Recycled asphalt mixture of high-consumption RAP fine material and preparation method of recycled asphalt mixture

By using the technical means of cold addition of recycled adhesive mortar and warm mix additive, the problem of high-proportion stable disposal of RAP fine aggregate in recycled asphalt mixtures has been solved, realizing the efficient recycling of RAP fine aggregate and improving the water stability and durability of recycled asphalt mixtures.

CN122036238APending Publication Date: 2026-05-15HUBEI PROVINCE FREEWAY IND DEV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610295643.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-11
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

In existing technologies, it is difficult to achieve high-proportion, stable, and controllable recycling of RAP fines, especially at room temperature where they are difficult to effectively wet and disperse, resulting in poor recycling performance and resource waste.

Method used

By using cold-added recycled asphalt and warm-mixing agents, cold-gelled fine aggregates are formed through room-temperature pre-coating and hot-end mixing. The temperature difference drives the evaporation of the aqueous phase and the charge instability of the emulsifier, achieving a high proportion of stable RAP fine aggregate incorporation. Furthermore, the water stability and durability of the mixture are improved by modifying asphalt and using interface modifiers.

Benefits of technology

It achieves a high proportion of stable RAP fine aggregate in recycled asphalt mixtures, significantly reduces energy consumption and disposal rate, improves water stability and durability, enhances the bonding effect between new and old asphalt, and meets the performance requirements of recycled asphalt mixtures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122036238A_ABST
    Figure CN122036238A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of recycled asphalt, in particular to a high-consumption RAP fine aggregate recycled asphalt mixture and a preparation method thereof.The high-consumption RAP fine aggregate recycled asphalt mixture is prepared from, by weight, 30-50 parts of RAP fine aggregate, 10-30 parts of RAP coarse aggregate, 25-30 parts of new coarse aggregate, 4-5.2 parts of matrix asphalt, 3-5 parts of cold additive recycled rubber cement, 3-5 parts of mineral powder and 0.2-0.26 part of warm mixing agent. When the total doping amount of the RAP is 60%, the proportion of the fine materials in the total RAP is larger than or equal to 50%, the fine materials can be stably doped, the discarding rate and energy consumption of the fine materials are remarkably reduced, and the RAP fine materials can be consumed in a high proportion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of recycled asphalt technology, specifically to a recycled asphalt mixture with high RAP fine aggregate absorption and its preparation method. Background Technology

[0002] With the continuous increase in road maintenance volume, the efficient recycling of reclaimed asphalt pavement (RAP) has become an important direction for the sustainable construction of asphalt pavements. The fine aggregate portion of RAP (typically with a particle size of 0–4.75 mm) contains a high proportion of aged asphalt and is the most difficult component in RAP to achieve a high and stable proportion for disposal. Current engineering practices generally limit the amount of RAP fine aggregate to a low range, or treat it as a low-value material for off-site transport and backfilling, resulting in resource waste, increased carbon emissions, and low recycling rates.

[0003] In traditional thermal recycling systems, RAP fine aggregates require high-temperature preheating to soften aged asphalt. However, due to their large specific surface area and severe surface aging, they are prone to secondary oxidation at high temperatures, further increasing viscosity and hardness and generating fumes, thus affecting recycling efficiency and the construction environment. Simultaneously, the fine aggregates have strong adsorption properties, easily encapsulating new asphalt to form "black clumps," making it difficult for new and old asphalt to blend uniformly, resulting in an imbalanced asphalt-aggregate ratio and a significant decline in mixture performance. Adding new asphalt at high temperatures exacerbates this problem. Although technologies such as foamed asphalt and warm-mix additives have developed, they still cannot avoid heat treatment of RAP and lack effective means to wet and disperse fine aggregates at room temperature. This makes it difficult to achieve high-proportion, stable, and controllable utilization of fine aggregates, becoming a major technical bottleneck for improving RAP utilization.

