An ionic liquid flame retardant, an epoxy resin composite material, its preparation method and application
By introducing an ionic liquid flame retardant with a phosphorus-nitrogen-sulfur ternary synergistic flame retardant system into epoxy resin, the problems of the flammability of epoxy resin and the environmental pollution caused by traditional flame retardants have been solved, achieving high-efficiency flame retardancy and improved mechanical properties.
Patent Information
- Application Number
- CN202610098463.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-26
- Publication Date
- 2026-05-26
AI Technical Summary
The flammability of epoxy resins and the environmental pollution caused by traditional flame retardants are particularly important in the aerospace and electronics industries, where there is an urgent need for flame retardant properties and traditional flame retardants can negatively impact mechanical properties.
An ionic liquid flame retardant with a phosphorus-nitrogen-sulfur ternary synergistic flame retardant system constructed by containing amino, sulfonyl and pentaerythritol phosphate is introduced into the epoxy resin network through chemical bonding to improve flame retardant performance and enhance mechanical properties.
It significantly improves the flame retardant and mechanical properties of epoxy resin, increasing the limiting oxygen index to 29.3% and achieving a UL-94 vertical flammability rating of V-0. At the same time, the tensile strength, flexural modulus, and impact strength are increased by 46.10%, 57.43%, and 87.67%, respectively.
Smart Images

Figure CN122080070A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to ionic liquid technology, and more particularly to an ionic liquid flame retardant, an epoxy resin composite material, its preparation method, and its application. Background Technology
[0002] Epoxy resins possess excellent mechanical properties, as well as good thermal stability and chemical resistance, making them suitable for use in general adhesives, high-performance coatings, and encapsulation materials. Currently, epoxy resins have wide applications in various fields such as aerospace, automotive industry, and composite materials. In 2024, the global demand for epoxy resins reached 3.72 million tons, and due to the continuous development of end-use applications such as wind power development, electronic packaging, automotive industry, and coatings, the global market demand for epoxy resins is expected to maintain a growth trend. However, epoxy resins are extremely flammable, with an oxygen index of only about 19%, and their flammability and sustained combustion can easily lead to fires. The flammability of epoxy resins is a major limiting factor in some high-end applications with extremely stringent flame retardant requirements, such as the electronics industry and aerospace. Therefore, it is necessary to modify epoxy resins to provide better flame retardancy and excellent thermodynamic properties.
[0003] Currently, there are two main types of epoxy resin flame retardants: additive flame retardants and reactive flame retardants. Additive flame retardants do not react with epoxy resin but rather form a physical mixture by dispersing within it. This additive method often leads to flame retardant migration and a significant reduction in the resin's mechanical properties. Reactive flame retardants, on the other hand, react with epoxy resin. The flame-retardant molecules can attach to the epoxy resin's molecular chain, thereby binding flame-retardant elements (P, N, halogens, etc.) into the epoxy resin's molecular chain, resulting in good flame retardancy, anti-migration properties, and good mechanical properties. However, while halogenated flame retardants possess high flame retardancy and good mechanical properties, they generate large amounts of corrosive and toxic gases during use and recycling, easily causing environmental pollution. The toxic gases released after combustion can also cause secondary injuries.
[0004] In recent years, with the increasing global awareness of environmental protection and the rising safety requirements for flame-retardant materials in various countries, the development of green and efficient new flame retardants has become a research frontier and hot topic in this field. Ionic liquids typically refer to molten salts that are liquid at or near room temperature, composed entirely of organic cations and inorganic / organic anions, and possess characteristics such as low vapor pressure, good thermal stability, non-flammability, and strong structural designability. Studies have shown that ionic liquids can not only be directly added to epoxy resins as flame retardants, but also work synergistically with other flame-retardant components to significantly improve the flame-retardant properties of epoxy resins. In particular, phosphorus- and nitrogen-containing functionalized ionic liquids, through a synergistic flame-retardant mechanism of gas-phase quenching and condensed-phase charring, can effectively suppress the release of heat and smoke during the combustion process of epoxy resins. Against this backdrop, the development of a novel ionic liquid flame retardant provides a new research direction for the flame-retardant modification of epoxy resins, and has significant importance and industrial application value. Summary of the Invention
[0005] The purpose of this invention is to address the aforementioned problems by proposing a method for preparing an ionic liquid flame retardant. This method introduces amino, sulfonyl, and pentaerythritol phosphate into an ionic liquid to construct a phosphorus-nitrogen-sulfur ternary synergistic flame retardant system. The resulting ionic liquid flame retardant contains amino groups that can participate in the curing reaction of epoxy resins, significantly improving the flame retardant properties of epoxy resin composites while effectively enhancing their tensile, flexural, and impact strengths.
