A high-strength rare earth magnesium alloy based on a room-temperature rotary swaging composite process and a preparation method thereof

By adding elements such as Gd, Y, and Zn to magnesium alloys, combined with room temperature rotary forging and aging treatment, the problems of low strength and complex processes of magnesium alloys have been solved, and the preparation of high-strength rare earth magnesium alloys has been realized to meet the needs of aerospace and other fields.

CN122071762APending Publication Date: 2026-05-22SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411678613.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-22
Publication Date
2026-05-22

AI Technical Summary

Technical Problem

Traditional magnesium alloys have low absolute strength and ductility at room temperature, which limits their applications. Existing high-temperature rotary forging processes increase production costs and reduce production efficiency.

Method used

By adding rare earth elements Gd and Y and transition element Zn, the smelting and heat treatment processes are optimized. Combined with extrusion composite room temperature rotary forging deformation process and artificial aging treatment, the grains are refined, the texture is improved, dislocations and twins are introduced, and the aging strengthening ability is enhanced.

Benefits of technology

High-strength rare-earth magnesium alloys can be prepared in a short process to meet the demand for high-performance lightweight materials in aerospace, rail transportation and automotive fields, with tensile strength of 500-580 MPa and high production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122071762A_ABST
    Figure CN122071762A_ABST
Patent Text Reader

Abstract

The application provides a high-strength rare earth magnesium alloy based on a room-temperature rotary swaging composite process and a preparation method thereof.The method comprises the following specific steps: according to designed components, raw materials are smelted to obtain a semi-continuous casting ingot, the rare earth magnesium alloy ingot is subjected to homogenization treatment, then is preheated and kept warm to be subjected to differential temperature extrusion, the extruded rare earth magnesium alloy is subjected to multi-pass rotary swaging treatment with a small deformation at room temperature, and finally is subjected to artificial aging treatment.Through the composite process with the room-temperature rotary swaging, the grains can be refined, the texture can be improved, and a large number of dislocations and twins can be introduced into the grains, so that the nucleation sites and precipitation power of precipitated phases in the aging process are improved, the aging strengthening capacity is more excellent, and the high-strength rare earth magnesium alloy is obtained.The application of the light-weight high-strength rare earth magnesium alloy in the fields of aerospace, rail transportation and automobiles can be accelerated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal structural materials technology, and more particularly to the field of rare earth magnesium alloy design and preparation technology. Specifically, it relates to a high-strength rare earth magnesium alloy based on a room temperature rotary forging composite process and its preparation method. Background Technology

[0002] Magnesium alloys, as lightweight structural materials with excellent specific strength and specific stiffness, show promising potential to replace steel and aluminum alloys in rail transportation, aerospace, and automotive fields, reducing weight and improving economic efficiency. However, the relatively low absolute strength and ductility of traditional magnesium alloys at room temperature limit their applications. Therefore, there is an urgent need for magnesium alloys with superior mechanical properties to further enhance their applications.

[0003] Alloying can effectively improve the mechanical properties of magnesium alloys. Rare earth magnesium alloys possess excellent solid solution strengthening and age hardening capabilities, and adding heavy rare earth elements such as Gd and Y is an effective way to develop high-strength magnesium alloys. Adding appropriate amounts of transition elements such as Zn and Ni to rare earth magnesium alloys can form a long-period stacked ordered structure, namely the LPSO phase. The LPSO phase can improve the alloy's strength while also undergoing flexural deformation, thus improving the alloy's plasticity. Patent document CN201510900499.6 describes achieving a room-temperature tensile strength exceeding 400 MPa by casting an alloy of Mg-(10.0~18.0)wt.%Gd-(0.5~2.0)wt.%Zn-(0.3~0.7)wt.%Zr, but this still does not meet the performance requirements.

[0004] The mechanical properties of magnesium alloys can also be improved through plastic deformation such as grain refinement and work hardening. Large plastic deformation (SPD) techniques, such as equal channel angular compression (ECAP) and high pressure torsion (HPT), can significantly improve the strength and plasticity of alloys. However, the small sample size, specialized equipment requirements, and low processing efficiency limit their widespread application. In contrast, rotary forging (RS), as a conventional forming technique with high processing efficiency, low cost, and adjustable and controllable deformation, can improve material properties with relatively small strain accumulation. During rotary forging, the continuous change in shear stress direction and high strain rate promote the formation of deformation twins, stacked dislocations, and high-density dislocations within the coarse grains, thereby significantly improving the alloy's strength.

[0005] Martynenko et al. investigated the effects of high-temperature RS (reverse rotation) at 400℃ on the microstructure evolution and mechanical properties of Mg-Zn-Ca alloys. Thermal RS significantly reduced the grain size of the alloy, thereby increasing the ultimate tensile strength from 217 MPa to 276 MPa. Chen et al. obtained a nano-magnesium alloy with a UTS (Ultra-Thickness) of 560 MPa by RS treatment of AZ31 magnesium alloy at liquid nitrogen temperature. In CN108707848A, the forging temperature ranges from 100 to 370℃. The above studies mainly focus on hot RS and low-temperature RS, but these preparation processes increase production costs and reduce production efficiency in actual production. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a high-strength rare-earth magnesium alloy based on a room-temperature rotary forging composite process and its preparation method. This invention optimizes the smelting and heat treatment processes by adding rare-earth elements Gd and Y, and transition element Zn. It utilizes a deformation process combining extrusion and room-temperature rotary forging, along with artificial aging treatment, to refine grains, improve texture, and introduce defects such as dislocations and twins, thereby increasing the nucleation sites and precipitation kinetics of precipitates during aging and achieving superior age-strength capabilities. This invention obtains a high-strength rare-earth magnesium alloy in a short process, overcoming the current problems of low strength, complex processes, and high equipment requirements for magnesium alloys. It can meet the urgent needs of aerospace, rail transportation, and automotive industries for high-performance, lightweight magnesium alloy materials.

[0007] The objective of this invention is achieved through the following technical solution:

[0008] In a first aspect, the present invention provides a method for preparing a high-strength rare-earth magnesium alloy based on a room-temperature rotary forging composite process, the method comprising the following steps:

[0009] A. Prepare high-strength rare earth magnesium alloy semi-continuous casting ingots according to preset composition;

[0010] B. Homogenize the magnesium alloy semi-continuous casting ingot at 480-525℃ to obtain homogenized rare earth magnesium alloy.

