A method for preparing and applying graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles

The graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles were prepared by a dual-feed atomization drying and microwave reduction synergistic process, which solved the problems of uneven metal ion mixing, particle agglomeration and poor loading stability in the existing technology, and achieved high efficiency and stable catalytic performance, which is suitable for the field of water electrolysis.

CN122077008APending Publication Date: 2026-05-26NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610234796.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-27
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

Existing methods for preparing graphene-loaded high-entropy nanoparticles suffer from problems such as uneven mixing of metal ions, particle agglomeration, poor loading stability, and long preparation cycles, which limit their industrial application.

Method used

A dual-feed atomization drying and microwave reduction synergistic process was adopted. The dual-feed atomization drying equipment realizes the instantaneous mixing and atomization of metal ions on the graphene surface, and combined with microwave reduction technology for rapid and uniform loading, so as to prepare graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles with uniform particle size and pure phase.

Benefits of technology

Uniform and stable loading of metal ions on the graphene surface was achieved, resulting in the preparation of high-entropy nanoparticles with excellent catalytic performance. This shortened the preparation cycle, reduced energy consumption, and improved loading stability and catalytic activity, making them suitable for industrial applications in water electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122077008A_ABST
    Figure CN122077008A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles. The method includes: dissolving iridium, ruthenium, cobalt, copper, and nickel metal salts in an equiatomic ratio to prepare a metal precursor solution; simultaneously preparing a graphene oxide dispersion; and then mixing and atomizing the dispersion using a dual-feed atomization drying device to obtain a composite precursor powder. Finally, the powder is subjected to microwave reduction under inert gas protection to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles. This invention employs a synergistic process of dual-feed atomization and microwave reduction, avoiding metal ion aggregation and elemental segregation, achieving uniform and stable loading of high-entropy nanoparticles on the graphene surface. The high-entropy nanoparticles have a single-phase face-centered cubic structure with a particle size of 8 nm to 25 nm. The process is simple, efficient, low-consumption, and allows for controllable proportions. The prepared graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles can be widely used in water electrolysis, exhibiting advantages such as low overpotential and high stability, making them suitable for large-scale production and industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nanomaterial preparation and electrocatalysis technology, specifically relating to a method for preparing and applying graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles. Background Technology

[0002] With the growing prominence of the global energy crisis and environmental issues, water electrolysis for hydrogen production, as a clean and sustainable hydrogen energy production technology, has attracted widespread attention. The catalyst is the core component of the water electrolysis system, and its performance directly determines the energy conversion efficiency, stability, and industrial feasibility of water electrolysis.

[0003] High-entropy nanoparticles exhibit excellent catalytic activity and structural stability in electrocatalysis due to their multi-element synergistic effect, high-entropy stabilization effect, and lattice distortion effect. Compared with traditional single-component or binary alloy catalysts, they can effectively optimize the adsorption-desorption energy barrier of reaction intermediates and improve catalytic kinetic rates. Iridium and ruthenium-based materials are highly efficient catalytic components for water electrolysis, while cobalt, copper, and nickel can regulate the electronic structure of the catalyst and reduce the amount of precious metals used. Constructing high-entropy nanoparticles with these five elements can achieve a balance between activity, stability, and cost. Graphene, due to its ultra-large specific surface area, excellent conductivity, and good chemical stability, is often used as a catalyst support to disperse nanoparticles, prevent their aggregation, and accelerate electron transport. Existing methods for preparing graphene-supported high-entropy nanoparticles mostly employ processes such as wet chemical soaking and solvothermal reduction, which suffer from problems such as uneven mixing of metal ions and graphene, severe particle aggregation, poor loading stability, and long preparation cycles, limiting their industrial application.

[0004] Dual-feed atomization drying technology enables independent feeding, instant mixing, and rapid atomization curing of two materials, effectively avoiding metal ion agglomeration and elemental segregation. Microwave reduction offers advantages such as uniform heating, high speed, and low energy consumption, promoting the in-situ reduction of metal ions on the graphene surface to form high-entropy nanoparticles and strengthening the bond between particles and the carrier. However, there are currently no reports on combining dual-feed atomization drying with microwave reduction processes to prepare graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles. To address the shortcomings of existing technologies, such as uneven metal ion mixing, particle agglomeration, poor loading stability, and long preparation cycles, this invention proposes a dual-feed atomization drying synergistic with microwave reduction method, aiming to solve these problems and achieve uniform and stable loading of high-entropy nanoparticles on the graphene surface. Summary of the Invention