[0006] It should be noted that, in this invention, unless otherwise specified, the specific meaning of "comprising" in relation to composition and description includes both open-ended meanings such as "comprising," "including," etc., and closed-ended meanings such as "composed of," "consisting of," etc., and similar meanings.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is: a method for preparing an ionic liquid flame retardant, comprising the following steps:
[0008] S1. Solvent, acid-binding agent and pentaerythritol phosphate (PEPA) are added to a reaction vessel, and then an alkyl sulfonyl chloride compound is added dropwise to carry out the reaction. After the reaction is completed, the mixture is separated and purified to obtain intermediate PEPA-Ps (also known as [PMoam]Ps), which is a white solid powder.
[0009] S2. The intermediate PEPA-Ps is dissolved in an organic solvent and reacted with an amino-containing heterocyclic compound. After the reaction is completed, the mixture is separated and purified to obtain the ionic liquid flame retardant, which is a pale yellow flake solid or a pale yellow liquid.
[0010] Further, in step S1, the solvent is one or more selected from dichloromethane, dichloroethane, dichloroethane, chloroform, carbon tetrachloride, cyclohexane, and petroleum ether.
[0011] Further, in step S1, the acid-binding agent is one or more of triethylamine, pyridine, and N,N-diisopropylethylamine.
[0012] Further, in step S1, the alkyl sulfonyl chloride compound is propyl sulfonyl chloride and / or ethyl sulfonyl chloride.
[0013] Further, in step S1, the molar ratio of the pentaerythritol phosphate, the acid-binding agent, and the alkyl sulfonyl chloride compound is 1:1-1.5:1-1.5.
[0014] Furthermore, in step S1, the amount of solvent used is determined by its ability to dissolve the reactants, for example, the ratio of solvent to acid-binding agent is 50-200:0.1-0.5 (mL:mol).
[0015] Furthermore, in step S1, the alkyl sulfonyl chloride compound is added dropwise over a period of 1-5 hours, the reaction temperature is room temperature, and the reaction time is 2-4 hours.
[0016] Further, in step S1, the separation and purification includes: removing the solvent by vacuum distillation, dispersing in water, ultrasonic oscillation, washing and filtering with water, and drying under vacuum conditions.
[0017] Furthermore, the ultrasonic oscillation time is 3-10 minutes.
[0018] Furthermore, the water washing and filtration is performed 3-5 times.
[0019] Furthermore, the vacuum drying temperature is 60-90℃, and the vacuum drying time is 24-48 hours.
[0020] Further, in step S2, the amino-containing heterocyclic compound is selected from one or more of N-aminopropylmorpholine, 1-(3-aminopropyl)imidazolium, and 2-aminopyridine.
[0021] Further, in step S2, the organic solvent is one or more of acetonitrile, 1,4-dioxane, and N,N-dimethylformamide.
[0022] Further, in step S2, the molar ratio of the intermediate PEPA-Ps to the amino-containing heterocyclic compound is 1:1-1.2.
[0023] Furthermore, in step S2, the amount of solvent used is determined by its ability to dissolve the reactants. For example, the ratio of solvent to intermediate PEPA-Ps is 50-100:0.1-0.5 (mL:mol).
[0024] Furthermore, in step S2, the reaction temperature is 40-60℃ and the reaction time is 24-48 hours.
[0025] Further, in step S2, the separation and purification includes: removing acetonitrile by vacuum distillation and drying under vacuum conditions.
[0026] Furthermore, the vacuum drying temperature is 60-80℃, and the vacuum drying time is 24-48 hours.
[0027] Another object of the present invention discloses an ionic liquid flame retardant prepared by the above-described method. The ionic liquid flame retardant comprises a phosphorus-containing organic cation and a sulfonate anion. The phosphorus-containing organic cation is formed by linking a PEPA structure to an amino-containing heterocyclic compound via an alkyl sulfonyl group. The ionic liquid contains phosphorus, nitrogen, and sulfur, three synergistic flame-retardant elements. The nitrogen-containing group is a nitrogen-containing heterocyclic group or an organic group provided by an amino compound. The nitrogen-containing heterocyclic group is selected from morpholino, imidazolyl, or pyridinyl. The amino compound is selected from N-aminopropylmorpholine, 1-(3-aminopropyl)imidazolium, or 2-aminopyridine. The sulfonyl group is provided by propylsulfonyl chloride or ethylsulfonyl chloride.
