Nickel sulfide selenide cocatalyst, photocatalyst and preparation method and application of nickel sulfide selenide cocatalyst and photocatalyst

By introducing nickel sulfide selenide cocatalyst into the NiS2 structure to form a substitution solid solution NiSexS2-x, and then loading it onto carbon nitride material, the problem of photocatalyst detachment was solved, and the efficiency and stability of photocatalytic water splitting for hydrogen production were improved.

CN122032592APending Publication Date: 2026-05-15XI'AN PETROLEUM UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610265458.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-05
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

In the process of photocatalytic water splitting to produce hydrogen, the shedding of the co-catalyst limits the stability of the composite material and affects the hydrogen production efficiency.

Method used

By introducing nickel sulfide selenide cocatalyst into the NiS2 structure, a substitutional solid solution NiSexS2-x is formed, in which Se atoms replace S atoms at the atomic level, forming a single-phase, uniform crystal structure. This structure is then loaded onto carbon nitride materials to form a composite material.

Benefits of technology

This improved the structural stability and hydrogen production kinetics of the photocatalyst, reduced the hydrogen production overpotential, enhanced the material's resistance to photocorrosion and electron transfer rate, and improved the stability and hydrogen production efficiency of the photocatalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122032592A_ABST
    Figure CN122032592A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of photocatalysts, and particularly relates to a sulfur nickel selenide cocatalyst, a photocatalyst and a preparation method and application of the sulfur nickel selenide cocatalyst, and the preparation method of the sulfur nickel selenide cocatalyst comprises the steps that a soluble nickel source, a soluble sulfur source and a soluble selenium source are dispersed in an alcohol solvent to be mixed, a reaction is conducted for 10-20 h at the temperature of 160-200 DEG C, and the sulfur nickel selenide is obtained after washing and drying; the molar ratio of the soluble nickel source to the soluble sulfur source to the soluble selenium source is 1: (0.5-1.5): (0.5-1.5). In the cocatalyst, Se is introduced into a NiS2 structure, lattice spacing is increased, a replacement solid solution NiSexS2-x is formed, in the solid solution, Se atoms replace S atoms in an atomic level and enter NiS2 lattices instead of being simply attached to the surface of NiS2 or forming heterojunctions, a single-phase and uniform crystal structure is formed instead of physically mixed two phases, and the structure is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalyst technology, specifically relating to a nickel sulfide selenide cocatalyst, a photocatalyst, its preparation method, and its application. Background Technology

[0002] Hydrogen energy, as a clean and high-energy-density secondary energy source, is considered an important pathway to alleviate the depletion of fossil fuels and the pressure on the ecological environment. Solar-driven photocatalytic water splitting provides a sustainable and green technological solution for hydrogen production. To promote the implementation of the "dual-carbon" strategy, constructing a high-performance hydrogen production catalytic system is particularly crucial. Among these efforts, improving the activity and synergistic effect of catalyst promoters has become an effective strategy for enhancing the efficiency of photocatalytic hydrogen production.

[0003] In recent years, transition metal chalcogenides have been widely used in supercapacitors, batteries, and electrocatalysts due to their superior electron-trapping capabilities. Compared with their corresponding sulfides, transition metal selenides possess similar structures and higher electrical conductivity. Studies have found that the Se-H bond energy is closer to the Pt-H bond energy (251 kJ·mol⁻¹) than the SH bond energy. -1 The presence of selenium atoms indicates that they are superior H2 desorption sites. The rational construction of nickel sulfide rich in Se atoms is an effective pathway to improve the hydrogen production activity of nickel-based co-catalysts; however, the shedding of the co-catalyst during the photocatalytic reaction limits the stability of the composite material. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a nickel sulfide selenide co-catalyst, a photocatalyst, its preparation method, and its application.

[0005] A method for preparing a nickel sulfoselenide co-catalyst includes the following steps: dispersing a soluble nickel source, a soluble sulfur source and a soluble selenium source in ethylene glycol, reacting at 160~200℃ for 10~20h, washing, and drying to obtain the nickel sulfoselenide; The molar ratio of the soluble nickel source, soluble sulfur source, and soluble selenium source is 1:0.5~1.5:0.5~1.5.

[0006] In this invention, the nickel sulfide selenide co-catalyst Se is introduced into the NiS2 structure, increasing the lattice spacing and forming a substitutional solid solution NiSe. x S 2-x In the solid solution, Se atoms do not simply attach to the surface of NiS2 or form a heterojunction, but rather replace S atoms at the atomic level and enter the NiS2 lattice, forming a single-phase, homogeneous crystal structure, rather than a physically mixed two-phase structure, which is structurally stable.