[0005] The technical problem to be solved by this invention is to address the shortcomings of the prior art by providing a method for preparing graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles. This method employs a dual-feed atomization drying and microwave reduction synergistic process to achieve uniform and stable loading of metal ions on the graphene surface, thus preparing graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles with uniform particle size, pure phase, and excellent catalytic performance.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles, characterized in that the method includes the following steps: Step 1: Dissolve iridium salt, ruthenium salt, cobalt salt, copper salt, and nickel salt in a solvent at an equiatomic ratio and stir until homogeneous to obtain a metal precursor solution with a total metal ion concentration of 0.01 mol / L to 0.02 mol / L; disperse graphene oxide powder in water and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 2 mg / mL to 10 mg / mL. Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into the two independent feed channels of the dual-feed atomizing dryer. They are mixed in the atomizing chamber and then atomized into tiny droplets. After drying in the drying chamber, graphene-loaded metal ion composite precursor powder with a size of 1μm~2μm is collected. Step 3: Place the graphene-loaded metal ion composite precursor powder obtained in Step 2 into a microwave reduction device and perform microwave reduction treatment under an inert gas atmosphere to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

[0007] The above-mentioned method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles is characterized in that, in step one, the iridium salt is at least one of iridium chloride, ammonium chloroiridate, iridium acetate, and iridium tetrachloride hydrate; the ruthenium salt is at least one of ruthenium chloride, ammonium chloroiridate, and ruthenium acetate; the cobalt salt is at least one of cobalt acetate tetrahydrate, cobalt chloride hexahydrate, and anhydrous cobalt chloride; the copper salt is at least one of copper chloride dihydrate, anhydrous copper chloride, cuprous chloride, and anhydrous copper sulfate; and the nickel salt is at least one of anhydrous nickel chloride, nickel chloride hexahydrate, and anhydrous nickel sulfate.

[0008] The above-mentioned method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles is characterized in that, in step two, the feed flow ratio of the metal precursor solution to the graphene oxide dispersion is 1:1~4, and the flow control accuracy is ±0.5%. This invention regulates the feed rate of two independent feed channels using a dual-channel precision metering pump. By controlling the feed flow ratio of the metal precursor solution to the graphene oxide dispersion to be 1:1~4, and combining this with density parameter calibration, the density of the metal precursor solution is 1.0 g / cm³. 3 ~1.03g / cm3 The density of the graphene oxide dispersion is 1.0 g / cm³. 3 ~1.05g / cm 3 This allows for precise control of the mass ratio of metal element loading to graphene, which is 1:1 to 2.

[0009] The above-described method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles is characterized in that the atomization pressure of the dual-feed atomizing drying equipment in step two is 0.2 MPa to 0.4 MPa, and the drying temperature is 160℃ to 220℃. This invention ensures rapid solidification of droplets to form a uniform composite precursor by controlling the atomization pressure and drying temperature, thus avoiding metal ion segregation.

[0010] The above-mentioned method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles is characterized in that, in step three, the microwave reduction treatment uses a microwave power of 800W~1200W for 5min~20min, and the temperature after microwave reduction treatment is 300℃~500℃; the inert gas is nitrogen or argon, and the flow rate is 40mL / min~60mL / min. This invention avoids particle aggregation and lattice distortion caused by prolonged high temperatures by controlling the parameters of the microwave reduction treatment.

[0011] The above-mentioned method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles is characterized in that, in step three, the high-entropy nanoparticles in the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles have a single-phase face-centered cubic structure with a particle size of 8 nm to 25 nm, are uniformly dispersed on the graphene surface, and have no obvious agglomeration.

[0012] Compared with the prior art, the present invention has the following advantages: 1. This invention employs a dual-feed atomization drying and microwave reduction synergistic process. The dual-channel independent feeding avoids premature mixing and agglomeration of metal ions and graphene, enabling immediate mixing and atomization to form tiny droplets. This ensures uniform distribution of metal ions on the graphene surface and uniform distribution of elements within the metal salt, preventing elemental segregation and thus controlling the phase composition of the high-entropy alloy nanoparticles. Microwave reduction heating is rapid and uniform, achieving graphene reduction and in-situ rapid reduction of metal ions on the graphene surface in one step. This suppresses precursor structure collapse and avoids particle agglomeration and lattice distortion caused by prolonged high-temperature calcination, significantly shortening the preparation cycle and reducing energy consumption. Under the synergistic effect of these two technologies, the product exhibits significantly better catalytic performance, stability, preparation efficiency, and energy consumption than traditional processes.