[0028] Another object of the present invention discloses the application of an ionic liquid flame retardant in epoxy resin composites.
[0029] Another object of the present invention discloses a flame-retardant epoxy resin composite material, comprising epoxy resin, curing agent and said ionic liquid flame retardant.
[0030] Furthermore, the amount of ionic liquid flame retardant added to the flame-retardant epoxy resin composite material is 2-10 wt., based on the weight of the epoxy resin.
[0031] Furthermore, the mass fraction of phosphorus in the flame-retardant epoxy resin composite material is 0.11-0.54 wt.%.
[0032] Furthermore, the epoxy resin is a bisphenol A type epoxy resin, and the shrinkage oxidizing agent is a bisphenol A type epoxy resin. Glyceryl ether Type resin, shrinkage Glycerides Type resin, Glycerin One or more of amine resins, alicyclic epoxy compounds, and linear aliphatic epoxy compounds; the curing agent is 4,4-diaminodiphenylmethane.
[0033] The ionic liquid flame retardant participates in the curing reaction of epoxy resin through its active amino groups, chemically bonding to the epoxy resin crosslinking network. The composite material has a limiting oxygen index of 24.2%-29.3% and achieves a UL-94 vertical flammability rating of V-0 or V-1.
[0034] The flame-retardant epoxy resin composite material has a tensile strength of 58.35-85.25 MPa, a flexural modulus of 2000.66-3228.50 MPa, and an impact strength of 6.57-12.33 KJ / m².
[0035] Another object of the present invention is to disclose the application of an epoxy resin composite material in the fields of aerospace, automotive industry, electronic packaging or coatings.
[0036] The ionic liquid flame retardant, epoxy resin composite material, their preparation method, and applications of this invention have the following advantages compared with existing technologies:
[0037] 1) This invention simultaneously introduces three flame-retardant elements—phosphorus (P), sulfur (S), and nitrogen (N)—into an ionic liquid. Through the synergistic flame-retardant effect of the PEPA structure, the nitrogen element on the cation, and the sulfur element on the anion, the flame-retardant properties of the epoxy resin are significantly improved. Experimental data show that when the addition amount is 10 parts, the limiting oxygen index (LOI) of the epoxy resin composite material increases from 22.3% to 29.3%, achieving the UL-94 V-0 rating.
[0038] 2) Improved compatibility and enhanced mechanical properties: This invention introduces amino groups that can participate in the curing of epoxy resin into the ionic liquid structure, enabling them to chemically bond into the resin network. This effectively solves the problems of poor compatibility and easy migration of traditional flame retardants. Results show that adding an appropriate amount of this ionic liquid (such as EP-4) can significantly improve the mechanical properties of the composite material. Tensile strength, flexural modulus, and impact strength can be increased by up to 46.10%, 57.43%, and 87.67% respectively compared to pure epoxy resin.
[0039] 3) The method for preparing ionic liquid flame retardants provided by this invention is simple, the raw materials are readily available, the reaction conditions are mild (room temperature to 60°C), the solvents used are conventional, the post-processing is simple, and the yield is high (up to 92.3%).
[0040] The ionic liquid flame retardant of this invention has both good flame retardant properties and the effect of enhancing the mechanical properties of epoxy resin, and has good application prospects and large-scale promotion potential in the field of epoxy resin composite materials. Attached Figure Description
[0041] Figure 1 The infrared spectrum of the ionic liquid flame retardant [PMoam]Ps in Example 1;
[0042] Figure 2 The 1H NMR spectrum of the ionic liquid flame retardant [PMoam]Ps in Example 1;
[0043] Figure 3 The mass spectrum of the ionic liquid flame retardant [PMoam]Ps in Example 1 is shown.
[0044] Figure 4 This is a schematic diagram of tensile strength.
[0045] Figure 5 This is a schematic diagram of the flexural modulus;
[0046] Figure 6 This is a schematic diagram of impact strength.