[0011] C. The homogenized rare earth magnesium alloy is subjected to differential temperature hot extrusion to obtain rare earth magnesium alloy extruded bars or plates; the temperature of the homogenized rare earth magnesium alloy used in the differential temperature hot extrusion is 450-520℃, the temperature of the extrusion die is 320-450℃, and the extrusion ratio is 4-16.

[0012] D. Perform multi-pass room temperature rotary forging on rare earth magnesium alloy extruded bars or plates to obtain forged bars or plates; the total deformation of the multi-pass room temperature rotary forging is 4-20%.

[0013] E. Artificial aging treatment is performed on the forged bars or plates to obtain the high-strength rare earth magnesium alloy.

[0014] As a preferred embodiment, in step A, the high-strength rare-earth magnesium alloy comprises the following elements in weight percentages: Gd 8-18%, Y 1.94-4%, Zn 0.5-2.0%, Mn 0-1%, with the balance being Mg and unavoidable impurities, wherein the total amount of impurities is less than 0.02%.

[0015] In this invention, the contents of Gd, Y, Zn, and Mn are adjusted, with Gd as the main element. At the eutectic point temperature, the limiting solid solubility of Gd in Mg is 23.49 wt.%, and the solid solubility decreases rapidly with decreasing temperature. The precipitated metastable nano-β' phase gives the Mg-Gd alloy significant age-hardening ability and room-temperature / high-temperature mechanical properties. Adding a certain amount of Y to the Mg-Gd alloy reduces the solid solubility of both elements and significantly increases the number density of the β' precipitate, further enhancing the age-hardening ability of the rare-earth magnesium alloy, thereby improving the room-temperature strength of the alloy. To ensure the alloy's aging ability and high strength, the Gd content is set to 8–18 wt.%, and the Y content is set to 1.94–4 wt.%.

[0016] This invention further introduces trace amounts of Zn: In rare earth magnesium alloys, the addition of appropriate amounts of Zn can form LPSO structural phases and basal γ' phases together with Gd and Y elements. The formation of high-modulus, high-strength LPSO structural phases is beneficial to improving the room temperature / high temperature strength of the alloy; the LPSO structural phases can undergo flexural deformation, thereby improving the plasticity of the alloy; the precipitate network formed by the basal γ' phase and the cylindrical β' phase can achieve a composite strengthening effect. In this invention, the Zn content is set to 0.5–2.0 wt.%.

[0017] In this invention, a small amount of Mn element is added. Mn element is cheaper than Zr element, which is commonly added to magnesium alloys. Mn element can promote recrystallization behavior during the extrusion process of magnesium alloys. At the same time, element segregation at the α-Mn particle interface can improve the room temperature / high temperature strength of the alloy. In this invention, the Mn content is set to 0-1 wt.%.

[0018] As a further preferred embodiment, the high-strength rare-earth magnesium alloy comprises the following elements in weight percentages: Gd 8–14.02%, Y 1.94–4%, Zn 0.5–1.51%, Mn 0.4–1%, with the balance being Mg and unavoidable impurities, wherein the total amount of impurities is less than 0.02%. More preferably, the high-strength rare-earth magnesium alloy comprises the following elements in weight percentages: Gd 10–12.06%, Y 1.94–3%, Zn 0.94–1.51%, Mn 0.4–0.61%, with the balance being Mg and unavoidable impurities, wherein the total amount of impurities is less than 0.02%.

[0019] As a preferred embodiment, step A, the preparation of the high-strength rare-earth magnesium alloy semi-continuous casting ingot, includes the following steps:

[0020] Under a protective atmosphere, pure magnesium ingots are heated in a furnace at room temperature and melted at 650–720°C. The temperature is then raised to 680–700°C, pure Zn is added, and the temperature is raised to 740–760°C. Mg-Gd master alloy, Mg-Y master alloy, and Mg-Mn master alloy are added, and then the mixture is melted to form a melt.

[0021] The melt is refined at 740–750℃, then held at 770–790℃ for 15–25 minutes, and then cast into a high-strength rare earth magnesium alloy semi-continuous ingot at 710–730℃.

[0022] As a preferred embodiment, the protective atmosphere is a mixture of SF6 and CO2.

[0023] As a preferred embodiment, step B, the specific steps of the homogenization treatment, are as follows: A high-strength rare-earth magnesium alloy semi-continuous casting ingot is heated in a furnace at 2–4°C / min to 470–290°C and held for 1.5–2.5 hours, then heated at 2–4°C / min to 500–525°C and held for 10–25 hours, followed by quenching in water at 80–100°C to obtain a homogenized rare-earth magnesium alloy. The use of water at 80–100°C for quenching reduces the formation of coarse precipitates during air cooling, and the use of hot water reduces the risk of cracking in large-sized ingots.

[0024] As a preferred embodiment, in step C, the specific steps of differential temperature hot extrusion are as follows: The homogenized rare-earth magnesium alloy is preheated to 480–520°C in a furnace for preheating and holding before extrusion. After reaching the preset temperature, it is held for 30–120 minutes. The die is preheated to 320–450°C, and the extrusion cylinder is preheated to 400–450°C. Extrusion is performed at an extrusion ratio of 4–16 and an extrusion rate of 1–5 mm / s. After extrusion, the alloy is quenched in water at 10–30°C to obtain rare-earth magnesium alloy extruded bars or sheets. Quenching in water at 10–30°C can reduce the temperature of the bars or sheets exiting the extrusion outlet, reduce recrystallization, and prevent grain growth.

[0025] As a preferred embodiment, in the specific steps of the differential temperature hot extrusion, the extrusion ratio is 5 to 10 and the extrusion rate is 1 to 2 mm / s.

[0026] As a preferred embodiment, in step D, the total deformation of the multi-pass room temperature rotary forging is 8-20%, more preferably 12-20%.

[0027] As a preferred option, in step D, the deformation amount of the single-pass room temperature rotary forging is 1-4% during multi-pass room temperature rotary forging; the deformation amount of each pass of room temperature rotary forging is the same as or less than that of the previous pass of room temperature rotary forging.

[0028] As a preferred option, in step D, during multi-pass room temperature rotary forging, the feeding direction is changed after each pass of room temperature rotary forging to ensure a stable strain rate and achieve a larger deformation.