[0007] Preferably, the soluble nickel source is selected from any one of nickel chloride, nickel nitrate, and nickel acetate; The soluble sulfur source is thiourea; The soluble selenium source is sodium selenite.

[0008] A nickel sulfoselenide cocatalyst prepared by the method described above.

[0009] A nickel sulfide selenide photocatalyst is a composite material in which nickel sulfide selenide cocatalyst is supported on carbon nitride material; The content of nickel sulfide selenide in the composite material is 10~25wt%, and the content of carbon nitride material is 75~90wt%.

[0010] Preferably, the carbon nitride material is carbon nitride nanosheets.

[0011] Preferably, the preparation method of the nickel sulfose selenide photocatalyst includes the following steps: adding the nickel sulfose selenide and the carbon nitride material into a solvent and reacting for 30 min to 60 min, then evaporating to dryness at 60 °C to 80 °C to obtain the nickel sulfose selenide photocatalyst; The solvent is anhydrous ethanol or water; The mass ratio of nickel sulfide selenide to carbon nitride is such that the content of nickel sulfide selenide in the composite material is 10~25wt%, and the content of carbon nitride is 75~90wt%.

[0012] Preferably, the preparation method of the nickel sulfoselenide photocatalyst includes the following steps: dispersing a soluble nickel source, a soluble sulfur source, a soluble selenium source and carbon nitride material in ethylene glycol, reacting at 160~200℃ for 10~20h, washing, and drying to obtain the nickel sulfoselenide photocatalyst; The mass ratio of soluble nickel source, soluble sulfur source, soluble selenium source and carbon nitride material is 18~50:8~27:6~20:100.

[0013] The application of the nickel sulfide selenide photocatalyst in photocatalytic water splitting for hydrogen production.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: In this invention, the nickel sulfide selenide co-catalyst Se is introduced into the NiS2 structure, increasing the lattice spacing and forming a substitutional solid solution NiSe. x S 2-x In the solid solution, Se atoms do not simply attach to the surface of NiS2 or form a heterojunction, but rather replace S atoms at the atomic level and enter the NiS2 lattice, forming a single-phase, homogeneous crystal structure, rather than a physically mixed two-phase structure. This structure is stable, can quickly transfer photogenerated electrons, reduce the hydrogen production overpotential, and improve the surface hydrogen production kinetics.

[0015] Furthermore, the radius of a Se atom is larger than that of a S atom. The introduction of a small number of Se atoms increases the lattice spacing. The uniformly expanded lattice of the solid solution acts like a "buffer pad" to prevent microcracks, defect aggregation, or structural collapse caused by stress concentration, thereby improving structural durability.

[0016] After the formation of the NiSexS2-x solid solution, the introduction of Se alters the local electronic structure and chemical bonding environment. The strength of the Se-S bond differs from that of the SS bond, and Se has lower electronegativity, which may make the material surface more resistant to photocorrosion. Attached Figure Description

[0017] Figure 1 NiSe x S 2-x The characterization results are shown in (a) XRD patterns of samples with different Se:S ratios and (b) partially magnified XRD patterns.

[0018] Figure 2 NiSe 0.5 S 1.5 Schematic diagram of in-situ solvothermal preparation process.

[0019] Figure 3 This is the XRD pattern of the composite material.

[0020] Figure 4 The images show scanned images of the composite materials: (a) is a SEM image of CNNs, and (b) is a NiSe image. 0.5 S 1.5 SEM images, (c) showing NiSe 0.5 S 1.5 SEM images of / CNNs(insitu), (d) is the elemental distribution map, (e) is the NiSe map. 0.5 S 1.5 / CNNs(insitu) TEM, (fg) is HR-TEM.

[0021] Figure 5 The images show the XPS high-resolution spectra of the composite materials: (a) C1s, (b) N1s, (c) Ni2p, (d) S2p, and (e) Se3d.

[0022] Figure 6 The graphs show the photocatalytic hydrogen production performance of the composite materials. (a) shows the CNNs loaded on different samples, and (b) shows the NiSe ratios at different percentages. 0.5 S 1.5 / CNNs, (c) is NiSe 0.5 S 1.5 / CNNs loop experiment.

[0023] Figure 7 The results show the photocatalytic hydrogen production activity of the composite material, (a) for NiSe.0.5 S 1.5 / CNNs(insitu) hydrogen production rate plot, (b) is 20% NiSe 0.5 S 1.5 / CNNs(insitu) loop experiment.