[0047] Figure 7 This is a process flow diagram of the present invention. Detailed Implementation
[0048] The present invention will be further described below with reference to embodiments. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:
[0049] Unless otherwise stated, all units used in this specification are international standard units, and all numerical values and ranges appearing in this invention should be understood to include systematic errors that are unavoidable in industrial production.
[0050] In this specification, the range of values referred to as "value A to value B" refers to the range including the endpoint values A and B.
[0051] In this specification, the numerical range indicated by "above" or "below" refers to the numerical range that includes the stated number.
[0052] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.
[0053] In this specification, the terms "optional" or "optional" are used to indicate the use or omission of certain substances, components, procedures, application conditions, etc.
[0054] In this instruction manual, when "room temperature" or "room temperature" is used, the temperature can be 15-25℃.
[0055] Unless otherwise specified, all reagents or instruments used in this instruction manual are commercially available products.
[0056] Example 1
[0057] This embodiment discloses an ionic liquid flame retardant, the preparation method of which is as follows: Figure 7 As shown, it includes the following steps:
[0058] S1. First, 50 mL of dichloromethane, 10.3 g (0.1 mol) of triethylamine, and 18.0 g (0.1 mol) of PEPA were placed in a three-necked flask. 14.2 g (0.1 mol) of propylsulfonyl chloride was added dropwise over 1 hour at atmospheric pressure. After the addition was complete, the mixture was stirred at room temperature for 2 hours. After the reaction was complete, dichloromethane was removed by vacuum distillation. The product was dispersed in water, sonicated for 3 minutes, washed with water and filtered three times, and dried under vacuum at 80°C for 24 hours to obtain 14.6 g of white solid powder PEPA-Ps, with a yield of 51.2%.
[0059] S2. Place 50 mL of acetonitrile and 28.6 g (0.1 mol) of PEPA-Ps into a three-necked flask. After the PEPA-Ps dissolves, add 14.4 g (0.1 mol) of aminopropylmorpholine and stir at 60 °C for 24 hours. After the reaction is complete, remove the acetonitrile by vacuum distillation.
[0060] Vacuum drying at 80℃ for 24 hours yielded 39.7 g of pale yellow flaky solid, with a yield of 92.3%.
[0061] The synthetic route of the ionic liquid flame retardant [PMoam]Ps of this invention is as follows:
[0062]
[0063] The infrared spectrum, proton NMR spectrum, and mass spectrum of the obtained ionic liquid product are shown in Figures 1-3. It can be seen that the infrared spectrum of the ionic liquid flame retardant in this embodiment is at 3401 cm⁻¹. -1 The peak at 2970 cm⁻¹ is a broad peak of NH stretching vibration. -1 This is a CH stretching symmetric peak, 1164 cm⁻¹. -1 1002cm -1 and 818cm -1 SO - The stretching vibration, P=O stretching symmetry and POC stretching symmetry. 1 The absorption peaks (f, g, h, i, and j) of the [PMoam]Ps NMR spectrum are attributed to the proton peaks of hydrogen atoms at positions f, g, h, i, and j on the [PMoam]Ps spectrum. 13 The C10 NMR spectrum perfectly matches the theoretical peak positions. The mass spectrum of [PMoam]Ps is shown in the figure, and the results of the mass spectrometry analysis of the fracture structure of [PMoam]Ps are also consistent with the theoretical relative molecular weight of [PMoam]Ps. The above tests confirm the successful preparation of the target ionic liquid [PMoam]Ps.
[0064] Examples 2-6
[0065] Examples 2-6 disclose various flame-retardant epoxy resin composite materials [PMoam]Ps / DDM / EP, and their preparation methods are as follows:
[0066] A measured amount of bisphenol A type epoxy resin (E-51) and the ionic liquid flame retardant [PMoam]Ps from Example 1 were placed in a beaker and mixed thoroughly. A measured amount of molten curing agent, 4,4-diaminodiphenylmethane (DDM), was added to the beaker, mechanically stirred, and then degassed under vacuum. Curing was performed at 69°C for 2 hours, 113°C for 4 hours, and 145°C for 2 hours. The epoxy resin composite system is shown in Table 1.