[0013] 2. The high-entropy nanoparticles prepared by this invention have a single-phase face-centered cubic structure with a particle size controlled between 8 nm and 25 nm. They exhibit no obvious agglomeration and rely on graphene support to achieve uniform loading and stable anchoring, resulting in strong loading stability. The electronic structure is synergistically optimized by multiple elements such as iridium, ruthenium, cobalt, copper, and nickel, reducing the loading of noble metals and balancing performance and cost. Combined with the high conductivity and large specific surface area of ​​graphene, the exposure of catalytic active sites is enhanced and electron transport is accelerated. In the water electrolysis reaction, they exhibit low overpotential, high current density, and long-cycle stability, with performance superior to traditional noble metal-based catalysts.

[0014] 3. This invention achieves precise control of the mass ratio of metal elements to graphene (with a deviation of no more than ±0.5%) by adjusting the feed flow rate ratio and calibrating the density parameter. The ratio can be flexibly adjusted according to actual catalytic needs, making it highly versatile.

[0015] 4. This invention also provides the application of the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles in the field of water electrolysis, solving the problems of existing catalysts such as agglomeration, poor stability, and high energy consumption.

[0016] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0017] Figure 1 The image shows the XRD pattern of graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in Example 1 of this invention.

[0018] Figure 2 This is a low-magnification STEM image of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in Example 1 of this invention.

[0019] Figure 3 This is a high-magnification STEM image of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in Example 1 of this invention.

[0020] Figure 4 This is a mapping diagram of the elemental surface distribution of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in Example 1 of this invention.

[0021] Figure 5 The image shows the EDS elemental distribution spectrum of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in Example 1 of this invention. Detailed Implementation

[0022] Example 1 This embodiment includes the following steps: Step 1: Dissolve iridium tetrachloride hydrate, ruthenium chloride, cobalt chloride hexahydrate, copper chloride dihydrate, and nickel chloride hexahydrate in deionized water in equal atomic ratios and stir until completely dissolved to obtain a precursor solution with a total metal ion concentration of 0.02 mol / L; disperse graphene oxide powder in deionized water and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 10 mg / mL. Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into two independent feed channels of a dual-feed atomizing dryer. The input rate of the metal precursor solution is 1.0 mL / min, and the input rate of the graphene oxide dispersion is 2.2 mL / min, with a flow ratio of 1:2.2, corresponding to a metal element to graphene mass ratio of 1:1.2. The flow control accuracy is ±0.3%. The atomization pressure is 0.3 MPa, and the drying temperature is 190℃. After instant mixing in the atomization chamber, the mixture is atomized into tiny droplets. After drying in the drying chamber, graphene-supported metal ion composite precursor powder with a size of 1 μm to 2 μm is collected, with a yield of 92%. Step 3: Place the graphene-loaded metal ion composite precursor powder obtained in Step 2 into a microwave reduction furnace, introduce argon gas at a flow rate of 50 mL / min, and then reduce it for 10 min at a microwave power of 1000 W, while controlling the temperature after microwave reduction treatment at 400℃. Cool to room temperature to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

[0023] Testing revealed that the atomic ratio of each metal element in the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment was 1:1:1:1:1, which is consistent with the experimental expectations.

[0024] Figure 1 The XRD pattern of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment is shown below. Figure 1 As can be seen, the broadened diffraction peak at 2θ≈25° corresponds to the (002) crystal plane of reduced graphene oxide (rGO), proving that the graphene carrier still maintains a layered structure after microwave reduction. The characteristic diffraction peaks near 2θ≈44°, 49°, and 71° are perfectly matched with the standard card of the face-centered cubic (FCC) high-entropy alloy, confirming that the product is a composite material of high-entropy alloy nanoparticles and graphene. Moreover, the high-entropy nanoparticles are a single-phase structure without phase separation. The peaks are pure and free of impurities, indicating that the high-entropy alloy has good crystallinity, which confirms the process advantage of microwave reduction in avoiding lattice distortion.

[0025] Figure 2 This is a low-magnification STEM image of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment. Figure 3 This is a high-magnification STEM image of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment. Figure 2 and Figure 3 As can be seen from the image, the graphene folded sheet structure and the iridium-ruthenium-cobalt-copper-nickel high-entropy alloy nanoparticles with a size of about 12nm~20nm are uniformly distributed on the surface. The particles have no obvious agglomeration, indicating that the dual-feed atomization drying process avoids the premature agglomeration of metal ions and graphene. Combined with the anchoring effect of graphene, the uniform dispersion of nanoparticles can be effectively achieved.

