Method for degrading organic pollutants by coupling nano confinement catalytic membrane with micro-nano bubbles

By combining nano-confined catalytic membranes with micro-nano bubble technology, the contradiction between catalyst loading density and membrane permeability is resolved, achieving efficient and stable degradation of organic pollutants and catalyst recovery, thus improving water treatment efficiency.

CN122079427APending Publication Date: 2026-05-26SHANDONG ANALYSIS AND TEST CENTER
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202610543430.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-23
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

Existing technologies are ineffective at removing recalcitrant organic pollutants. Membrane separation can easily lead to pollutant concentration and secondary pollution. Catalyst recovery is difficult, and there is a contradiction between catalyst loading density and membrane permeability, which affects water treatment efficiency.

Method used

By employing nano-confined catalytic membrane coupled with micro/nano bubble technology, a cobalt-iron layered double hydroxide catalyst is loaded into the membrane channels, and the oxidation process is enhanced by micro/nano bubbles, thereby achieving efficient catalyst immobilization and degradation of organic pollutants.

Benefits of technology

It achieves efficient degradation of organic pollutants, has stable membrane flux, easy catalyst recovery, and a wide range of applications, and can effectively treat organic pollutant wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122079427A_ABST
    Figure CN122079427A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of environmental pollution treatment and water treatment, and particularly relates to a method for degrading organic pollutants by coupling a nano confinement catalytic membrane with micro-nano bubbles. The method comprises the following steps: adding micro-nano bubble water and an oxidizing agent into an organic pollutant solution, regulating the pH value to prepare a pretreatment mixed solution, and enabling the pretreatment mixed solution to pass through a nano confinement catalytic membrane to catalytically degrade the organic pollutants, the nano confinement catalytic membrane comprises an organic polymer membrane substrate and a catalyst loaded in the organic polymer membrane substrate; the loading capacity of the catalyst is 5 to 30 mg. The problems that antibiotics are difficult to degrade, pollutant concentration is easily caused by membrane separation, a catalyst is difficult to recycle, and membrane flux and catalytic activity are difficult to balance are solved, the method has the advantages of being high in degradation efficiency, stable in membrane flux, easy to recycle the catalyst and wide in application range, and wastewater containing organic pollutants can be efficiently treated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of environmental pollution control and water treatment technology, specifically relating to a method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro-nano bubbles. Background Technology

[0002] With the widespread use of organic compounds such as antibiotics in medicine, animal husbandry, and aquaculture, large amounts of unmetabolized organic matter enter the aquatic environment, forming persistent and difficult-to-degrade organic pollutants that pose a continuous threat to ecological security and human health. Traditional water treatment processes are ineffective in removing these trace pollutants, and currently rely mainly on membrane separation and advanced oxidation technologies. While membrane separation technologies (such as ultrafiltration and nanofiltration) can retain some low-molecular-weight organic matter, they generally face problems such as severe membrane fouling, rapid flux decline, and easy concentration of pollutants and secondary pollution. Although advanced oxidation technologies can degrade organic matter through active free radicals, their commonly used heterogeneous nanocatalysts have defects such as easy aggregation, difficulty in recovery, and metal ion leaching, affecting the long-term stable operation of the system and the practical application effect.

[0003] In recent years, nano-confined catalytic membrane technology has alleviated the problems of catalyst aggregation and loss to some extent by immobilizing the catalyst within the membrane channels, and has improved catalytic degradation efficiency through the confinement effect. However, there is an inherent contradiction between catalyst loading density and membrane permeability. Excessive loading can easily clog the channels and significantly reduce membrane flux; insufficient loading leads to limited catalytic activity, affecting pollutant degradation efficiency and restricting its applicability in practical water treatment. Micro- and nano-bubble technology, due to its small size, long residence time, and high mass transfer efficiency, has been proven to effectively enhance mass transfer and reaction efficiency in oxidation processes. Effectively combining it with catalytic membrane systems presents the challenge of maintaining a high catalyst loading density to ensure degradation activity while avoiding membrane pore blockage and structural damage caused by excessive loading or micro- and nano-bubble disturbance, thereby ensuring high permeate flux and stable operation of the membrane system in the long term. Summary of the Invention

[0004] The purpose of this invention is to provide a method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro-nano bubbles, thereby overcoming the shortcomings of the prior art. This method has high degradation efficiency, stable membrane flux, easy catalyst recovery, and wide applicability, and can efficiently treat organic pollutant wastewater.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows: This invention provides a method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro-nano bubbles, comprising the following steps: adding micro-nano bubble water and an oxidant to an organic pollutant solution and adjusting the pH to obtain a pretreated mixture, and passing the pretreated mixture through a nano-confined catalytic membrane to catalytically degrade the organic pollutants.