[0024] Figure 8 The results show the photoelectric properties of the composite material. (a) is the transient photocurrent response diagram, (b) is the LSV curve, (c) is the electrochemical impedance diagram, and (d) is the photoluminescence spectrum.

[0025] Figure 9 The results show the intrinsic active specific surface area of ​​the composite material. (a) is the CV curve of CNNs, and (b) is the NiSe. 0.5 S 1.5 The CV curves, (c) are for NiSe. 0.5 S 1.5 The CV curves of / CNNs, (d) is the fitted curve of current density versus scan rate.

[0026] Figure 10 The results of the study on the photocatalytic activity enhancement mechanism of composite materials are as follows: (a) UV-Vis diffuse reflectance absorption spectrum, (b) Taco curve of CNNs, (c) Mott-Schottky curve of CNNs, and (d) NiSe. 0.5 S 1.5 The Mott-Schottky curve, (e) is the NiSe 0.5 S 1.5 VB-XPS.

[0027] Figure 11 NiSe 0.5 S 1.5 / Schematic diagram of the photocatalytic hydrogen production mechanism of CNNs. Detailed Implementation

[0028] The specific embodiments of the present invention are described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention. Unless otherwise specified, the experimental methods described in the embodiments of the present invention are conventional methods.

[0029] Catalyst preparation (1) Preparation of carbon nitride nanosheets A process combining microwave-assisted thermal polymerization and ultrasonic exfoliation was employed. The specific steps were as follows: using urea, dicyandiamide, or melamine as precursors, the precursors were placed in a crucible, wrapped in tin foil, and then placed in a microwave muffle furnace. The temperature was programmed to rise to 520-580℃ at a rate of 4-7℃ / min under air atmosphere, and held at this temperature for 2.5-3.5 hours for thermal polymerization. After the reaction, the resulting product was ground into powder particles, then ultrasonically dispersed and dried to finally obtain layered exfoliated g-C3N4 nanosheets.

[0030] (2) NiSe x S 2-x Catalyst preparation NiSe was prepared by in-situ solvothermal method. x S 2-x The nanospheres were prepared as follows: 1 mmol of Ni(Cl)₂·6H₂O was dissolved in 60 mL of ethylene glycol. Then, 1.5 mmol of thiourea and 0.5 mmol of sodium selenite were added as sulfur and selenium sources, respectively. After stirring thoroughly, the mixture was reacted at 180 °C for 18 h. The sample was repeatedly washed with anhydrous ethanol and distilled water, and dried to obtain the final sample. Based on the amount of Se and S in the feed, the sample was named NiSe. 0.5 S 1.5 .

[0031] A series of NiSe were synthesized by changing the molar ratio of Se and S (0:2, 0.5:1.5, 1:1, 1.5:0.5, 2:0). x S 2-x product.

[0032] NiSe 0.5 S 1.5 A schematic diagram of the in-situ solvothermal preparation process is shown below. Figure 2 .

[0033] (3) Preparation of composite materials NiSe was prepared by solvent evaporation. x S 2-x / CNNs composite materials. A certain amount of NiSe was added to 20 mL of anhydrous ethanol. x S 2-x The mixture was sonicated with g-C3N4 for 30 min. Subsequently, the suspension was placed in a water bath and stirred at 70°C to evaporate the solvent. Based on a total composite material mass of 100 mg, 10, 15, 20, and 25 mg of NiSe were weighed out respectively. x S2₋ x The corresponding masses of g-C3N4 (90, 85, 80, and 75 mg, respectively) were added to 20 mL of anhydrous ethanol, ultrasonically dispersed for 30 min, and then the solvent was evaporated by stirring in a 70 °C water bath to obtain different NiSe. xS2₋ x NiSe loading x S2₋ x / CNNs composite materials. The prepared composite materials were labeled as γ-NiSe. x S 2-x / CNNs. (y=10%, 15%, 20%, and 25%, where y represents NiSe) x S 2-x (percentage of quality).

[0034] NiSe was prepared by in-situ solvothermal method 0.5 S 1.5 / CNNs (insitu) composite materials, as detailed below: 1) Dissolve 100 mg of g-C3N4 in 60 mL of ethylene glycol. After ultrasonication and stirring to ensure homogeneity, add 18.1 mg of NiCl2·6H2O, 8.68 mg of thiourea, and 6.57 mg of sodium selenite sequentially. React at 180 °C for 18 hours. The product obtained is named 10%-NiSe. 0.5 S 1.5 / g-C3N4.