[0029] As a preferred embodiment, the multi-pass room temperature rotary forging involves 6 to 8 passes, wherein the deformation amount of at least 5 passes is reduced compared to the deformation amount of the previous pass. Previous experiments of this invention have shown that using too many or too few passes of room temperature rotary forging leads to a decrease in the properties of the magnesium alloy; the most preferred embodiment is 8 passes of room temperature rotary forging.

[0030] As a preferred embodiment, in step E, the conditions for the artificial aging treatment are: treatment at 175–250°C for 10–100 hours; more preferably, treatment at 200°C for 48–86 hours.

[0031] Secondly, the present invention provides a high-strength rare earth magnesium alloy prepared according to the aforementioned method.

[0032] The high-strength rare-earth magnesium alloy prepared by this invention has a tensile strength of 500–574 MPa, a yield strength of 456–545 MPa, and an elongation of 2.1–5.1% at room temperature. More preferably, the high-strength rare-earth magnesium alloy prepared by this invention has a tensile strength of 540–574 MPa and a yield strength of 508–545 MPa at room temperature.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] 1. The magnesium alloy of this invention optimizes the homogenization process after melting the alloy raw materials by adjusting elements such as Gd, Y, Zn, and Mn; performs hot extrusion and controls the extrusion temperature and extrusion ratio to regulate the recrystallization ratio and grain size; then performs rotary forging at room temperature, and reduces cracking caused by large deformation by controlling the deformation amount in a single pass and the total deformation amount in multiple passes; introduces a large number of dislocations and twins to improve the texture, enhance the aging strengthening ability, and improve the strength of the magnesium alloy.

[0035] 2. The high-strength rare earth magnesium alloy prepared by this invention has a tensile strength of 500-580 MPa at room temperature, which is higher and meets the urgent needs of aerospace, rail transportation, automobile and other fields for high-performance lightweight magnesium alloy materials.

[0036] 3. This invention involves rotary forging deformation at room temperature, resulting in a simple and flexible manufacturing process with adjustable and controllable microstructure and strength. It also requires low equipment specifications and has high production efficiency, making it suitable for large-scale continuous industrial production. Attached Figure Description

[0037] Other features, objects, and advantages of the invention will become more apparent from the following detailed description of non-limiting examples with reference to the accompanying drawings:

[0038] Figure 1 This is a schematic diagram of room temperature rotary forging of the high-strength rare-earth magnesium alloy of the present invention.

[0039] Figure 2 KAM diagram of the high-strength rare-earth magnesium alloy prepared in this invention;

[0040] Figure 3 The precipitation phase diagram of the high-strength rare-earth magnesium alloy prepared in this invention; wherein Figure 3 a represents the cylindrical nano-β' phase; Figure 3 b represents the basal plane γ' phase; Figure 3 a and Figure 3 The top right corner of diagram b shows the diffraction pattern of the corresponding region. Detailed Implementation

[0041] The present invention will be described in detail below with reference to specific examples. These examples will help those skilled in the art to further understand the invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0042] The raw materials used in the following embodiments are all obtained through conventional means, and the present invention does not impose any special limitations.

[0043] The performance tests conducted in the following examples are performed using the methods specified in GB / T 228.1-2010 "Metallic materials, tensile testing - Part 1: Test at room temperature".

[0044] Example 1

[0045] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0046] Gd: 12.06%, Y: 1.94%, Zn: 0.98%, Mn: 0.61%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0047] This embodiment is based on a method for preparing high-strength rare-earth magnesium alloys using a room-temperature rotary forging composite process, and includes the following steps:

[0048] (1) Material preparation: Prepare pure magnesium ingots, Mg-87Gd master alloy, Mg-70Y master alloy, pure Zn, and Mg3Mn master alloy according to the aforementioned alloy composition.

[0049] (2) Under a protective atmosphere of SF6 and CO2, pure magnesium ingots were heated in a furnace at room temperature and melted at 670°C. The temperature was then raised to 690°C, and pure Zn was added. The temperature was raised to 750°C, and Mg-87Gd, Mg-70Y, and Mg3Mn master alloys were slowly added, melting to form a molten body. Surface oxide scale and other impurities were removed, and the molten body was kept warm and stirred. The molten body was cooled to 750°C, and a refining agent (MgCl2 47.6%, KCl 37.4%, NaCl 12.5%, CaF2 2.5%, the total weight of the refining agent being 2% of the total weight of the alloy raw materials; unless otherwise specified, the refining agent in other examples and comparative examples is of this type) was added for refining treatment. The molten body was kept at 780°C for 20 minutes to allow impurities to fully precipitate. The molten body was then cooled to 710–730°C and cast into a semi-continuous ingot.

[0050] (3) After cooling, an ingot with a diameter of 95 mm is obtained by wire cutting.

[0051] (4) Homogenize the ingot obtained in step (3): After removing the oxide scale from the surface of the ingot, place it in a muffle furnace and heat it to 480°C at room temperature at 3°C / min and hold for 2 hours. Then heat it to 515°C at 3°C / min and hold for 15 hours. Then quench it in water at 90°C. Pyrite is placed in the muffle furnace to prevent the alloy from oxidizing and igniting.

[0052] (5) The homogenized ingot prepared in step (4) is subjected to differential hot extrusion: the homogenized alloy is heated to 500°C and held for 60 minutes in the furnace; the mold is preheated to 320°C; the extrusion cylinder is preheated to 400°C; the extrusion is carried out at an extrusion ratio of 5:1 and the extrusion rate is 2 mm / s; the extrusion cylinder is kept warm during the extrusion process; the extruded bar is immediately quenched in cold water.

[0053] (6) Rare earth magnesium alloy extruded bars with a diameter of 20 mm were obtained by wire cutting. The extruded magnesium alloy bars were then subjected to 8 passes of rotary forging at room temperature (e.g., ...). Figure 1 As shown, by adding shims, forging is performed with a radial compression of 0.1 to 0.4 mm per pass, and a deformation of 1% to 3% per pass. The deformation of each pass is the same as or less than that of the previous pass (the deformation of each pass is 3%, 2.1%, 1.4%, 1.3%, 1.2%, 1.2%, 1.1%, and 1% respectively). The feeding direction is changed after each pass of rotary forging, and finally a rod-shaped rare earth magnesium alloy material with a diameter of 18.7 mm is obtained, with a total deformation of 12.3%.