[0006] Nanoconfined catalytic membranes consist of an organic polymer membrane substrate and a catalyst supported thereon. The catalyst is a cobalt-iron layered double hydroxide (CoFe-LDH) catalyst; The catalyst loading in the nano-confined catalytic membrane ranged from 0.4 to 2.4 mg / cm³. 2 .

[0007] Preferably, the catalyst loading in the nano-confined catalytic membrane is 1.0~2.0 mg / cm³. 2 .

[0008] In other embodiments, the roughness of the nanoconfined catalytic membrane is ≤6.11 nm, and the transmembrane flux is 165~1400 L / (m²). 2 ·h).

[0009] In some other embodiments, the concentration of organic pollutants is 5 to 20 mg / L.

[0010] In some other embodiments, the organic pollutant is one or more of spiramycin, ofloxacin, ciprofloxacin hydrochloride, and erythromycin.

[0011] In some other embodiments, the concentration of the oxidant is 0.05~0.4 mM; preferably, the concentration of the oxidant is 0.2~0.4 mM. The oxidizing agent is peracetic acid.

[0012] In some other embodiments, the pH is 3 to 11; the volume ratio of micro-nano bubble water is 20% to 80%.

[0013] Preferably, the pH is 5-9; the volume ratio of micro-nano bubble water is 60%-80%.

[0014] In some other embodiments, the catalyst is prepared as follows: Cobalt salt, urea, NH4F and MIL-88A were added to water and mixed to prepare a mixed solution. The mixed solution was subjected to a hydrothermal reaction, and the catalyst was obtained by centrifugation, washing and drying. The catalyst was loaded onto an organic polymer membrane substrate using a vacuum filtration method to obtain a nano-confined catalytic membrane. The molar ratio of cobalt salt, urea, and NH4F is (0.4~0.6):(8~12):(3~5); 100~300 ml of water is added per gram of MIL-88A. Preferably, the molar ratio of cobalt salt, urea, and NH4F is 0.5:10:4; 200 ml of water is added per gram of MIL-88A.

[0015] In some other embodiments, the cobalt salt is selected from one or both of cobalt nitrate and cobalt chloride; The hydrothermal reaction is carried out at a temperature of 110-130℃ for 3-8 hours. Preferably, the hydrothermal reaction is carried out at a temperature of 120℃ for 5 hours.

[0016] In some other embodiments, the preparation method of MIL-88A is as follows: Fumaric acid and iron salt are added to water, mixed, heated to react, and then centrifuged, washed, and dried to obtain MIL-88A. The mass ratio of fumaric acid to iron salt is (1.1~1.2):(4.5~5).

[0017] In some other embodiments, the iron salt is selected from one or more of ferric nitrate, ferric chloride, and ferric sulfate; The heating reaction is carried out at a temperature of 90~110℃ for 4~8 hours.

[0018] Preferably, the heating reaction is carried out at a temperature of 100°C for 5 hours.

[0019] The beneficial effects of this invention are: This invention significantly increases the contact area between the gas-liquid mass transfer interface and pollutants by introducing micro- and nano-bubbles. The localized high temperature, high pressure, and free radicals generated during the collapse of these bubbles can pre-oxidize or directly degrade some pollutants. The nano-confined catalyst supported within the membrane substrate effectively enriches pollutants and oxidants within the confined space, increasing the local concentration of reactants. Simultaneously, the confinement effect modulates the electronic structure of the catalytic active center, improving the catalyst's activation efficiency and stability for oxidants. Furthermore, the membrane-based reactor integrates catalysis and separation, enabling stable operation in continuous flow mode and preventing catalyst loss. The lift-off effect of micro- and nano-bubbles, combined with the micro-turbulence on the membrane surface, enhances interfacial renewal, preventing membrane fouling. Even under wide pH ranges and low oxidant dosage conditions, efficient, rapid, and sustained degradation of organic pollutants can still be achieved. Attached Figure Description