[0004] In summary, under current technological conditions, it is difficult to achieve a high proportion, stable and controllable recycling of RAP fines, which has become a key bottleneck in further increasing the total amount of RAP consumed. Summary of the Invention

[0005] The purpose of this invention is to overcome the above-mentioned shortcomings and provide a recycled asphalt mixture and its preparation method that achieves a high proportion of stable RAP fines incorporation without high-temperature preheating of RAP fines, and ensures high absorption of RAP fines in mixing, dispersion, interfacial bonding and water stability.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: a recycled asphalt mixture with high absorption capacity of RAP fine aggregate, comprising by weight: 30-50 parts of RAP fine aggregate, 10-30 parts of RAP coarse aggregate, 25-30 parts of new coarse aggregate, 4-5.2 parts of base asphalt, 3-5 parts of cold-added recycled binder, 3-5 parts of mineral powder and 0.2-0.26 parts of warm mix additive.

[0007] Furthermore, the particle size of the RAP fine aggregate is 0-6 mm; the particle size of the RAP coarse aggregate is 6-17 mm; and the new coarse aggregate is limestone with a particle size of 11-24 mm.

[0008] Furthermore, the cold-added recycled adhesive comprises, by weight, 60-80 parts of bio-based fatty acid ester, 15-30 parts of deionized water, 3-8 parts of polyol and 1.5-4.0 parts of cationic emulsifier.

[0009] Furthermore, the bio-based fatty acid ester is a mixture of fatty acid methyl esters (FAME) obtained from vegetable oil through a transesterification process.

[0010] Furthermore, the polyol is glycerol.

[0011] Furthermore, the cationic emulsifier is a quaternary ammonium chloride, including but not limited to hexadecyltrimethylammonium chloride.

[0012] Furthermore, the mineral powder is S95 slag powder with a moisture content of ≤1%.

[0013] Furthermore, the warm mixing agent is an organic wax-based warm mixing agent.

[0014] A method for preparing recycled asphalt mixture with high absorption capacity of RAP fines, comprising the following steps: S1. Room temperature pre-coating: Mix RAP fines and cold-added recycled adhesive in a mixing pot for 60-90 seconds, then pour out and let stand for 10-20 minutes to complete room temperature penetration and initial coagulation, and obtain cold gelled fine particles. S2. Warm mix modification: After heating the base asphalt to 140℃, add the warm mix agent and mix at 140℃ for 15-20 minutes using a high-speed shear machine at a stirring speed of 2000r / min to obtain modified asphalt. S3. Hot end mixing: The RAP coarse aggregate is heated to 140°C. The new coarse aggregate and mineral powder are mixed and then heated to 160°C. The heated RAP coarse aggregate, new coarse aggregate and mineral powder are then mixed with the modified asphalt obtained in S2 at 140°C for 60 seconds to obtain the mixed mixture. S4. Cold addition: The cold gelled fine aggregates obtained in S1 are added to the mixture that has been hot-mixed in S3 through a cold hopper, and the mixture is further mixed at 140°C for 60-90 seconds to obtain a recycled asphalt mixture with high RAP fine aggregate absorption.

[0015] Furthermore, the preparation method of the cold-added regenerated adhesive is to mix bio-based fatty acid esters, deionized water, polyols, and cationic emulsifiers at room temperature, and then shear them at 2000 r / min for 8-12 min using a high-speed shearing machine to form a stable microemulsion. After standing for defoaming for 30 min, the mixture is obtained.