[0035] 2) 100 mg of g-C3N4 was dissolved in 60 mL of ethylene glycol. After ultrasonication and stirring to ensure homogeneity, 28.7 mg of NiCl2·6H2O, 13.78 mg of thiourea, and 10.44 mg of sodium selenite were added sequentially. The reaction was carried out at 180 °C for 18 hours. The product was named 15%-NiSe. 0.5 S 1.5 / g-C3N4.

[0036] 3) Dissolve 100 mg of g-C3N4 in 60 mL of ethylene glycol, and mix thoroughly by sonication and stirring. Then, add 40.7 mg of NiCl2·6H2O, 19.55 mg of thiourea, and 14.80 mg of sodium selenite sequentially. React at 180 °C for 18 hours. The product obtained is named 20%-NiSe. 0.5 S 1.5 / g-C3N4.

[0037] 4) Dissolve 100 mg of g-C3N4 in 60 mL of ethylene glycol. After ultrasonication and stirring to ensure homogeneity, add 54.20 mg of NiCl2·6H2O, 26.03 mg of thiourea, and 19.72 mg of sodium selenite sequentially. React at 180 °C for 18 hours. The product obtained is named 25%-NiSe. 0.5 S 1.5 / g-C3N4.

[0038] result 1. NiSe x S 2-x The effect of Se:S ratio on the products First, we studied NiSe under different Se:S ratios. x S 2-x The product of. For example... Figure 1 As shown, without the addition of an S source, the XRD diffraction peaks correspond to the standard card of NiSe2 (JCPDS: 88-1711), with the peaks at 29.9°, 33.6°, 36.9°, and 50.7° corresponding to the (200), (210), (211), and (311) crystal planes of NiSe2, respectively. The product generated without the addition of a Se source corresponds to the XRD diffraction peaks of α-phase NiS (JCPDS: 02-1280). When both Se and S sources are added simultaneously, the XRD diffraction peaks are located between NiSe2 and NiS2. As the Se:S ratio increases, the peak position gradually shifts to the left, as seen in the magnified XRD pattern. This indicates that Se, with its larger atomic radius, was successfully introduced into the NiS2 structure, increasing the lattice spacing and forming a substitutional solid solution, NiSe. x S 2-x These results demonstrate that adjusting the Se and S ratio can effectively control the NiSe content. x S 2-x The structural characteristics provide a foundation for further optimization of photocatalytic performance.

[0039] Furthermore, under these reaction conditions, nickel sulfide exhibits selective growth of the α-phase NiS, while the formation of nickel selenide is strictly dependent on the feed ratio. Specifically, when the Ni:Se ratio is 1:1, the product selectively grows into NiSe, while at a Ni:Se ratio of 1:2, it tends to grow into NiSe2 crystals with a pyrite structure. Adding a large amount of S source along with a small amount of Se source significantly affects the product's composition, with the actual product being NiSe with a predominantly pyrite structure of NiS2. x S 2-x Solid solution. When the Se:S ratio is 1:1, its structure begins to exhibit a NiSe structure that is more predominantly NiSe2. x S 2-x Solid solution. When the Se:S ratio in the feed reaches 1.5:0.5, the relatively small amount of S atoms affects the crystal phase structure of the product. The XRD pattern shows phases attributable to elemental Se and Ni, respectively. 0.85 The characteristic peak of Se.