[0020] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0021] Figure 1 This is a photograph of the nano-confined catalytic membrane in Example 1 of the present invention; Figure 2 This is a SEM image of CoFe-LDH in Example 1 of the present invention; Figure 3 This is the XPS full spectrum of CoFe-LDH in Example 1 of the present invention; Figure 4 The image shown is the XRD pattern of CoFe-LDH in Example 1 of this invention. Figure 5 This is the AFM image of the nano-confined catalytic membrane in Example 1 of the present invention; Figure 6 This is a physical image of the device for degrading antibiotics using a nano-confined catalytic membrane coupled with micro / nano bubbles in Embodiment 2 of the present invention; Figure 7 This is a comparison chart of the degradation effects of different systems on spiramycin in Example 2 of the present invention; Figure 8 This is a graph showing the removal rate of spiramycin under different transmembrane fluxes in Example 2 of the present invention; Figure 9 This is a graph showing the effect of catalyst loading on the membrane on the degradation effect in Example 2 of the present invention; Figure 10 This is a graph showing the removal rate of spiramycin at different PAA dosages in Example 2 of the present invention; Figure 11 This is a graph showing the effect of the proportion of micro / nano bubble water on the degradation effect in Example 2 of the present invention; Figure 12 This is a graph showing the removal rate of spiramycin at different pH values ​​in Example 2 of the present invention; Figure 13 The figure shows the experimental results of free radical quenching in Example 2 of the present invention. Detailed Implementation

[0022] Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be construed as limiting the scope of the invention. Specific conditions not specified in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Components whose manufacturers are not specified are all commercially available conventional products.

[0023] To address the existing problems of recalcitrant degradation of organic pollutants such as antibiotics, easy concentration of pollutants due to membrane separation, difficulty in catalyst recovery, and difficulty in balancing membrane flux and catalytic activity, this invention provides a method for degrading antibiotics using a nano-confined catalytic membrane coupled with micro / nano bubbles. This method has high degradation efficiency, stable membrane flux, easy catalyst recovery, and wide applicability, and can efficiently treat organic pollutant wastewater.

[0024] The solution of the present invention will be further described below with reference to specific embodiments: Example 1 This embodiment provides a method for preparing a nano-confined catalytic membrane, specifically including the following steps: (1) Preparation of MIL-88A precursor: 1.165 g of fumaric acid and 4.848 g of Fe(NO3)3·9H2O were dispersed in 100 mL of ultrapure water. After ultrasonic mixing, the solution was heated in an oil bath at 100 °C for 5 h, then centrifuged at 10000 rpm for 5 minutes, washed once with deionized water and once with ethanol. After centrifugation, the product was dried at 60 °C for 12 hours to obtain MIL-88A.

[0025] (2) Preparation of CoFe-LDH catalyst: Layered stacked CoFe-LDH was synthesized on the surface of the MIL-88A precursor by a simple hydrothermal etching method. 0.5 mmol Co(NO3)2·6H2O, 10.0 mmol urea, 4.0 mmol NH4F, and 250.0 mg MIL-88A were mixed in 50 mL of ultrapure water. After ultrasonic mixing, the mixture was transferred to a polytetrafluoroethylene-lined high-pressure reactor and hydrothermally reacted at 120 °C for 5 h. The reaction product was centrifuged at 7000 rpm for 5 min, washed twice with deionized water, and once with ethanol. After centrifugation, the product was dried at 60 °C for 12 h to obtain a reddish-brown cobalt-iron layered double hydroxide catalyst, abbreviated as CoFe. LDH powder.

[0026] (3) Assembly of nano-confined catalytic membrane: 5~30 mg CoFe was used as a vacuum filtration method. LDH catalyst is uniformly supported on a PVDF (polyvinylidene fluoride) membrane substrate to obtain a nano-confined catalytic membrane (e.g., Figure 1 (As shown).