[0016] Compared with the prior art, the present invention has the following beneficial effects: 1. In this invention, when the total RAP content is 60%, the proportion of fine materials in the total RAP is ≥50%, and it can be stably incorporated, which significantly reduces the waste rate of fine materials and energy consumption, and can consume RAP fine materials in a high proportion. 2. This invention adds cold-added recycled asphalt slurry to the recycled asphalt mixture. The cold-added recycled asphalt slurry wets, penetrates, and softens the RAP fine aggregates at room temperature, achieving cold coating of the RAP fine aggregates and forming cold-gelled fine agglomerates. The cold-gelled fine agglomerates are added coldly into the mixture of heated RAP coarse aggregate, new coarse aggregate, mineral powder, and modified base asphalt through a cold hopper. The temperature difference drives the rapid evaporation of the aqueous phase and the instability of the emulsifier charge, while the oil phase rapidly solidifies and forms a continuous recycled film, thereby achieving rapid redispersion and uniform coating, and solving the defects of traditional thermal recycling in the prior art. 3. This invention adds a warm mix agent to the recycled asphalt mixture. The warm mix agent can act as an interface modifier between the base asphalt and the cold-added recycled mortar, so that the room temperature coating and hot end recycling processes can form a compatible system, thereby significantly improving the water stability and durability of the recycled asphalt mixture. Attached Figure Description

[0017] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The images show actual photos of the recycled asphalt mixture prepared according to the present invention and the recycled asphalt mixture prepared by thermal addition and thermal recycling.

[0018] In the figures: the left figure shows the recycled asphalt mixture prepared by the present invention; the right figure shows the recycled asphalt mixture prepared by thermal addition and thermal recycling in the prior art. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] Please see Figure 1 .

[0021] Example 1: The present invention relates to a high-absorption RAP fine aggregate recycled asphalt mixture, wherein the RAP content is 60%, and by weight it comprises: 30 parts RAP fine aggregate, 30 parts RAP coarse aggregate, 26.54 parts new coarse aggregate, 5.2 parts base asphalt, 3 parts cold-added recycled asphalt mortar, 5 parts mineral powder and 0.26 parts warm mix agent.

[0022] It should be noted that the particle size of the RAP fine aggregate is 0-6 mm; the particle size of the RAP coarse aggregate is 6-17 mm; and the new coarse aggregate is limestone with a diameter of 11-24 mm and an apparent density ≥2.50 g / cm³. 3 Water absorption rate ≤2.0%.

[0023] It should be noted that the oil content of RAP fines is 7.5-8.5%, and the oil content of RAP coarses is 2.8-3.2%.

[0024] It should be noted that the cold-added recycled adhesive comprises, by weight, 60-80 parts of bio-based fatty acid ester, 15-30 parts of deionized water, 3-8 parts of polyol and 1.5-4.0 parts of cationic emulsifier.

[0025] It should be noted that the bio-based fatty acid ester is a mixture of fatty acid methyl esters (FAME) obtained from vegetable oil through a transesterification process. Bio-based fatty acid esters, as the main phase oily regenerator, have the core function of penetrating and softening aged asphalt at room temperature: 1. RAP materials contain a large number of ketone groups, carbonyl groups, carboxylates, and aromatic structures. The polarity of the ester groups matches that of the RAP materials, which can selectively dissolve and penetrate the polar components of aged asphalt. 2. Promotes the formation of a "flowable transition layer" on the surface of RAP fine aggregate, which can form a thin oily penetrating layer at room temperature; during hot-end mixing, this layer quickly dissolves with the hot matrix asphalt to form a unified binder phase.

[0026] It should be noted that the polyol is glycerol. To enhance the wettability of water relative to the polar aged film in RAP fines, the polyol has multiple hydroxyl groups, which can form hydrogen bonds with the carbonyl groups in the aged film, increasing the affinity of water relative to its surface and improving wetting efficiency at room temperature. The polyol also reduces the interfacial tension between the oil and water phases, ensuring that the microemulsion does not separate and improving its stability.

[0027] It should be noted that the cationic emulsifier is a quaternary ammonium chloride, including but not limited to hexadecyltrimethylammonium chloride. Limestone and aged asphalt are mostly negatively charged in water, while cationic emulsifiers are positively charged and have the advantage of charge adsorption on aggregates and aged adhesive films. They improve the dispersibility at room temperature and the ability to break up agglomerates of fine materials. The cationic emulsifier reduces the interfacial energy, making it easier for RAP fine materials to be adsorbed and dispersed by the oil phase and to prevent agglomeration.