[0026] Figure 4 This is a mapping of the elemental surface distribution of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment. Figure 4 As can be seen, the elements are evenly distributed without segregation or agglomeration, proving that the dual-feed atomization drying process can achieve uniform loading of metal ions and precisely control the synthesis of high-entropy alloy phases.

[0027] Figure 5 The image shows the EDS elemental distribution spectrum of the graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment. Figure 5 As can be seen from the spectrum, six characteristic peaks of C, Ir, Ru, Co, Cu and Ni were clearly detected, which are completely consistent with the elemental composition of the target product. The unlabeled weak peaks are mainly minor characteristic line peaks of the elements or instrument false peaks. There are no impurity peaks, which proves that the product has high purity. The characteristic peaks of each metal element appear stably, which further verifies the uniformity of element distribution.

[0028] Example 2 This embodiment includes the following steps: Step 1: Dissolve iridium acetate, ruthenium chloride, cobalt acetate tetrahydrate, anhydrous copper chloride, and nickel sulfate hexahydrate in a water-ethanol mixed solvent according to the equiatomic ratio, and stir until completely dissolved to obtain a precursor solution with a total metal ion concentration of 0.01 mol / L. Disperse graphene oxide powder in deionized water and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 8 mg / mL. Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into two independent feed channels of a dual-feed atomizing dryer. The input rate of the metal precursor solution is 1.02 mL / min, and the input rate of the graphene oxide dispersion is 1.2 mL / min, with a flow ratio of 1:1.176, corresponding to a metal element to graphene mass ratio of 1:1. The flow control accuracy is ±0.2%. The atomization pressure is 0.2 MPa, and the drying temperature is 180℃. After instant mixing in the atomization chamber, the mixture is atomized into tiny droplets. After drying in the drying chamber, graphene-supported metal ion composite precursor powder with a size of 1 μm to 2 μm is collected, with a yield of 90%. Step 3: Place the graphene-loaded metal ion composite precursor powder obtained in Step 2 into a microwave reduction furnace, introduce nitrogen gas at a flow rate of 45 mL / min, and then reduce it for 12 min at a microwave power of 900 W. Control the temperature after microwave reduction treatment to 380℃, and cool it to room temperature to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

[0029] Testing revealed that the atomic ratio of each metal element in the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment was 1:1:1:1:1, which is consistent with the experimental expectations. The high-entropy nanoparticles have a single-phase face-centered cubic structure with a particle size of 10 nm to 18 nm, and are uniformly dispersed on the graphene surface without obvious agglomeration.

[0030] Example 3 This embodiment includes the following steps: Step 1: Dissolve iridium chloride, ammonium ruthenium chloride, cobalt chloride hexahydrate, copper chloride dihydrate, and nickel chloride hexahydrate in deionized water in an equiatomic ratio and stir until completely dissolved to obtain a precursor solution with a total metal ion concentration of 0.015 mol / L; disperse graphene oxide powder in deionized water and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 2 mg / mL. Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into two independent feed channels of a dual-feed atomizing dryer. The input rate of the metal precursor solution is 1.0 mL / min, and the input rate of the graphene oxide dispersion is 3.56 mL / min, with a flow ratio of 1:3.56, corresponding to a metal element to graphene mass ratio of 1:1.5. The flow control accuracy is ±0.4%. The atomization pressure is 0.32 MPa, and the drying temperature is 200℃. The components are mixed in the atomization chamber and atomized into tiny droplets. After drying in the drying chamber, graphene-supported metal ion composite precursor powder with a size of 1 μm to 2 μm is collected, with a yield of 93%. Step 3: Place the graphene-loaded metal ion composite precursor powder obtained in Step 2 into a microwave reduction furnace, introduce argon gas at a flow rate of 55 mL / min, and then reduce it for 8 min at a microwave power of 1100 W, while controlling the temperature after microwave reduction treatment at 450℃. Cool to room temperature to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

[0031] Testing revealed that the atomic ratio of each metal element in the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment was 1:1:1:1:1, which is consistent with the experimental expectations. The high-entropy nanoparticles have a single-phase face-centered cubic structure with a particle size of 15nm~22nm, and are uniformly dispersed on the graphene surface without obvious agglomeration.