[0067] Table 1 Flame-retardant epoxy resin composites
[0068]
[0069] The flame-retardant epoxy resin composite materials of Examples 2-6 and Comparative Example 1 were tested respectively. The test methods and test results are as follows:
[0070] The flame retardant properties of the [PMoam]Ps / DDM / EP composite material were comprehensively evaluated using the Limiting Oxygen Index (LOI) test and the UL-94 vertical burning test. Table 2 shows the Limiting Oxygen Index (LOI) and UL-94 vertical burning test results for the [PMoam]Ps / DDM / EP composite material system. As shown in Table 2, in the LOI test, the LOI value of pure EP was 22.3%. With the increase of [PMoam]Ps addition, the LOI of the epoxy resin composite material increased significantly, with the LOI of EP-5 reaching 29.3%, and the UL-94 vertical burning test achieving a V-0 rating.
[0071] Table 2 Limiting oxygen index and UL-94 vertical burning data of flame-retardant epoxy resin composites
[0072]
[0073] Comparative Example 1: Mechanical properties of pure epoxy resin EP-0 and epoxy resin composites with different amounts of [PMoam]Ps are as follows Figure 4-6As shown in the figure. According to the experimental results, the tensile strength of the epoxy resin composite material first increases and then decreases with the increase of the amount of ionic liquid [PMoam]Ps. The tensile strength of pure epoxy resin EP-0 is 58.35 MPa, while the highest tensile strength of EP-4 sample is 85.25 MPa, which is 46.10% higher than EP-0. Regarding flexural properties, the flexural modulus of EP-0 is 2000.66 MPa, while the highest flexural modulus of EP-4 sample is 3228.50 MPa, which is 57.43% higher than EP-0. Regarding impact properties, the impact strength of EP-0 is 6.57 KJ / m. 2 The highest impact strength of the EP-4 sample was 12.33 KJ / m. 2 EP-0 improved by 87.67%.
[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an ionic liquid flame retardant, characterized in that, Includes the following steps: S1. Solvent, acid-binding agent and pentaerythritol phosphate are added to the reaction vessel, and then alkyl sulfonyl chloride compound is added dropwise to carry out the reaction. After the reaction is completed, the mixture is separated and purified to obtain the intermediate PEPA-Ps. S2. The intermediate PEPA-Ps is dissolved in an organic solvent and reacted with an amino-containing heterocyclic compound. After the reaction is completed, the mixture is separated and purified to obtain the ionic liquid flame retardant.
2. The method for preparing the ionic liquid flame retardant according to claim 1, characterized in that, In step S1, the solvent is one or more selected from dichloromethane, dichloroethane, chloroform, carbon tetrachloride, cyclohexane, and petroleum ether. And / or, the acid-binding agent is one or more of triethylamine, pyridine, and N,N-diisopropylethylamine; And / or, the alkyl sulfonyl chloride compound is propyl sulfonyl chloride and / or ethyl sulfonyl chloride; And / or, the molar ratio of the pentaerythritol phosphate, the acid-binding agent, and the alkyl sulfonyl chloride compound is 1:1-1.5:1-1.
5.
3. The method for preparing the ionic liquid flame retardant according to claim 1, characterized in that, In step S1, the reaction temperature is room temperature and the reaction time is 2-4 hours.
4. The method for preparing the ionic liquid flame retardant according to claim 1, characterized in that, In step S1, the separation and purification includes: removing the solvent by vacuum distillation, dispersing in water, ultrasonic oscillation, washing and filtering with water, and drying under vacuum conditions.
5. The method for preparing the ionic liquid flame retardant according to claim 1, characterized in that, In step S2, the amino-containing heterocyclic compound is selected from one or more of N-aminopropylmorpholine, 1-(3-aminopropyl)imidazolium, and 2-aminopyridine; And / or, the organic solvent is one or more of acetonitrile, 1,4-dioxane, and N,N-dimethylformamide; And / or, the molar ratio of the intermediate PEPA-Ps to the amino-containing heterocyclic compound is 1:1-1.
2.
6. The method for preparing the ionic liquid flame retardant according to claim 1, characterized in that, In step S2, the reaction temperature is 40-60℃ and the reaction time is 24-48 hours.
7. An ionic liquid flame retardant, characterized in that, It is prepared by any one of the preparation methods described in claims 1-6.
8. A flame-retardant epoxy resin composite material, characterized in that, It includes epoxy resin, curing agent and the ionic liquid flame retardant as described in claim 7.
9. The flame-retardant epoxy resin composite material according to claim 8, characterized in that, The amount of ionic liquid flame retardant added is 2-10 wt.%.
10. The application of the flame-retardant epoxy resin composite material of claim 8 in the fields of aerospace, automotive industry, electronic packaging or coatings.