[0028] It should be noted that the warm mix agent is an organic wax-based warm mix agent. In the preparation of recycled asphalt mixtures, the warm mix agent exerts multiple effects, including reducing asphalt viscosity, improving interfacial spread, enhancing coating penetration of RAP, lowering construction temperature, reducing secondary aging, and improving compaction, thus making the recycling of high-content RAP, especially RAP fines, more stable and feasible. The warm mix agent can also act as an interfacial modifier between new asphalt and recycled binder, creating a compatible system for room-temperature coating and hot-end recycling processes, thereby significantly improving the water stability and durability of the mixture.

[0029] Preferably, the deionized water is distilled water, which serves as the external phase of the microemulsion, allowing the oil phase to disperse in "nano-particles" to form a microemulsion structure (oil droplets dispersed in the aqueous phase) → the oil droplets can more easily enter the "micro-cracks" of the aged adhesive film, improving the penetration efficiency; after the cold-gelled fine particles are added to the hot end at 140~160℃: the aqueous phase vaporizes instantaneously → the microemulsion ruptures → the oil phase is immediately released and mixes with the hot matrix asphalt, completing the two-stage action of cold addition → hot end regeneration.

[0030] Preferably, the mineral powder is S95 slag powder with a moisture content of ≤1%.

[0031] A method for preparing recycled asphalt mixture with high absorption capacity of RAP fines, comprising the following steps: S1. Room temperature pre-coating: Mix RAP fines and cold-added recycled adhesive in a mixing pot for 60-90 seconds, then pour out and let stand for 10-20 minutes to complete room temperature penetration and initial coagulation, and obtain cold gelled fine particles. S2. Warm mix modification: After heating the base asphalt to 140℃, add the warm mix agent and mix at 140℃ for 15-20 minutes using a high-speed shear machine at a stirring speed of 2000r / min to obtain modified asphalt. S3. Hot end mixing: The RAP coarse aggregate is heated to 140°C. The new coarse aggregate and mineral powder are mixed and then heated to 160°C. The heated RAP coarse aggregate, new coarse aggregate and mineral powder are then mixed with the modified asphalt obtained in S2 at 140°C for 60 seconds to obtain the mixed mixture. S4. Cold addition: The cold gelled fine aggregates obtained in S1 are added to the mixture that has been hot-mixed in S3 through a cold hopper, and the mixture is further mixed at 140°C for 60-90 seconds to obtain a recycled asphalt mixture with high RAP fine aggregate absorption.

[0032] It should be noted that the preparation method of the cold-added regenerated adhesive is to mix bio-based fatty acid esters, deionized water, polyols and cationic emulsifiers at room temperature, and then shear them at 2000 r / min for 8-12 min using a high-speed shearing machine to form a stable microemulsion. After standing for defoaming for 30 min, the mixture is obtained.

[0033] Example 2: The difference between this embodiment and Embodiment 1 is that, by weight, it includes 40 parts of RAP fine aggregate, 20 parts of RAP coarse aggregate, 27.17 parts of new coarse aggregate, 4.6 parts of base asphalt, 4 parts of cold-added recycled adhesive, 4 parts of mineral powder, and 0.23 parts of warm mix additive.

[0034] Example 3: The difference between this embodiment and Embodiment 1 is that, by weight, it includes 50 parts of RAP fine aggregate, 10 parts of RAP coarse aggregate, 27.8 parts of new coarse aggregate, 4 parts of base asphalt, 5 parts of cold-added recycled adhesive, 3 parts of mineral powder, and 0.2 parts of warm mix agent.

[0035] Comparative Example 1: The difference between this comparative example and Example 1 is that the S1 step is omitted in the preparation method of a recycled asphalt mixture with high RAP fine aggregate absorption. The cold-added recycled mortar is sprayed into the RAP fine aggregate, and in the S3 step, it is directly added to the hot aggregate through the cold hopper.