[0054] (7) The extruded-room temperature rotary forged rare earth magnesium alloy prepared in step (6) is subjected to artificial aging treatment at 200°C in an oil bath furnace for 64 hours.

[0055] (8) According to GB / T16865-2013, the high-strength rare-earth magnesium alloy prepared according to the above steps was subjected to a room temperature tensile test on a ZwickBTC-Z100 electronic universal testing machine at a tensile testing rate of 0.6 mm / min. The room temperature tensile strength of the alloy was 540 MPa, the yield strength was 508 MPa, and the elongation was 3.8%. The KAM diagram of the high-strength rare-earth magnesium alloy prepared in this embodiment is shown below. Figure 2 As shown, by Figure 2 As can be seen, the alloy maintains a bimodal structure, and the dislocation density of the recrystallized grains increases significantly. TEM observation of the precipitated phases of the high-strength rare-earth magnesium alloy prepared in this embodiment shows... Figure 3 As shown, the main precipitated phase in the alloy is the cylindrical nano-β' phase ( Figure 3 a) Phase with basal plane γ' ( Figure 3 b) The precipitated phases are fine and dense, forming a network structure, which together improves the strength and plasticity of the alloy.

[0056] Example 2

[0057] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0058] Gd: 12.06%, Y: 1.94%, Zn: 0.94%, Mn: 0.61%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0059] This embodiment is based on a method for preparing high-strength rare-earth magnesium alloys using a room-temperature rotary forging composite process, and includes the following steps:

[0060] (1) Material preparation: Prepare pure magnesium ingots, Mg-87Gd master alloy, Mg-70Y master alloy, pure Zn, and Mg3Mn master alloy according to the aforementioned alloy composition.

[0061] (2) Under a protective atmosphere of SF6 and CO2, pure magnesium ingots are heated in a furnace at room temperature and melted at 670°C. The temperature is then raised to 690°C, and pure Zn is added. The temperature is raised to 750°C, and Mg-87Gd, Mg-70Y, and Mg3Mn master alloys are slowly added, melting to form a molten body. Surface oxide scale and other impurities are removed, and the molten body is held at this temperature while being stirred. The molten body is cooled to 750°C, and a refining agent is added for refining. The molten body is held at 780°C for 20 minutes to allow impurities to fully precipitate. When the molten body cools to 710–730°C, it is poured into a semi-continuous ingot.

[0062] (3) After cooling, an ingot with a diameter of 95 mm is obtained by wire cutting.

[0063] (4) Homogenize the ingot obtained in step (3): After removing the oxide scale from the surface of the ingot, place it in a muffle furnace and heat it to 480°C at room temperature at 3°C / min and hold for 2 hours. Then heat it to 515°C at 3°C / min and hold for 15 hours. Then quench it in water at 90°C. Pyrite is placed in the muffle furnace to prevent the alloy from oxidizing and igniting.

[0064] (5) The homogenized ingot prepared in step (4) is subjected to differential hot extrusion: the homogenized alloy is heated to 500°C and held for 60 minutes in the furnace; the mold is preheated to 350°C; the extrusion cylinder is preheated to 400°C; extrusion is carried out at an extrusion ratio of 10:1 and the extrusion rate is 1 mm / s; the extrusion cylinder is kept warm during the extrusion process; the extruded bar is immediately quenched in cold water.

[0065] (6) Rare earth magnesium alloy extruded bars with a diameter of 20 mm were obtained by wire cutting. At room temperature, the extruded magnesium alloy bars were subjected to 8 passes of rotary forging deformation. The radial compression of each pass was 0.1 to 0.4 mm, and the deformation of each pass was 1% to 3%. The deformation of each pass was the same as or reduced compared to the previous pass (the deformation of each pass was 3%, 2.1%, 1.4%, 1.3%, 1.2%, 1.2%, 1.1%, and 1% respectively). The feeding direction was changed after each pass of rotary forging, and finally, a rod-shaped rare earth magnesium alloy material with a diameter of 18.7 mm was obtained, with a total deformation of 12.3%.

[0066] (7) The extruded-room temperature rotary forged rare earth magnesium alloy prepared in step (6) is subjected to artificial aging treatment at 200°C in an oil bath furnace for 64 hours.

[0067] (8) According to GB / T16865-2013, the high-strength rare-earth magnesium alloy prepared according to the above steps was subjected to a room temperature tensile test on a ZwickBTC-Z100 electronic universal testing machine at a tensile test rate of 0.6 mm / min. The room temperature tensile strength of the alloy was 574 MPa, the yield strength was 545 MPa, and the elongation was 2.6%.

[0068] Example 3

[0069] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0070] Gd: 10.02%, Y: 2.98%, Zn: 0.96%, Mn: 0.60%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0071] This embodiment is based on a method for preparing high-strength rare-earth magnesium alloys using a room-temperature rotary forging composite process, and includes the following steps:

[0072] (1) Material preparation: Prepare pure magnesium ingots, Mg-87Gd master alloy, Mg-70Y master alloy, pure Zn, and Mg3Mn master alloy according to the aforementioned alloy composition.

[0073] (2) Under a protective atmosphere of SF6 and CO2, pure magnesium ingots are heated in a furnace at room temperature and melted at 670°C. The temperature is then raised to 690°C, and pure Zn is added. The temperature is raised to 750°C, and Mg-87Gd, Mg-70Y, and Mg3Mn master alloys are slowly added, melting to form a molten body. Surface oxide scale and other impurities are removed, and the molten body is held at this temperature while being stirred. The molten body is cooled to 750°C, and a refining agent is added for refining. The molten body is held at 780°C for 20 minutes to allow impurities to fully precipitate. When the molten body cools to 710–730°C, it is poured into a semi-continuous ingot.

[0074] (3) After cooling, an ingot with a diameter of 95 mm is obtained by wire cutting.

[0075] (4) Homogenize the ingot obtained in step (3): After removing the oxide scale from the surface of the ingot, place it in a muffle furnace and heat it to 480°C at room temperature at 3°C / min and hold for 2 hours. Then heat it to 515°C at 3°C / min and hold for 15 hours. Then quench it in water at 90°C. Pyrite is placed in the muffle furnace to prevent the alloy from oxidizing and igniting.