[0027] Characterization of nano-confined catalytic membranes: Depend on Figure 2 SEM images of CoFe-LDH show that a flower-like structure of CoFe-LDH was synthesized on rod-shaped MIL-88A, which can increase the specific surface area and expose more active sites.

[0028] Depend on Figure 3 The XPS full spectrum of CoFe-LDH shows that the synthesized material contains Co, Fe, O and C elements.

[0029] Depend on Figure 4 The XRD pattern of CoFe-LDH shows that the diffraction peaks appearing on the crystal planes at (003), (006), (012), (009), (015) and (018) are characteristic peaks of CoFe-LDH, indicating that CoFe-LDH was successfully synthesized.

[0030] Depend on Figure 5The AFM diagram of the nanoconfined catalytic membrane shows that the arithmetic mean roughness of the assembled nanoconfined catalytic membrane is only 6.11 nm.

[0031] The morphology, structure, and elemental composition of the catalytic membrane were characterized and analyzed by SEM, XRD, XPS, and AFM. The results showed that the CoFe catalyst on the membrane... LDH was successfully synthesized, and the assembled nanoconfined catalytic membrane had an arithmetic mean roughness of only 6.11 nm.

[0032] Example 2 This embodiment provides the construction of a nano-confined catalytic membrane coupled with a micro / nano bubble degradation system. A physical image of the device for degrading antibiotics using a nano-confined catalytic membrane coupled with micro / nanobubbles is shown below. Figure 6 As shown, the system includes a micro / nano bubble generator, a solution preparation device, and a nano-confined catalytic membrane reactor connected in sequence. The micro / nano bubble generator is used to prepare micro / nano bubble water with uniform size and stable concentration. The solution preparation device is used to prepare antibiotic solutions by mixing the micro / nano bubble water with ordinary water and an oxidant in different proportions. The nano-confined catalytic membrane reactor contains a nano-confined catalytic membrane and is used to degrade antibiotics. The flow rate is controlled by adjusting the speed of a peristaltic pump, and the filtrate is periodically taken from the nano-confined catalytic membrane reactor, weighed, and the transmembrane flux is calculated.

[0033] The working process of the device for degrading antibiotics using a nano-confined catalytic membrane coupled with micro / nanobubbles is as follows: The micro-nano bubble generator is activated, and by adjusting the aeration time, micro-nano bubble water with uniform size and stable concentration is obtained. The micro-nano bubble water, oxidant, and organic pollutants are added to the water in the preparation device (such as a beaker), and the pH is adjusted. After stirring and mixing, the solution to be treated is prepared. The solution to be treated is added to the nano-confined catalytic membrane reactor through a peristaltic pump, and the antibiotic is degraded by coupling micro-nano bubbles with the nano-confined catalytic membrane.

[0034] During the experiment, the optimal process parameters were optimized by controlling variables such as the initial concentration of pollutants, oxidant concentration, membrane flux, initial pH, and catalyst loading. The specific optimization process is as follows: 1. Optimization of antibiotic degradation process parameters A nano-confined catalytic membrane was coupled with micro-nano bubbles, and peracetic acid (PAA) oxidant was activated through a filtration device to degrade antibiotics. Taking spiramycin (SPM) as an example, the optimal process parameters were explored. The initial antibiotic concentration was 10 mg / L; the PAA oxidant concentration was 0.05–0.4 mM; the catalyst loading on the membrane (the membrane was a 2 cm diameter circle) was 5–30 mg; the reaction pH was 3–11; and the ratio of micro-nano bubble water to ordinary water was 20%–80%.

[0035] A beaker containing 200 mL of mixed nanobubble water with 10 mg / L spiramycin (SPM) was placed on a magnetic stirrer. A certain amount of PAA was added to the beaker, and the pH was adjusted. Magnetic stirring was then performed for 10 min. Subsequently, the contaminant solution was pumped into the membrane reactor using a peristaltic pump, with the flow rate controlled by adjusting the pump speed. Every 5–15 min, samples were taken and filtered through a 0.22 μm filter membrane to determine the SPM concentration.