[0040] 2. NiSe 0.5 S 1.5 Microstructure and Composition of CNNs Figure 3 NiSe was prepared by solvent evaporation and in-situ solvothermal methods, respectively.0.5 S 1.5 XRD patterns of the CNNs composite material and the CNNs themselves. The CNNs exhibited diffraction characteristic peaks at 13.0° and 27.8° corresponding to the (100) and (002) crystal planes, respectively, with the 27.8° diffraction peak related to interlayer stacking. In NiSe... 0.5 S 1.5 In the XRD of the CNNs composite material, NiSe and its components can be observed simultaneously. 0.5 S 1.5 The characteristic peaks of NiSe and CNNs. Among them, the characteristic peaks belonging to the (002) crystal plane of CNNs have shifted slightly to the left, indicating that NiSe 0.5 S 1.5 It was successfully applied to CNNs and affected the inter-layer structure of CNNs. NiSe... 0.5 S 1.5 In the XRD analysis of the in-situ NiSe / CNNs composite material, the (002) crystal plane of the CNNs did not shift, indicating that the structure of the CNNs remained almost unchanged during in-situ growth. Two sets of NiSe samples obtained using different methods... 0.5 S 1.5 / CNNs Composites contains information about NiSe 0.5 S 1.5 The diffraction peak positions did not shift, which further proves that the solid solution product is controlled by the Se:S ratio, i.e., NiSe. x S 2-x The generation is controllable, and CNNs do not affect NiSe during in-situ growth. 0.5 S 1.5 The structure is affected. Furthermore, the in-situ grown NiSe... 0.5 S 1.5 The larger full width at half maximum (FWHM) indicates that the in-situ addition of CNNs will improve NiSe. 0.5 S 1.5 Insufficient grain growth in NiSe may be due to... 0.5 S 1.5 The growth of CNNs is limited by their size. Fourier transform infrared (FT-IR) spectroscopy was used to analyze pure CNNs and NiSe. 0.5 S 1.5 / CNNs and NiSe 0.5 S 1.5 The surface functional groups of the CNNs (insitu) composite material were analyzed. CNNs were analyzed at 810 cm⁻¹. -1 The absorption peak at 1200-1700 cm⁻¹ is related to the triazine units in the CNNs sample. -1 The absorption peaks between 2900-3400 cm⁻¹ are correlated with C=N single bonds and C=N double bonds. -1The absorption peak at the NiSe content originates from the NH stretching vibrations on the surface of the CNNs. The absorption peak positions of the composites prepared by both methods did not change significantly compared to pure CNNs, indicating that the surface functional groups of the CNNs were not affected by NiSe. 0.5 S 1.5 The load changes.

[0041] SEM and TEM images ( Figure 4 This indicates that pure CNNs exhibit smooth, two-dimensional ultrathin nanosheets, while NiSe... 0.5 S 1.5 The monomers exhibit spherical structures with a diameter of approximately 200 nm. After in-situ recombination, it is clearly observed that the surface of the CNNs is no longer smooth, and some NiSe... 0.5 S 1.5 The constraints of CNNs result in smaller crystal sizes that are fixed on the surface and between layers of the CNNs. Generally, the nucleation rate and growth rate of a crystal determine the morphology, size, and dispersion of the particles; a higher nucleation rate leads to smaller and more uniform particle sizes. NiSe grown in situ on CNNs... 0.5 S 1.5 Obtained a higher purity than monomer NiSe 0.5 S 1.5 Smaller particle size and more uniform dispersion. The elemental distribution map shows a uniform distribution of C, N, Ni, S, and Se, further confirming NiSe. 0.5 S 1.5 Successful synthesis of / CNNs (insitu). NiSe in the composite material was measured using HR-TEM. 0.5 S 1.5 lattice stripes ( Figure 4 fg). NiSe with larger dimensions 0.5 S 1.5 The exposed lattice spacing of the nanospheres corresponds to NiSe. 0.5 S 1.5 The (210) and (211) crystal planes, while NiSe grown on smaller-sized CNNs. 0.5 S 1.5 The exposed lattice spacing corresponds to the (111) and (200) crystal planes. This indicates that during in-situ growth, CNNs exhibit size effects on NiSe. 0.5 S 1.5 The microstructure of NiSe was affected, and it also affected the microstructure of NiSe. 0.5 S 1.5 The exposed crystal planes also changed.

[0042] NiSe prepared by XPS analysis 0.5 S 1.5The surface elemental composition and chemical state of / CNNs (insitu) are as follows: Figure 5 The C1s peak (284.8 eV) was used as a reference for calibration. Figure 5 a represents the C1s spectrum, with the fitted peaks at 284.8 eV and 288.3 eV corresponding to C atoms in the C-C and NC=N bonds, respectively. Based on the peak height and area, it can be seen that the proportion of NC=N bonds in the composite material increases compared to pure CNNs. This may be because the solvothermal process provides favorable conditions for CNN growth, helping to elongate the basic units of CNNs, resulting in more triazine ring structures and a larger specific surface area, thus allowing for the absorption of more NiSe. 0.5 S 1.5 Loaded onto CNNs. The fitted peaks at 398.6 eV, 400.2 eV, and 401.2 eV in the N1s spectrum belong to N atoms in bicoordinate (C=NC), tricoordinate (N-C3), and free -NHx groups, respectively. Similar to the C1s spectrum, a higher proportion of bicoordinate C=NC bonds can be observed in the N1s spectrum, further confirming that CNNs underwent regrowth in ethylene glycol solvent. Additionally, NiSe was also observed. 0.5 S 1.5 In CNNs (insitu), the binding energy of C1s and N1s does not have in-situ solvothermal activity or NiSe. 0.5 S 1.5 The change is due to the load, indicating that small-sized NiSe 0.5 S 1.5 It does not significantly affect the growth of CNNs; on the contrary, CNNs limit NiSe. 0.5 S 1.5 The morphology is consistent with the results obtained from XRD.