[0076] (5) The homogenized ingot prepared in step (4) is subjected to differential hot extrusion: the homogenized alloy is heated to 500°C and held for 60 minutes in the furnace; the mold is preheated to 320°C; the extrusion cylinder is preheated to 400°C; the extrusion is carried out at an extrusion ratio of 5:1 and the extrusion rate is 2 mm / s; the extrusion cylinder is kept warm during the extrusion process; the extruded bar is immediately quenched in cold water.

[0077] (6) Rare earth magnesium alloy extruded bars with a diameter of 20 mm were obtained by wire cutting. At room temperature, the extruded magnesium alloy bars were subjected to 8 passes of rotary forging deformation. The radial compression of each pass was 0.1 to 0.4 mm, and the deformation of each pass was 1% to 3%. The deformation of each pass was the same as or reduced compared to the previous pass (the deformation of each pass was 3%, 2.1%, 1.4%, 1.3%, 1.2%, 1.2%, 1.1%, and 1% respectively). The feeding direction was changed after each pass of rotary forging, and finally, a rod-shaped rare earth magnesium alloy material with a diameter of 18.7 mm was obtained, with a total deformation of 12.3%.

[0078] (7) The extruded-room temperature rotary forged rare earth magnesium alloy prepared in step (6) is subjected to artificial aging treatment at 200°C in an oil bath furnace for 64 hours.

[0079] (8) According to GB / T16865-2013, the high-strength rare-earth magnesium alloy prepared according to the above steps was subjected to a room temperature tensile test on a ZwickBTC-Z100 electronic universal testing machine at a tensile testing rate of 0.6 mm / min. The room temperature tensile strength of the alloy was 547 MPa, the yield strength was 511 MPa, and the elongation was 3.6%.

[0080] Example 4

[0081] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0082] Gd: 8.07%, Y: 3.99%, Zn: 1.02%, Mn: 0.63%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0083] This embodiment is based on a method for preparing high-strength rare-earth magnesium alloys using a room-temperature rotary forging composite process, and includes the following steps:

[0084] (1) Material preparation: Prepare pure magnesium ingots, Mg-87Gd master alloy, Mg-70Y master alloy, pure Zn, and Mg3Mn master alloy according to the aforementioned alloy composition.

[0085] (2) Under a protective atmosphere of SF6 and CO2, pure magnesium ingots are heated in a furnace at room temperature and melted at 650–720°C. The temperature is then raised to 690°C, and pure Zn is added. The temperature is raised to 750°C, and Mg-87Gd, Mg-70Y, and Mg3Mn master alloys are slowly added, melting to form a molten body. Surface oxide scale and other impurities are removed, and the molten body is held at this temperature while being stirred. The molten body is cooled to 750°C, and a refining agent is added for refining. The molten body is held at 780°C for 20 minutes to allow impurities to fully precipitate. The molten body is then cooled to 710–730°C and cast into a semi-continuous ingot.

[0086] (3) After cooling, an ingot with a diameter of 95 mm is obtained by wire cutting.

[0087] (4) Homogenize the ingot obtained in step (3): After removing the oxide scale from the surface of the ingot, place it in a muffle furnace and heat it to 480°C at room temperature at 3°C / min and hold for 2 hours. Then heat it to 515°C at 3°C / min and hold for 15 hours. Then quench it in water at 90°C. Pyrite is placed in the muffle furnace to prevent the alloy from oxidizing and igniting.

[0088] (5) The homogenized ingot prepared in step (4) is subjected to differential hot extrusion: the homogenized alloy is heated to 500°C and held for 60 minutes; the mold is preheated to 320°C; the extrusion cylinder is preheated to 400°C; the extrusion is carried out at an extrusion ratio of 9:1 and the extrusion rate is 1 mm / s; the extrusion cylinder is kept warm during the extrusion process; the extruded bar is immediately quenched in cold water.

[0089] (6) Rare earth magnesium alloy extruded bars with a diameter of 20 mm were obtained by wire cutting. At room temperature, the extruded magnesium alloy bars were subjected to 8 passes of rotary forging deformation. The radial compression of each pass was 0.1 to 0.4 mm, and the deformation of each pass was 1.3% to 4%. The deformation of each pass was the same as or reduced compared to the previous pass (the deformation of each pass was 4%, 3.5%, 3%, 2.5%, 2%, 2%, 1.5%, and 1.3% respectively). The feeding direction was changed after each pass of rotary forging. Finally, a rod-shaped rare earth magnesium alloy material with a diameter of 17.9 mm was obtained, and the total deformation was 19.8%.

[0090] (7) The extruded-room temperature rotary forged rare earth magnesium alloy prepared in step (6) is subjected to artificial aging treatment at 200°C in an oil bath furnace for 48 hours.

[0091] (8) According to GB / T16865-2013, the high-strength rare-earth magnesium alloy prepared according to the above steps was subjected to a room temperature tensile test on a ZwickBTC-Z100 electronic universal testing machine at a tensile testing rate of 0.6 mm / min. The room temperature tensile strength of the alloy was 509 MPa, the yield strength was 464 MPa, and the elongation was 4.8%.

[0092] Example 5

[0093] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0094] Gd: 8.05%, Y: 3.97%, Zn: 0.52%, Mn: 0.61%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0095] This embodiment is based on a method for preparing high-strength rare-earth magnesium alloys using a room-temperature rotary forging composite process, and includes the following steps:

[0096] (1) Material preparation: Prepare pure magnesium ingots, Mg-87Gd master alloy, Mg-70Y master alloy, pure Zn, and Mg3Mn master alloy according to the aforementioned alloy composition.

[0097] (2) Under a protective atmosphere of SF6 and CO2, pure magnesium ingots are heated in a furnace at room temperature and melted at 670°C. The temperature is then raised to 690°C, and pure Zn is added. The temperature is raised to 750°C, and Mg-87Gd, Mg-70Y, and Mg3Mn master alloys are slowly added, melting to form a molten body. Surface oxide scale and other impurities are removed, and the molten body is held at this temperature while being stirred. The molten body is cooled to 750°C, and a refining agent is added for refining. The molten body is held at 780°C for 20 minutes to allow impurities to fully precipitate. When the molten body cools to 710–730°C, it is poured into a semi-continuous ingot.