[0036] Comparative Example 2: The difference between this comparative example and Example 1 is that step S2 is omitted in the preparation method of a recycled asphalt mixture with high absorption capacity of RAP fine aggregate. In step S3, the warm mix agent and the base asphalt are directly added to the mixing pot and mixed with the heated RAP coarse aggregate, new coarse aggregate and mineral powder.

[0037] Comparative Example 3: The difference between this comparative example and Example 1 is that cold-added recycled adhesive is not used, and step S1 is omitted in the preparation method.

[0038] Comparative Example 4: The difference between this comparative example and Example 1 is that a warm mixing agent was not used, and step S2 was omitted.

[0039] Comparative Example 5: The difference between this comparative example and Example 1 is that, instead of using cold-added recycled asphalt and warm-mixing agents, the RAP fine aggregate and RAP coarse aggregate are preheated together to 140°C, the new coarse aggregate is preheated to 170°C, the base asphalt is preheated to 160°C, and the recycled asphalt mixture is prepared by hot addition method at a mixing temperature of 180°C.

[0040] The performance of the recycled asphalt mixtures prepared in Examples 1-3 and Comparative Examples 1-5 was tested, and the specific results are shown in Table 1 below: Table 1. Performance test results of recycled asphalt mixtures in the examples and comparative examples.

[0041] As shown in Table 1: 1. Combining Examples 1-3, under the same RAP content (60%), increasing the RAP fine aggregate content will improve the water stability performance (residual stability and freeze-thaw splitting strength ratio) of recycled asphalt mixtures. The water stability performance reaches its peak when the content reaches 40%, but it will reduce the high and low temperature performance (high temperature rutting dynamic stability and low temperature beam bending strain). However, the overall performance is higher than the technical indicators and meets the performance requirements of recycled asphalt mixtures. 2. Combining Example 1 and Comparative Example 1, under the same RAP dosage, cold addition of recycled adhesive and warm mixing agent, using step S1 - room temperature pre-coating, the residual stability and freeze-thaw splitting strength ratio increased by 3.54 percentage points and 14.84 percentage points, respectively, the dynamic stability increased by 1677 cycles / mm, and the bending tensile failure strain increased by 3039 με. Combining Example 1 and Comparative Example 3, under the same RAP dosage and warm mixing conditions, cold addition of recycled adhesive and S1 step-room temperature pre-coating were used. Although the residual stability decreased, it still met the performance requirements. The freeze-thaw splitting strength ratio was significantly improved, specifically by 17.33 percentage points, the dynamic stability was improved by 4724 cycles / mm, and the bending tensile failure strain was improved by 4940με. That is, by introducing cold-added recycled adhesive and performing step S1 - room temperature pre-coating, the water stability, high-temperature rutting resistance and low-temperature crack resistance of high-content RAP recycled mixtures are significantly improved. 3. Combining Example 1 and Comparative Example 2, under the same RAP content, cold addition of recycled adhesive and warm mix agent, the S2 step-warm mix agent modification of the base asphalt can improve the residual stability and freeze-thaw splitting strength ratio by 1.78 percentage points and 3.58 percentage points, respectively, improve the dynamic stability by 3048 cycles / mm, and improve the flexural tensile failure strain by 6289με. Combining Example 1 and Comparative Example 4, under the same RAP dosage and cold addition of recycled adhesive, the use of warm mixing agent for modification and the S2 step-warm mixing agent modification resulted in an increase of 9.65 percentage points and 12.07 percentage points in residual stability and freeze-thaw splitting strength ratio, respectively, an increase of 4669 cycles / mm in dynamic stability, and an increase of 5864 με in flexural tensile failure strain. That is, by adding a warm mix agent and performing the S2 step-warm mix agent modification to modify the base asphalt, the viscosity of the base asphalt can be effectively reduced, the coating effect can be improved and the compaction properties can be increased, thereby significantly enhancing the water stability, high temperature rutting resistance and overall toughness of the recycled mixture. 4. In conjunction with Example 1 and Comparative Example 5, the present invention is compared with the conventional hot-addition hot recycling scheme. The technical solution of the present invention can improve the residual stability and freeze-thaw splitting strength ratio by 14.89 percentage points and 21.65 percentage points, respectively, improve the dynamic stability by 6068 cycles / mm, and improve the flexural tensile failure strain by 9434με. The results show that the technical solution of the present invention can effectively avoid the secondary aging of RAP fines, significantly enhance the bonding ability between new and old asphalt, and achieve a comprehensive improvement in water stability, high-temperature rutting resistance and low-temperature crack resistance of recycled asphalt mixtures with a high proportion of RAP fines.