[0043] Figure 5 The fitted peak at 853.2 eV in the c spectrum belongs to Ni in the Ni-S bond. The fitted peak around 856.8 eV is related to Ni atoms in the Ni-SOx bond. The tailed peak with a large half-broadening near 862 eV is a satellite peak of Ni atoms, and the remaining peaks above 870 eV belong to the 2p1 / 2 orbital of Ni, all corresponding to the Ni 2p3 / 2 peak in the fitted spectrum. In the S2p spectrum, a set of signal peaks fitted near 160.0 eV is related to the 3p orbital of Se, a set of signals at 162.0 eV is related to metal sulfides corresponding to the Ni-S bond, the peak at 165.0 eV belongs to unsaturated S, and the appearance of the signal peak at 168.0 eV indicates the presence of oxidized sulfur on the sample surface. Figure 5e represents the Se 3d spectrum. The peaks at 54.6 eV belong to the Se atoms in the Ni-Se bond, while the signal peak at 58.8 eV belongs to the oxidized Ni-SeO. x Se atoms in the species. Comparison of monomer and composite material NiSe. 0.5 S 1.5 / CNNs (insitu) Ni2p, S2p, and Se3d clearly show that in NiSe 0.5 S 1.5 The signals in / CNNs (insitu) are all shifted towards lower binding energies, indicating that NiSe 0.5 S 1.5 The close contact formed on CNNs and the environment that provides greater electron density are beneficial to NiSe. 0.5 S 1.5 Electron collection, and in-situ grown NiSe 0.5 S 1.5 Nanoparticles did not significantly affect the chemical environment and chemical state of CNNs. In summary, in NiSe... 0.5 S 1.5 After in-situ composite with CNNs, the CNNs underwent secondary growth after solvothermal treatment, resulting in the addition of more triazine ring units. Meanwhile, NiSe... 0.5 S 1.5 During in-situ growth, the limitations imposed by the layered structure of CNNs resulted in smaller growth sizes, which were then uniformly dispersed between and on the surfaces of the CNNs, leading to significant changes in morphology. NiSe 0.5 S 1.5 The increased electron density in the chemical environment of nanoparticles makes them more likely to gain electrons. The morphology, structure, and chemical environment of CNNs were not affected by NiSe. 0.5 S 1.5 The load changes accordingly. This indicates that the two have formed a closer contact and maintained the original characteristics of CNNs, providing a good foundation for further applications.

[0044] 3. NiSe 0.5 S 1.5 Study on photocatalytic hydrogen production performance of CNNs Using 20 vol.% TEOA as the reaction solvent, the effects of different Se:S ratios on the prepared NiSe were first investigated. x S 2-x The effect of co-catalysts on the photocatalytic hydrogen production performance of CNNs. For example... Figure 6 a. After loading a co-catalyst, the hydrogen production rate of CNNs was improved to some extent. Among them, the photocatalytic hydrogen production efficiency of samples loaded with pure NiS and NiSe2 was significantly lower than that of samples loaded with NiSe2. x S2-x Solid solution samples. Experimental comparisons were conducted on NiSe with a Se:S ratio of 0.5:1.5. 0.5 S 1.5 NiSe exhibits the best co-catalytic effect. Therefore, NiSe was selected. 0.5 S 1.5 A more detailed study was conducted, and after loading with different concentration gradients, it was found that NiSe at a loading of 20%... 0.5 S 1.5 / CNNs exhibited the best photocatalytic hydrogen production activity. However, after five cycles, their hydrogen production efficiency decreased significantly, which is due to the degradation of NiSe. 0.5 S 1.5 The nanospheres are large in size and the connection formed by physical composite with CNNs is not tight enough. They fall off during hydrogen production, causing a rapid decrease in photocatalytic activity.

[0045] Therefore, in order to slow down NiSe 0.5 S 1.5 To facilitate catalyst release and improve photocatalyst stability, in-situ solvothermal evaporation was used to prepare NiSe with tighter linkages. 0.5 S 1.5 / CNNs(insitu) samples. Comparison revealed that the in-situ prepared composite material exhibited superior photocatalytic hydrogen production activity. Figure 7 ), 20%-NiSe 0.5 S 1.5 / CNNs(insitu) exhibited the most superior photocatalytic hydrogen production activity, reaching 19569.04 μmol·g. -1 ·h -1 After five cycles of experiments, the hydrogen production showed almost no significant decrease, indicating that the in-situ synthesis method effectively improved the photocatalytic performance and stability of the composite material.