[0098] (3) After cooling, an ingot with a diameter of 95 mm is obtained by wire cutting.

[0099] (4) Homogenize the ingot obtained in step (3): After removing the oxide scale from the surface of the ingot, place it in a muffle furnace and heat it to 480°C at room temperature at 3°C / min and hold for 2 hours. Then heat it to 515°C at 3°C / min and hold for 15 hours. Then quench it in water at 90°C. Pyrite is placed in the muffle furnace to prevent the alloy from oxidizing and igniting.

[0100] (5) The homogenized ingot prepared in step (4) is subjected to differential hot extrusion: the homogenized alloy is heated to 500°C and held for 60 minutes; the mold is preheated to 320°C; the extrusion cylinder is preheated to 400°C; the extrusion is carried out at an extrusion ratio of 9:1 and the extrusion rate is 1 mm / s; the extrusion cylinder is kept warm during the extrusion process; the extruded bar is immediately quenched in cold water.

[0101] (6) Rare earth magnesium alloy extruded bars with a diameter of 20 mm were obtained by wire cutting. At room temperature, the extruded magnesium alloy bars were subjected to 8 passes of rotary forging deformation. The radial compression of each pass was 0.1 to 0.4 mm, and the deformation of each pass was 1.3% to 4%. The deformation of each pass was the same as or reduced compared to the previous pass (the deformation of each pass was 4%, 3.5%, 3%, 2.5%, 2%, 2%, 1.5%, and 1.3% respectively). The feeding direction was changed after each pass of rotary forging. Finally, a rod-shaped rare earth magnesium alloy material with a diameter of 17.9 mm was obtained, and the total deformation was 19.8%.

[0102] (7) The extruded-room temperature rotary forged rare earth magnesium alloy prepared in step (6) is subjected to artificial aging treatment at 200°C in an oil bath furnace for 48 hours.

[0103] (8) According to GB / T16865-2013, the high-strength rare-earth magnesium alloy prepared according to the above steps was subjected to a room temperature tensile test on a ZwickBTC-Z100 electronic universal testing machine at a tensile testing rate of 0.6 mm / min. The room temperature tensile strength of the alloy was 507 MPa, the yield strength was 456 MPa, and the elongation was 5.1%.

[0104] Example 6

[0105] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0106] Gd: 14.02%, Y: 3.95%, Zn: 1.01%, Mn: 0.59%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0107] This embodiment is based on a method for preparing high-strength rare-earth magnesium alloys using a room-temperature rotary forging composite process, including the following steps:

[0108] (1) Material preparation: Prepare pure magnesium ingots, Mg-87Gd master alloy, Mg-70Y master alloy, pure Zn, and Mg3Mn master alloy according to the aforementioned alloy composition.

[0109] (2) Under a protective atmosphere of SF6 and CO2, pure magnesium ingots are heated in a furnace at room temperature and melted at 670°C. The temperature is then raised to 690°C, and pure Zn is added. The temperature is raised to 750°C, and Mg-87Gd, Mg-70Y, and Mg3Mn master alloys are slowly added, melting to form a molten body. Surface oxide scale and other impurities are removed, and the molten body is held at this temperature while being stirred. The molten body is cooled to 750°C, and a refining agent is added for refining. The molten body is held at 780°C for 20 minutes to allow impurities to fully precipitate. When the molten body cools to 710–730°C, it is poured into a semi-continuous ingot.

[0110] (3) After cooling, an ingot with a diameter of 95 mm is obtained by wire cutting.

[0111] (4) Homogenize the ingot obtained in step (3): After removing the oxide scale from the surface of the ingot, place it in a muffle furnace and heat it to 480°C at room temperature at 3°C / min and hold for 2 hours. Then heat it to 515°C at 3°C / min and hold for 15 hours. Then quench it in water at 90°C. Pyrite is placed in the muffle furnace to prevent the alloy from oxidizing and igniting.

[0112] (5) The homogenized ingot prepared in step (4) is subjected to differential hot extrusion: the homogenized alloy is heated to 500°C and held for 60 minutes in the furnace; the mold is preheated to 370°C; the extrusion cylinder is preheated to 400°C; the extrusion is carried out at an extrusion ratio of 5:1 and the extrusion rate is 1 mm / s; the extrusion cylinder is kept warm during the extrusion process; the extruded bar is immediately quenched in cold water.

[0113] (6) Rare earth magnesium alloy extruded bars with a diameter of 20 mm were obtained by wire cutting. At room temperature, the extruded magnesium alloy bars were subjected to 8 passes of rotary forging deformation. The radial compression of each pass was 0.1 to 0.4 mm, and the deformation of each pass was 1% to 4%. The deformation of each pass was the same as or reduced compared to the previous pass (the deformation of each pass was 1.1%, 1%, 1%, 1%, 1%, 1%, 1%, 1%, 1%). The feeding direction was changed after each pass of rotary forging. Finally, a rod-shaped rare earth magnesium alloy material with a diameter of 19.2 mm was obtained, and the total deformation was 8.1%.

[0114] (7) The extruded-room temperature rotary forged rare earth magnesium alloy prepared in step (6) is subjected to artificial aging treatment at 200°C in an oil bath furnace for 86 hours.

[0115] (8) According to GB / T16865-2013, the high-strength rare-earth magnesium alloy prepared according to the above steps was subjected to a room temperature tensile test on a ZwickBTC-Z100 electronic universal testing machine at a tensile testing rate of 0.6 mm / min. The room temperature tensile strength of the alloy was 522 MPa, the yield strength was 498 MPa, and the elongation was 3.2%.

[0116] Example 7

[0117] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0118] Gd: 12.04%, Y: 1.94%, Zn: 0.94%, Mn: 0.42%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0119] The preparation method of the high-strength rare-earth magnesium alloy based on the room temperature rotary forging composite process in this embodiment is the same as that in Example 2. The obtained high-strength rare-earth magnesium alloy has a room temperature tensile strength of 564 MPa, a yield strength of 530 MPa, and an elongation of 2.7%.