[0042] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

Claims

1. A recycled asphalt mixture with high absorption capacity for RAP fine aggregates, characterized in that, By weight, it includes: 30-50 parts RAP fine aggregate, 10-30 parts RAP coarse aggregate, 25-30 parts new coarse aggregate, 4-5.2 parts base asphalt, 3-5 parts cold-added recycled binder, 3-5 parts mineral powder, and 0.2-0.26 parts warm mix additive.

2. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 1, characterized in that, The fine RAP aggregate has a particle size of 0-6 mm; the coarse RAP aggregate has a particle size of 6-17 mm; and the new coarse aggregate is limestone with a particle size of 11-24 mm.

3. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 1, characterized in that, The cold-added regenerated adhesive comprises, by weight, 60-80 parts of bio-based fatty acid ester, 15-30 parts of deionized water, 3-8 parts of polyol and 1.5-4.0 parts of cationic emulsifier.

4. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 3, characterized in that, The bio-based fatty acid ester is a mixture of fatty acid methyl esters (FAME).

5. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 3, characterized in that, The polyol is glycerol.

6. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 3, characterized in that, The cationic emulsifier is a quaternary ammonium chloride, including but not limited to hexadecyltrimethylammonium chloride.

7. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 3, characterized in that, The mineral powder is S95 slag powder with a moisture content of ≤1%.

8. The recycled asphalt mixture with high RAP fine aggregate absorption according to claim 1, characterized in that, The warm mixing agent is an organic wax-based warm mixing agent.

9. A method for preparing recycled asphalt mixture with high RAP fine aggregate absorption, characterized in that, The method for preparing recycled asphalt mixtures with high RAP fines according to any one of claims 1-8 comprises the following steps: S1. Room temperature pre-coating: Mix RAP fines and cold-added recycled adhesive in a mixing pot for 60-90 seconds, then pour out and let stand for 10-20 minutes to complete room temperature penetration and initial coagulation, and obtain cold gelled fine particles. S2. Warm mix modification: After heating the base asphalt to 140℃, add the warm mix agent and mix at 140℃ for 15-20 minutes using a high-speed shear machine at a stirring speed of 2000r / min to obtain modified asphalt. S3. Hot end mixing: The RAP coarse aggregate is heated to 140°C. The new coarse aggregate and mineral powder are mixed and then heated to 160°C. The heated RAP coarse aggregate, new coarse aggregate and mineral powder are then mixed with the modified asphalt obtained in S2 at 140°C for 60 seconds to obtain the mixed mixture. S4. Cold addition: The cold gelled fine aggregates obtained in S1 are added to the mixture that has been hot-mixed in S3 through a cold hopper, and the mixture is further mixed at 140°C for 60-90 seconds to obtain a recycled asphalt mixture with high RAP fine aggregate absorption.

10. The method for preparing recycled asphalt mixture with high RAP fine aggregate according to claim 9, characterized in that, The preparation method of the cold-added regenerated adhesive is as follows: bio-based fatty acid ester, deionized water, polyol and cationic emulsifier are mixed at room temperature, sheared at 2000 r / min for 8-12 min using a high-speed shearing machine to form a stable microemulsion, and then allowed to stand for defoaming for 30 min to obtain the final product.