[0032] Example 4 This embodiment includes the following steps: Step 1: Dissolve iridium tetrachloride hydrate, ruthenium acetate, cobalt chloride hexahydrate, cuprous chloride, and anhydrous nickel sulfate in deionized water in an equiatomic ratio, and stir until completely dissolved to obtain a precursor solution with a total metal ion concentration of 0.015 mol / L; disperse graphene oxide powder in deionized water, and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 6 mg / mL; Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into two independent feed channels of a dual-feed atomizing dryer. The input rate of the metal precursor solution is 1.0 mL / min, and the input rate of the graphene oxide dispersion is 4.0 mL / min, with a flow ratio of 1:4, corresponding to a metal element to graphene mass ratio of 1:1.8. The flow control accuracy is ±0.45%. The atomization pressure is 0.25 MPa, and the drying temperature is 160℃. After instant mixing in the atomization chamber, the mixture is atomized into tiny droplets. After drying in the drying chamber, graphene-supported metal ion composite precursor powder with a size of 1 μm to 2 μm is collected, with a yield of 89%. Step 3: Place the graphene-supported metal ion composite precursor powder obtained in Step 2 into a microwave reduction furnace, introduce nitrogen gas at a flow rate of 40 mL / min, and then reduce it for 20 min at a microwave power of 800 W. Control the temperature after microwave reduction treatment to 300℃, and cool it to room temperature to obtain graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

[0033] Testing revealed that the atomic ratio of each metal element in the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment was 1:1:1:1:1, which is consistent with the experimental expectations. The high-entropy nanoparticles have a single-phase face-centered cubic structure with a particle size of 8 nm to 15 nm, and are uniformly dispersed on the graphene surface without obvious agglomeration.

[0034] Example 5 This embodiment includes the following steps: Step 1: Dissolve ammonium chloroiridate, ammonium chlororuthenate, anhydrous cobalt chloride, anhydrous copper sulfate, and nickel sulfate hexahydrate in deionized water in an equiatomic ratio, and stir until completely dissolved to obtain a precursor solution with a total metal ion concentration of 0.01 mol / L; disperse graphene oxide powder in deionized water, and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 8 mg / mL; Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into two independent feed channels of a dual-feed atomizing dryer. The input rate of the metal precursor solution is 1.01 mL / min, and the input rate of the graphene oxide dispersion is 2.4 mL / min, with a flow ratio of 1:2.376, corresponding to a metal element to graphene mass ratio of 1:2. The flow control accuracy is ±0.35%. The atomization pressure is 0.4 MPa, and the drying temperature is 220℃. After instantaneous mixing in the atomization chamber, the mixture is atomized into tiny droplets. After drying in the drying chamber, graphene-supported metal ion composite precursor powder with a size of 1 μm to 2 μm is collected, with a yield of 91%. Step 3: Place the graphene-loaded metal ion composite precursor powder obtained in Step 2 into a microwave reduction furnace, introduce argon gas at a flow rate of 60 mL / min, and then reduce it for 5 min at a microwave power of 1200 W. Control the temperature after microwave reduction treatment to 500℃, and cool it to room temperature to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

[0035] Testing revealed that the atomic ratio of each metal element in the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in this embodiment was 1:1:1:1:1, which was consistent with the experimental expectations. The high-entropy nanoparticles had a single-phase face-centered cubic structure with a particle size of 18 nm to 25 nm, and were uniformly dispersed on the graphene surface without obvious agglomeration.

[0036] Comparative Example 1 This comparative example includes the following steps: Step 1: Dissolve iridium tetrachloride hydrate, ruthenium chloride, cobalt chloride hexahydrate, copper chloride dihydrate, and nickel chloride hexahydrate in deionized water in equal atomic ratios and stir until completely dissolved to obtain a precursor solution with a total metal ion concentration of 0.02 mol / L; disperse graphene oxide powder in deionized water and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 10 mg / mL. Step 2: Mix the metal precursor solution prepared in Step 1 with the graphene oxide dispersion at a metal element mass ratio of 1:1.2. Soak the mixture at room temperature for 2 hours with continuous stirring, then centrifuge at 8000 r / min for 15 minutes to obtain a precipitate. Dry the precipitate under vacuum at 80℃ for 12 hours, then place it in a tube furnace and heat it to 500℃ under argon protection for 1 hour. Cool it to room temperature to obtain the product.