[0120] Example 8

[0121] The high-strength rare-earth magnesium alloy provided in this embodiment has the following alloy composition (by weight percentage):

[0122] Gd: 12.06%, Y: 1.96%, Zn: 1.51%, Mn: 0.62%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0123] The preparation method of the high-strength rare-earth magnesium alloy based on the room temperature rotary forging composite process in this embodiment is the same as that in Example 2. The obtained high-strength rare-earth magnesium alloy has a room temperature tensile strength of 569 MPa, a yield strength of 538 MPa, and an elongation of 2.4%.

[0124] Example 9

[0125] The high-strength rare earth magnesium alloy provided in this embodiment has the same alloy composition (weight percentage) as in Example 2.

[0126] This embodiment describes a method for preparing a high-strength rare-earth magnesium alloy using a room-temperature rotary forging composite process. The method is essentially the same as that used in Example 2, except that in step (6), the deformation amount in each rotary forging pass is either the same as or reduced compared to the previous pass, specifically 1.8%, 1.8%, 1.8%, 1.8%, 1.3%, 1.3%, 1.3%, and 1.2%, respectively. The total deformation amount is the same as in Example 2. The resulting high-strength rare-earth magnesium alloy has a room-temperature tensile strength of 549 MPa, a yield strength of 521 MPa, and an elongation of 3.2%.

[0127] Example 10

[0128] The high-strength rare earth magnesium alloy provided in this embodiment has the same alloy composition (weight percentage) as in Example 2.

[0129] This embodiment describes a method for preparing high-strength rare-earth magnesium alloy using a room-temperature rotary forging composite process. The method is essentially the same as that used in Example 2, except that in step (6), the extruded magnesium alloy bar undergoes six passes of rotary forging deformation. The deformation amount in each pass gradually decreases, successively at 3%, 2.5%, 2%, 1.8%, 1.6%, and 1.4%, with the total deformation amount remaining the same as in Example 2. The resulting high-strength rare-earth magnesium alloy exhibits a room-temperature tensile strength of 546 MPa, a yield strength of 530 MPa, and an elongation of 2.1%.

[0130] Example 11

[0131] The high-strength rare earth magnesium alloy provided in this embodiment has the same alloy composition (weight percentage) as in Example 6.

[0132] This embodiment describes a method for preparing a high-strength rare-earth magnesium alloy using a room-temperature rotary forging composite process. The method is essentially the same as that used in Example 6, except that in step (6), the forging is performed with a radial compression of 0.1 mm per pass, a deformation of 1% per pass, and the same deformation for each pass (the deformation per pass is 1%, 1%, 1%, 1%, 1%, 1%, 1%), for a total deformation of 6%. The resulting high-strength rare-earth magnesium alloy has a room-temperature tensile strength of 500 MPa, a yield strength of 472 MPa, and an elongation of 3.3%.

[0133] Comparative Example 1

[0134] The high-strength rare-earth magnesium alloy provided in this comparative example has the following alloy composition (by weight percentage):

[0135] Gd: 12.06%, Y: 1.94%, Mn: 0.61%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0136] This comparative example uses a method similar to that used in Example 1 for preparing a high-strength rare-earth magnesium alloy based on a room-temperature rotary forging composite process. The only difference is that pure Zn was not added in step (1) of this comparative example. The resulting high-strength rare-earth magnesium alloy has a room-temperature tensile strength of 477 MPa, a yield strength of 424 MPa, and an elongation of 5.1%. Compared with Example 1, the room-temperature strength of the alloy is significantly reduced. The difference lies in the absence of the Zn-containing LPSO structural phase and the basal nano-γ' phase, which reduces the strengthening effect of the alloy.

[0137] Comparative Example 2

[0138] The high-strength rare-earth magnesium alloy provided in this comparative example has the same alloy composition (weight percentage) as that in Example 1.

[0139] This comparative example is based on a high-strength rare earth magnesium alloy preparation method using a room temperature rotary forging composite process. The preparation method is basically the same as that used in Example 1, except that in the preparation process, in step (6), the radial compression of each pass is 0.8 mm, and the deformation of each pass is 8%. Due to the large deformation of each pass, the rare earth magnesium alloy bar cracked after the third rotary forging pass and could not be rotary forged.

[0140] Comparative Example 3

[0141] The high-strength rare-earth magnesium alloy provided in this comparative example has the same alloy composition (weight percentage) as that in Example 1.

[0142] This comparative example demonstrates a method for preparing a high-strength rare-earth magnesium alloy using a room-temperature rotary forging composite process. The method is essentially the same as that used in Example 1, except that step (6) is omitted. The resulting high-strength rare-earth magnesium alloy exhibits a room-temperature tensile strength of 465 MPa, a yield strength of 393 MPa, and an elongation of 5.2%. Compared to Example 1, the room-temperature strength of the alloy is significantly reduced. This is because the room-temperature rotary forging process is absent, resulting in fewer defects such as dislocations and twins within the alloy, and a decrease in its age-hardening ability.

[0143] Comparative Example 4

[0144] The high-strength rare-earth magnesium alloy provided in this comparative example has the following alloy composition (by weight percentage):

[0145] Gd: 12.06%, Y: 1.94%, Zn: 4.02%, Mn: 0.61%, with the remainder being magnesium and unavoidable impurities, the total content of which is less than 0.02%.

[0146] This comparative example demonstrates the preparation method of a high-strength rare-earth magnesium alloy based on a room-temperature rotary forging composite process, which is the same as the preparation method used in Example 1. The obtained high-strength rare-earth magnesium alloy has a room-temperature tensile strength of 484 MPa, a yield strength of 463 MPa, and an elongation of 3.2%. Compared with Example 1, the room-temperature strength of the alloy is significantly reduced. The difference lies in the excessive LPSO structural phase formed by the added Zn element and rare-earth elements Gd and Y, which consumes a large amount of Gd and Y solutes, reducing the strengthening effect during the subsequent artificial aging process.

[0147] Comparative Example 5

[0148] The high-strength rare-earth magnesium alloy provided in this comparative example has the same alloy composition (weight percentage) as that in Example 1.

[0149] This comparative example demonstrates a preparation method for a high-strength rare-earth magnesium alloy based on a room-temperature rotary forging composite process. This method is essentially the same as that used in Example 1, with the only difference being that in step (5), the homogenized alloy is heated to 400°C and held for 60 minutes; the mold is preheated to 400°C. The resulting high-strength rare-earth magnesium alloy exhibits a room-temperature tensile strength of 479 MPa, a yield strength of 427 MPa, and an elongation of 2.2%. Compared to Example 1, the room-temperature strength of the alloy is significantly reduced. The difference lies in the fact that holding at 400°C causes some solute to precipitate, reducing the strengthening effect during subsequent artificial aging; simultaneously, the increased extrusion temperature coarsens the grains in the extruded alloy, reducing its performance.

