering bonding, characterized in that: It is a metal sintering bonding coating having an electroless nickel-phosphorus plating film (A), wherein the phosphorus content of the electroless nickel-phosphorus plating film (A) is 4% by mass or less when the electroless nickel-phosphorus plating film is set to 100% by mass.
2. The coating film for metal sintering as described in claim 1, characterized in that: The sulfur content of the electroless nickel-phosphorus plating film (A) is less than 0.0005% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.
3. The coating film for metal sintering as described in claim 1, characterized in that: The sulfur content of the electroless nickel-phosphorus plating film (A) is less than 0.0001% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.
4. The coating film for metal sintering as described in claim 1, characterized in that: The thickness of the electroless nickel-phosphorus plating film (A) is less than 0.1 to 20 μm.
5. The coating film for metal sintering bonding as described in claim 1, characterized in that: The (A) electroless nickel-phosphorus plating film also has (B) an electroless silver plating film or an electroless gold plating film.
6. The coating film for metal sintering as described in claim 5, characterized in that: The thickness of the electroless silver-plated film or the electroless gold-plated film (B) is 0.02 to 2 μm.
7. The coating film for metal sintering as described in claim 5, characterized in that: Between the (A) electroless nickel-phosphorus plating film and the (B) electroless silver plating film or electroless gold plating film, there is also a (C) barrier metal layer.
8. The coating film for metal sintering as described in claim 7, characterized in that: The barrier metal layer (C) is an electroless palladium-plated film or an electroless palladium-phosphorus-plated film.
9. The coating film for metal sintering as described in claim 1, characterized in that: Used for sintered metal materials containing silver and / or copper.
10. A method for manufacturing a plating film for metal sintering bonding, comprising forming a plating film for metal sintering bonding on a substrate, characterized in that: Step 1 comprises: (1) contacting an electroless nickel-phosphorus plating solution with the surface of a substrate to form an (A) electroless nickel-phosphorus plating film on the substrate. The phosphorus content of the electroless nickel-phosphorus plating film (A) is less than 4% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.
11. The manufacturing method as described in claim 10, characterized in that: It also includes step 2, which involves bringing an electroless silver plating solution or an electroless gold plating solution into contact with the surface of the electroless nickel-phosphorus plating film to form an electroless silver plating film or an electroless gold plating film on the (A) electroless nickel-phosphorus plating film.
12. A semiconductor mounting substrate, characterized in that: A metal sintering bonding coating having an electroless nickel-phosphorus plating film (A) is laminated on the substrate. A semiconductor element is formed on the metal sintering bonding film via a metal sintering material layer. The phosphorus content of the electroless nickel-phosphorus plating film (A) is less than 4% by mass when the electroless nickel-phosphorus plating film is set to 100% by mass.