[0036] (1) Optimization of degradation methods: PAA (peracetic acid) group, PAA+MNB (peracetic acid + micro / nano bubble water) group, PAA+LDH membrane (peracetic acid + nano confined catalytic membrane) group, PAA+MNB+LDH membrane (peracetic acid + micro / nano bubble water + nano confined catalytic membrane) group, and PVDF (polyvinylidene fluoride) membrane group were set up respectively to study the degradation effect of each group on spiramycin, such as Figure 7 As shown. By Figure 7 It was found that PAA alone could only degrade 8.9% of pollutants in 20 minutes, the degradation rate of PAA+MNB was about 23%, the removal rate of PAA+LDH membrane was stable at about 82%, and the removal rate of PAA+MNB+LDH membrane was stable at over 98%. Pollutants passing through the PVDF membrane substrate alone showed almost no degradation effect. This indicates that nano-confined catalytic membrane coupled with micro / nano bubbles can effectively promote antibiotic degradation.

[0037] (2) Optimization of transmembrane flux: The removal rate of spiramycin was studied at transmembrane fluxes of 169.85, 382.17, 679.41 and 1358.82 L / (m²·h), respectively. The results are as follows: Figure 8 As shown. By Figure 8 It can be seen that the removal rate is the highest at a membrane flux of 382.17 L / (m²·h), which is close to 100%.

[0038] (3) Optimization of catalyst loading on the membrane: The removal rate of spiramycin was studied at catalyst loadings of 5, 10, 20 and 30 mg on the membrane, respectively. The results are as follows: Figure 9 As shown. By Figure 9 It can be seen that when the catalyst loading of the catalytic membrane is 10 mg, the removal rate can reach 100%.

[0039] (4) Optimization of different PAA oxidant concentrations: The removal rate of spiramycin was studied at different PAA oxidant concentrations of 0.05, 0.1, 0.2 and 0.4 mM, and the results are as follows. Figure 10 As shown. By Figure 10 It can be seen that when the concentration of the oxidant PAA is 0.2 mM, the removal rate can reach 100%.

[0040] (5) Optimization of different ratios of micro / nano bubble water to ordinary water: The removal rate of spiramycin was studied under different ratios of micro / nano bubble water to ordinary water of 20%, 40%, 60%, and 80%, and the results are as follows. Figure 11 As shown. By Figure 11 It can be seen that the removal rate is the highest, close to 100%, when the ratio of micro-nano bubble water to ordinary water is 80%.

[0041] (6) Optimization at different pH values: The removal rate of spiramycin was studied at pH values ​​of 3, 5, 6.17, 7, 9 and 11, respectively. The results are as follows: Figure 12 As shown. By Figure 12 It can be seen that when the pH value is 5-9, the removal rate of spiramycin is close to 100%.

[0042] The above studies indicate that the optimal degradation conditions for spiramycin at 10 mg / L are: membrane flux of 382.17 L / (m²·h), catalyst loading of 10 mg, PAA oxidant concentration of 0.2 mM, nanobubble water ratio of 80%, and pH range of 5–9. This demonstrates that the nano-confined catalytic membrane coupled with micro / nanobubbles can effectively promote antibiotic degradation.

[0043] 2. Investigation into the degradation mechanism The types of free radicals generated in the catalytic membrane system were determined through free radical quenching experiments (adding specific "quenchers" to the reaction system to verify or identify which active free radicals are the main reactive species leading to the degradation or reaction of the target substance). The added quenchers included methanol (MA), tert-butanol (TBA), benzoquinone (BQ), and furfuryl alcohol (FAA). The results of the free radical quenching experiments are as follows: Figure 13 As shown.

[0044] Methanol (MA) can quench some free radicals in the system, including peroxyacetyl radicals. The removal rate decreased to 17.2% after the addition of methanol, indicating the presence of peroxyacetyl radicals in the reaction system and their significant contribution. Tert-butanol (TBA) has a good quenching effect on hydroxyl radicals; when TBA is added to 100 mM, the degradation rate decreases to 77.8%, indicating that hydroxyl radicals in the reaction system contribute to degradation to some extent, but the effect is weak. Benzoquinone (BQ) can quench superoxide radicals. The removal rate decreased to 58.3% when 10 mM BQ was added to the system, indicating that superoxide radicals play a certain role in degradation. Furfuryl alcohol (FAA) can quench singlet oxygen. The removal rate was 42.6% when 10 mM furfuryl alcohol was added to the system, indicating that the presence of singlet oxygen also promotes the degradation effect.