[0150] Comparative Example 6

[0151] The high-strength rare-earth magnesium alloy provided in this comparative example has the same alloy composition (weight percentage) as that in Example 5.

[0152] This comparative example demonstrates a method for preparing a high-strength rare-earth magnesium alloy using a room-temperature rotary forging composite process. The method is essentially the same as that used in Example 5, except that in step (6), the radial compression in each pass is 0.15 mm to 0.4 mm, the deformation per pass is 1.5% to 4%, and the deformation per pass gradually decreases (the deformation per pass is 4%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, and 1.5% respectively), with a total deformation of 22%. The resulting high-strength rare-earth magnesium alloy exhibits a room-temperature tensile strength of 487 MPa, a yield strength of 467 MPa, and an elongation of 0.9%.

[0153] Comparative Example 7

[0154] The high-strength rare-earth magnesium alloy provided in this comparative example has the same alloy composition (weight percentage) as that in Example 5.

[0155] This comparative example demonstrates a method for preparing a high-strength rare-earth magnesium alloy using a room-temperature rotary forging composite process. The method is essentially the same as that used in Example 5, except that in step (6), the radial compression in each pass is 0.1 mm to 0.6 mm, the deformation per pass is 1% to 6%, and the deformation per pass gradually decreases (the deformation per pass is 6%, 4%, 3%, 2%, 1.4%, 1.4%, 1%, and 1%), with a total deformation of 19.8%. The resulting high-strength rare-earth magnesium alloy exhibits a room-temperature tensile strength of 477 MPa, a yield strength of 449 MPa, and an elongation of 1.1%.

[0156] The above description of the embodiments is provided to enable those skilled in the art to understand and use the present invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for preparing high-strength rare-earth magnesium alloy based on a room-temperature rotary forging composite process, characterized in that, The method includes the following steps: A. Prepare high-strength rare earth magnesium alloy semi-continuous casting ingots according to preset composition; B. Homogenize the magnesium alloy semi-continuous casting ingot at 480-525℃ to obtain homogenized rare earth magnesium alloy. C. The homogenized rare earth magnesium alloy is subjected to differential temperature hot extrusion to obtain rare earth magnesium alloy extruded bars or plates; the temperature of the homogenized rare earth magnesium alloy used in the differential temperature hot extrusion is 450-520℃, the temperature of the extrusion die is 320-450℃, and the extrusion ratio is 4-16. D. Perform multi-pass room temperature rotary forging on rare earth magnesium alloy extruded bars or plates to obtain forged bars or plates; the total deformation of the multi-pass room temperature rotary forging is 4-20%. E. Artificial aging treatment is performed on the forged bars or plates to obtain the high-strength rare earth magnesium alloy.

2. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 1, characterized in that, In step A, the high-strength rare-earth magnesium alloy contains the following elements in weight percentages: Gd 8-18%, Y 1.94-4%, Zn 0.5-2.0%, Mn 0-1%, with the balance being Mg and unavoidable impurities, wherein the total amount of impurities is less than 0.02%.

3. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 2, characterized in that, The high-strength rare-earth magnesium alloy contains the following elements in weight percentages: Gd 8-14.02%, Y 1.94-4%, Zn 0.5-1.51%, Mn 0.4-1%, with the balance being Mg and unavoidable impurities, wherein the total amount of impurities is less than 0.02%.

4. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 2 or 3, characterized in that, In step A, the preparation of the high-strength rare-earth magnesium alloy semi-continuous casting ingot includes the following steps: Under a protective atmosphere, pure magnesium ingots are heated in a furnace at room temperature and melted at 650–720°C. The temperature is then raised to 680–700°C, pure Zn is added, and the temperature is raised to 740–760°C. Mg-Gd master alloy, Mg-Y master alloy, and Mg3Mn master alloy are added, and then the mixture is melted to form a melt. The melt is refined at 740–750℃, then held at 770–790℃ for 15–25 minutes, and then cast into a high-strength rare earth magnesium alloy semi-continuous ingot at 710–730℃.

5. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 1, characterized in that, In step B, the specific steps of the homogenization treatment are as follows: the high-strength rare earth magnesium alloy semi-continuous casting ingot is heated to 470-290℃ at room temperature at 2-4℃ / min and held for 1.5-2.5h, then heated to 500-525℃ at 2-4℃ / min and held for 10-25h, and then quenched in water at 80-100℃ to obtain homogenized rare earth magnesium alloy.

6. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 1, characterized in that, In step C, the specific steps of differential temperature hot extrusion are as follows: the homogenized rare earth magnesium alloy is heated to 480-520℃ in the furnace for preheating and heat preservation before extrusion. After reaching the preset temperature, it is kept at the temperature for 30-120 minutes; the die is preheated to 320-450℃ and the extrusion cylinder is preheated to 400-450℃, and extrusion is carried out at an extrusion ratio of 4-16 with an extrusion rate of 1-5 mm / s; after extrusion, it is quenched in water at 10-30℃ to obtain rare earth magnesium alloy extruded bars or plates.

7. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 1, characterized in that, In step D, during multi-pass room temperature rotary forging, the deformation amount of a single-pass room temperature rotary forging is 1-4%; the deformation amount of each pass of room temperature rotary forging is the same as or less than that of the previous pass.

8. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 1, characterized in that, In step D, during the multi-pass room temperature rotary forging, the feeding direction is changed after each pass of room temperature rotary forging.

9. The method for preparing high-strength rare-earth magnesium alloy based on room temperature rotary forging composite process according to claim 1, characterized in that, In step E, the conditions for the artificial aging treatment are: treatment at 175–250°C for 10–100 hours.

10. A high-strength rare-earth magnesium alloy prepared by the method according to any one of claims 1-9.

Citation Information

Patent Citations

  • A high-strength cast magnesium alloy containing Zn and heavy rare earth element Gd and its preparation method

    CN105483485B

  • Aging heat treatment process for VW93M nano heterogeneous magnesium alloy

    CN108707848A