[0046] 4. NiSe 0.5 S 1.5 / CNNs photoelectric performance research exist Figure 8 In a, NiSe 0.5 S 1.5 / CNNs (insitu) exhibit a higher dark current density under no-light conditions than pure CNNs, indicating better conductivity. Under illumination, NiSe... 0.5 S 1.5 The change in transient photocurrent density of / CNNs (insitu) is similar to that of pure CNNs, indicating that NiSe 0.5 S 1.5 / CNNs (insitu) do not increase the number of photogenerated carriers in CNNs. Furthermore, it is clearly observed that, unlike pure CNNs, in NiSe... 0.5 S 1.5 The / CNNs (insitu) composite material reacts instantly to changes in light conditions, indicating that NiSe... 0.5 S 1.5 It can effectively accelerate the transfer rate of photogenerated electrons. Figure 8 b represents the LSV polarization curve at -5 mA·cm⁻¹ -2 NiSe at current density 0.5 S 1.5 The electrocatalytic hydrogen evolution overpotential is only -0.86V, indicating its superior electrocatalytic hydrogen evolution performance. NiSe 0.5 S 1.5 The overpotential of the / CNNs (insitu) composite material is lower than that of pure CNNs, indicating that the added NiSe... 0.5 S 1.5 The co-catalyst effectively reduced the hydrogen evolution overpotential of CNNs, promoting the evolution of H2 from the catalyst surface. Figure 8 c represents the impedance spectrum, indicating that NiSe 0.5 S 1.5 With a very small Faraday impedance, its introduction significantly reduces the charge transfer impedance of CNNs and improves their conductivity. Furthermore, the equivalent circuit of this test system is shown in the illustration. NiSe 0.5 S 1.5 The charge transfer resistance R1 is approximately 2.0 kΩ, while NiSe 0.5 S 1.5 The charge transfer resistance of the CNNs (insitu) composite material is approximately 25.6 kΩ, and the charge transfer efficiency of the composite material is improved compared with that of pure CNNs. Figure 8 d is the PL spectrum of the sample, NiSe 0.5 S 1.5 The fluorescence intensity of / CNNs (insitu) decreased significantly, while NiSe at this excitation wavelength... 0.5 S 1.5 Almost no fluorescence was produced, indicating that NiSe 0.5 S 1.5 The introduction of this technology can suppress the recombination of photogenerated carriers in CNNs and improve the separation efficiency of photogenerated electron-hole pairs.

[0047] To investigate the intrinsic active specific surface area of ​​the catalyst, the double-layer capacitance (Cdl) of the sample during the non-Radidatic reaction stage was measured to represent the electrochemically active specific surface area (ECSA) of the material, such as... Figure 9 As shown. At 10mVs -1 ~140mVs-1 CV cycling tests were performed on the non-reactive region of the sample at a scan rate of [missing information]. Figure 8 By fitting the voltage and current density curves at different scan rates, NiSe was obtained. 0.5 S 1.5 The Cdl value is 78 μF·cm. -2 CNNs and NiSe 0.5 S 1.5 The Cdl values ​​of the / CNNs (insitu) are very close. The ECSA of the catalyst = Cdl / Cs, and under the same test conditions, the specific capacitance Cs of the system is similar. This indicates that NiSe 0.5 S 1.5 It grows closely with CNNs, and during in situ compositing, it is restricted by CNNs to grow to a smaller size and provides almost no more active sites for CNNs, which is consistent with the XPS analysis and It curve results.

[0048] 5. NiSe 0.5 S 1.5 Research on the mechanism of enhanced photocatalytic activity of CNNs like Figure 10 As shown, black NiSe 0.5 S 1.5 The monomer exhibited strong light absorption across the entire test wavelength range, and no absorption sidebands could be obtained from the absorption spectrum. In contrast, the absorption sidebands of CNNs were around 460 nm. (The last sentence appears to be incomplete and possibly refers to NiSe.) 0.5 S 1.5 In-situ recombination resulted in a redshift of the absorption sideband, significantly enhancing the system's light absorption. The band gap of the CNNs was calculated to be 2.66 eV using the Tauc equation, and the NiSe... 0.5 S 1.5 The individual components have almost no optical band gap. The band structure of the CNNs was determined using MS curves. The flat band potential of the n-type semiconductor CNNs is approximately -0.91V, and the difference between the flat band potential of the n-type semiconductor and the CB is approximately 0.2V. Therefore, the CB position of the CNNs is approximately -1.11V. According to the empirical formula (Equation 2.1), the VB position of the CNNs is +1.55V. Meanwhile, the NiSe... 0.5 S 1.5 The conduction band potential of NiSe is approximately -0.84V. Additionally, XPS was used to test the NiSe... 0.5 S 1.5 The maximum VB value is -0.57eV.