[0045] In addition, long-term continuous flow experiments were conducted to evaluate the stability of the catalytic membrane. It maintained a high degradation rate for more than 5 hours of continuous operation, exhibiting good performance, stable flux, and no significant membrane blockage. This demonstrates the excellent performance of nano-confined catalysis.

[0046] This invention immobilizes the catalyst within a membrane, simplifying solid-liquid separation. The nano-confinement effect enhances the generation of active substances, while micro- and nano-bubbles improve mass transfer efficiency. The synergistic effect of free radicals and singlet oxygen leads to more thorough degradation. It has a wide range of applicable degradation targets, capable of degrading various antibiotics such as spiramycin, ofloxacin, ciprofloxacin hydrochloride, and erythromycin.

[0047] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for degrading organic pollutants using a nano-confined catalytic membrane coupled with micro / nanobubbles, characterized in that, Includes the following steps: Micro-nano bubble water and oxidant were added to an organic pollutant solution and the pH was adjusted to prepare a pretreated mixture. The pretreated mixture was then passed through a nano-confined catalytic membrane to catalytically degrade the organic pollutants. The nano-confined catalytic membrane comprises an organic polymer membrane substrate and a catalyst supported thereon; the catalyst is a cobalt-iron layered double hydroxide catalyst. The catalyst loading in the nanoconfined catalytic membrane is 0.4~2.4 mg / cm³. 2 .

2. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 1, characterized in that, The roughness of the nanoconfined catalytic membrane is ≤6.11 nm, and the transmembrane flux is 165~1400 L / (m²). 2 ·h).

3. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 1, characterized in that, The concentration of the organic pollutant is 5~20 mg / L.

4. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 2, characterized in that, The organic pollutant is one or more of spiramycin, ofloxacin, ciprofloxacin hydrochloride, and erythromycin.

5. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 1, characterized in that, The concentration of the oxidant is 0.05~0.4 mM; The oxidant is peracetic acid.

6. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 1, characterized in that, The pH value is 3 to 11; the volume ratio of the micro-nano bubble water is 20% to 80%.

7. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 1, characterized in that, The catalyst is prepared as follows: Cobalt salt, urea, NH4F and MIL-88A were added to water and mixed to prepare a mixed solution. The mixed solution was subjected to a hydrothermal reaction, and the catalyst was obtained by centrifugation, washing and drying. The catalyst was loaded onto an organic polymer membrane substrate using a vacuum filtration method to obtain a nano-confined catalytic membrane. The molar ratio of the cobalt salt, urea and NH4F is (0.4~0.6):(8~12):(3~5); 100~300 ml of water is added per gram of MIL-88A.

8. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 7, characterized in that, The cobalt salt is selected from one or both of cobalt nitrate and cobalt chloride; The hydrothermal reaction is carried out at a temperature of 110~130℃ for 3~8 hours.

9. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 6, characterized in that, The preparation method of MIL-88A is as follows: Fumaric acid and iron salt are added to water, mixed, heated to react, and then centrifuged, washed, and dried to obtain MIL-88A. The mass ratio of fumaric acid to iron salt is (1.1~1.2):(4.5~5).

10. The method for degrading organic pollutants by coupling a nano-confined catalytic membrane with micro / nano bubbles as described in claim 9, characterized in that, The iron salt is selected from one or more of ferric nitrate, ferric chloride, and ferric sulfate; The heating reaction is carried out at a temperature of 90~110℃ for 4~8 hours.

Citation Information

Patent Citations

  • Ceramic catalytic membrane in-situ activated air micro-nano bubble sewage treatment system and treatment method for wastewater containing organic pollutants

    CN117263361A

  • CoFeCuMn LDH nanosheet, confinement catalytic membrane and preparation method of CoFeCuMn LDH nanosheet

    CN119490236A

  • Preparation method of catalytic oxidation peroxyacetic acid self-release oxygen membrane and application of catalytic oxidation peroxyacetic acid self-release oxygen membrane in water treatment field

    CN120532309A

  • P-n heterojunction composite material supported on surface of nickel foam, preparation method therefor and use thereof

    WO2021212923A1