[0037] Testing revealed that the high-entropy nanoparticles prepared by the traditional wet chemical soaking combined with high-temperature calcination reduction process exhibited severe agglomeration, with particle sizes ranging from 30 nm to 50 nm, and some showed impurity phases; the distribution of metal elements was also uneven.

[0038] As can be seen from the comparison between Example 5 and Comparative Example 1, the present invention adopts a dual-feed atomization drying and microwave reduction synergistic process to achieve uniform and stable loading of metal ions on the graphene surface, and prepares graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles with uniform particle size, pure phase and excellent catalytic performance. The performance is superior to that of high-entropy nanoparticles prepared by traditional wet chemical soaking combined with high-temperature calcination reduction process.

[0039] The graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared in Examples 1-5 and Comparative Example 1 were subjected to hydrogen evolution reaction (HER), oxygen evolution reaction (OER) performance and stability tests, using a glassy carbon working electrode with a diameter of 3 mm and a catalyst loading of 0.5 mg / cm³. 2 The testing system was a three-electrode system, using an Hg / HgO electrode as the reference electrode and a graphite rod as the counter electrode. 1.0M KOH was used as the electrolyte, and a current density of 10 mA / cm² was measured. 2 Overpotential at a current density of 10 mA / cm 2 A constant current stability test was conducted, and the decay rate (%) after 200 hours of cycling was measured. The results are shown in Table 1.

[0040] Table 1

[0041] As can be seen from Table 1, the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared by this invention exhibit advantages of low overpotential and high stability in the water electrolysis reaction, and can be widely used in the field of water electrolysis, suitable for large-scale production and industrial application.

[0042] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles, characterized in that, The method includes the following steps: Step 1: Dissolve iridium salt, ruthenium salt, cobalt salt, copper salt, and nickel salt in a solvent at an equiatomic ratio and stir until homogeneous to obtain a metal precursor solution with a total metal ion concentration of 0.01 mol / L to 0.02 mol / L; disperse graphene oxide powder in water and then ultrasonically disperse to obtain a graphene oxide dispersion with a solid content of 2 mg / mL to 10 mg / mL. Step 2: The metal precursor solution and graphene oxide dispersion obtained in Step 1 are simultaneously fed into the two independent feed channels of the dual-feed atomizing dryer. They are mixed in the atomizing chamber and then atomized into tiny droplets. After drying in the drying chamber, graphene-loaded metal ion composite precursor powder with a size of 1μm~2μm is collected. Step 3: Place the graphene-loaded metal ion composite precursor powder obtained in Step 2 into a microwave reduction device and perform microwave reduction treatment under an inert gas atmosphere to obtain graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles.

2. The method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles according to claim 1, characterized in that, In step one, the iridium salt is at least one of iridium chloride, ammonium chloroiridate, iridium acetate, and iridium tetrachloride hydrate; the ruthenium salt is at least one of ruthenium chloride, ammonium chlororuthenate, and ruthenium acetate; the cobalt salt is at least one of cobalt acetate tetrahydrate, cobalt chloride hexahydrate, and anhydrous cobalt chloride; the copper salt is at least one of copper chloride dihydrate, anhydrous copper chloride, cuprous chloride, and anhydrous copper sulfate; and the nickel salt is at least one of anhydrous nickel chloride, nickel chloride hexahydrate, and anhydrous nickel sulfate.

3. The method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles according to claim 1, characterized in that, In step two, the feed flow ratio of the metal precursor solution to the graphene oxide dispersion is 1:1~4, and the flow control accuracy is ±0.5%.

4. The method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles according to claim 1, characterized in that, The atomization pressure of the dual-feed atomizing dryer in step two is 0.2MPa~0.4MPa, and the drying temperature is 160℃~220℃.

5. The method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles according to claim 1, characterized in that, The microwave power of the microwave reduction treatment in step three is 800W~1200W, the time is 5min~20min, and the temperature after microwave reduction treatment is 300℃~500℃; the inert gas is nitrogen or argon, and the flow rate is 40mL / min~60mL / min.

6. The method for preparing graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles according to claim 1, characterized in that, In step three, the graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles have a single-phase face-centered cubic structure with a particle size of 8 nm to 25 nm. They are uniformly dispersed on the graphene surface without obvious agglomeration.

7. An application of graphene-supported iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles prepared by the method according to any one of claims 1 to 6, characterized in that, The graphene-loaded iridium-ruthenium-cobalt-copper-nickel high-entropy nanoparticles are applied in the field of water electrolysis.