[0049] Based on the above analysis, NiSe is proposed. 0.5 S 1.5 Enhanced mechanism of photocatalytic hydrogen production in composite materials formed by in-situ growth between and on the surface of CNNs (see [link to article]). Figure 11 NiSe 0.5 S 1.5 In-situ growth is constrained by the sheet-like structure of CNNs, resulting in uniform growth on CNNs with smaller size and lower crystallinity, without altering the morphology and chemical state of the CNNs. Due to NiSe... 0.5 S 1.5 NiSe forms a dense connection with CNNs. 0.5 S 1.5 It tends to expose the (111) and (200) crystal planes with larger lattice spacing. NiSe 0.5 S 1.5 Close contact with CNNs reduces the co-catalyst shedding during photocatalysis, significantly enhancing the stability of the photocatalyst. NiSe 0.5 S 1.5 CNNs form a Schottky barrier at the contact surface, and when exposed to light, NiSe... 0.5 S 1.5 Electrons in the CNNs (insitu) composite material undergo rapid migration, moving quickly from the conduction band of the CNNs to NiSe. 0.5 S 1.5 The above and enrichment of H + Restored to H2, holes remain in the valence band of CNNs and are consumed by TEOA. NiSe 0.5 S 1.5 As a co-catalyst, it can effectively reduce NiSe. 0.5 S 1.5 The charge transfer impedance of the / CNNs (insitu) system enables rapid transfer of photogenerated electrons, reduces carrier recombination, and thus improves the hydrogen production activity of the photocatalyst.

[0050] It should be noted that when numerical ranges are mentioned in the claims of this invention, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. To avoid redundancy, the present invention describes preferred embodiments.

[0051] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the invention.

[0052] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for preparing a nickel sulfide selenide co-catalyst, characterized in that, The process includes the following steps: dispersing a soluble nickel source, a soluble sulfur source, and a soluble selenium source in ethylene glycol, reacting at 160-200°C for 10-20 hours, washing, and drying to obtain the nickel sulfoselenide. The molar ratio of the soluble nickel source, soluble sulfur source, and soluble selenium source is 1:0.5~1.5:0.5~1.

5.

2. The preparation method according to claim 1, characterized in that, The soluble nickel source is selected from any one of nickel chloride, nickel nitrate, and nickel acetate; The soluble sulfur source is thiourea; The soluble selenium source is sodium selenite.

3. A nickel sulfoselenide cocatalyst prepared by the preparation method according to any one of claims 1 to 2.

4. A nickel sulfide selenide photocatalyst, characterized in that, It is a composite material in which the nickel sulfide selenide cocatalyst of claim 3 is supported on a carbon nitride material; The content of nickel sulfide selenide in the composite material is 10~25wt%, and the content of carbon nitride material is 75~90wt%.

5. The nickel sulfide photocatalyst according to claim 4, characterized in that, The carbon nitride material is carbon nitride nanosheets.

6. The nickel sulfide selenide photocatalyst according to claim 4, characterized in that, The preparation of the nickel sulfose selenide photocatalyst includes the following steps: the nickel sulfose selenide and the carbon nitride material are added to a solvent and reacted for 30 min to 60 min, and then evaporated to dryness at 60℃ to 80℃ to obtain the nickel sulfose selenide photocatalyst; The solvent is anhydrous ethanol or water.

7. The nickel sulfide photocatalyst according to claim 4, characterized in that, The preparation of the nickel sulfose selenide photocatalyst includes the following steps: dispersing a soluble nickel source, a soluble sulfur source, a soluble selenium source and carbon nitride material in ethylene glycol, reacting at 160~200℃ for 10~20h, washing, and drying to obtain the nickel sulfose selenide photocatalyst; The mass ratio of soluble nickel source, soluble sulfur source, soluble selenium source and carbon nitride material is 18~50:8~27:6~20:

100.

8. The application of the nickel sulfide photocatalyst according to claim 4 in photocatalytic water splitting for hydrogen production.