Efficient leaching method for waste lithium battery positive electrode material based on electron beam rapid oxidation and application of efficient leaching method
By treating the slurry with electron beam irradiation technology, and utilizing the hydrogen ions and free radicals generated by carboxylate salts for rapid oxidation-reduction, the problems of high energy consumption and high cost in the recycling of lithium battery cathode materials are solved, achieving efficient and environmentally friendly leaching of lithium ions.
Patent Information
- Application Number
- CN202610280889.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-09
- Publication Date
- 2026-05-26
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery recycling, specifically to an efficient leaching method for waste lithium battery cathode materials based on rapid electron beam oxidation and its application. Background Technology
[0002] With the increasing demand for new energy vehicles and energy storage, the annual production of lithium-ion batteries has exceeded 1 TWh, leading to a surge in the retirement of these batteries. The mainstream recycling process for lithium-ion batteries is wet leaching, which currently requires a large amount of chemical reagents. Hydrogen peroxide is used to oxidize metal ions and increase leaching efficiency, but this also increases production costs and wastewater generation. Furthermore, the leaching process typically requires heating, often using continuous steam injection, resulting in high energy consumption.
[0003] Based on this, the present invention is proposed. Summary of the Invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes an efficient leaching method for waste lithium-ion battery cathode materials based on rapid electron beam oxidation and its application. This method utilizes electron beam irradiation for rapid oxidation-reduction to achieve efficient recycling of waste lithium-ion battery cathode materials.
[0005] According to a first aspect of the present invention, a method for leaching lithium battery cathode material is provided, comprising the following steps: S1: Mix black powder with water and carboxylates to prepare the first slurry; S2: After electron beam irradiation of the first slurry, carbon dioxide is introduced, and after solid-liquid separation, a lithium bicarbonate solution is obtained.
[0006] In some embodiments, in step S1, the black powder is selected from lithium iron phosphate black powder.
[0007] Electron irradiation technology can ionize water molecules in the slurry, generating hydroxyl radicals, oxygen radicals, and H·, thereby oxidizing iron ions in lithium iron phosphate into trivalent metal ions, reducing the difficulty of lithium ion leaching. The presence of carboxylates can combine with hydrogen ions generated by water ionization to form formic acid. Formic acid, under irradiation conditions, forms carbon dioxide, which combines with lithium ions to form lithium carbonate. This, along with the strong oxidizing effect of hydroxyl and oxygen radicals, promotes lithium ion leaching. Lithium carbonate further reacts with carbon dioxide to form readily soluble lithium bicarbonate, thus achieving the separation of lithium from the solid phase.
[0008] In some embodiments, in step S1, the solid-liquid ratio of the black powder to water is (30~50) g: 1 L.
[0009] In some embodiments, in step S1, the carboxylate is selected from at least one of sodium carboxylate, lithium carboxylate, or ferric carboxylate; and / or, the mass of the carboxylate is 10% to 30% of the mass of the black powder.
[0010] In some embodiments, in step S2, the first slurry is irradiated with an electron beam in the form of a thin layer, the thickness of the thin layer being 1 to 4 cm, and the flow rate of the slurry being 50 to 100 m / min.
[0011] In some embodiments, in step S2, the energy of the electron beam irradiation is 1~10MeV, and the dose is 100~1000kGy.
[0012] In some preferred embodiments, in step S2, the electron beam irradiation treatment is performed 2 to 5 times.
[0013] In some embodiments, in step S2, the carbon dioxide flow rate is 15-20 L / min.
[0014] In some embodiments, in step S2, the solid-liquid separation is achieved by pressure filtration, and the pressure of the pressure filtration is 0.8~1.5MPa.
[0015] In some embodiments, the lithium battery cathode material leaching method further includes the following steps: S3: Mix the solid obtained after solid-liquid separation in step S2 with water to prepare a second slurry, and repeat step S2 with the second slurry to obtain a second lithium bicarbonate solution.
[0016] According to a second aspect of the present invention, the application of the lithium battery cathode material leaching method described in the first aspect of the present invention in the recycling of waste lithium-ion batteries is proposed. Compared with conventional acid leaching, the leaching method of the present invention can be carried out at room temperature and does not require the addition of hydrogen peroxide, reducing the generation of waste liquid, effectively reducing costs and benefiting the environment.
[0017] According to one embodiment of the present invention, at least the following beneficial effects are achieved: This invention utilizes electron beam irradiation technology to treat cathode material black powder in slurry form. It leverages carboxylates to compete with water for hydrogen ions generated under irradiation, converting them into carbon dioxide. This allows oxygen free radicals to generate oxidation, achieving rapid oxidation of iron ions in lithium iron phosphate and reducing the use of hydrogen peroxide. Simultaneously, electron beam irradiation can promote lithium ion leaching at room temperature, lowering the temperature requirements of wet leaching and thus reducing steam consumption. Detailed Implementation
[0018] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.
[0019] Unless otherwise specified, the experimental methods in the following examples or comparative examples were carried out according to conventional methods and conditions. Unless otherwise specified, the raw materials, reagents, or apparatus used in the following examples or comparative examples can be obtained from conventional commercial sources or by existing known methods. The main components of the lithium iron phosphate black powder are as follows: lithium iron phosphate (90%), PVDF binder (4%-6%), conductive carbon black, and graphite (4%-6%).
[0020] Example 1 This embodiment provides a highly efficient leaching method for waste lithium battery cathode materials based on rapid electron beam oxidation, including the following steps: Lithium iron phosphate black powder was mixed with water to form a slurry with a solid content of 30 g / L. Sodium formate (mass ratio of sodium formate to black powder was 1:5) was then added. The slurry was flowed through the electron beam region at a depth of 4 cm and a flow rate of 80 m / min. The electron beam irradiation energy was 10 MeV, the dose was 1000 kGy, and the process was repeated three times. Carbon dioxide was introduced into the electron-irradiated slurry at a flow rate of 18 L / min, and then the slurry was filtered in a filter press at a pressure of 1 MPa. The main component of the filtrate was lithium bicarbonate. The solid obtained from the filter press was mixed with water again to form a slurry with a solid content of 30 g / L. This slurry was then irradiated again under the same conditions and filtered to obtain insoluble matter. The filtrates from the two filtrations were combined.
[0021] Example 2 This embodiment provides a highly efficient leaching method for waste lithium battery cathode materials based on rapid electron beam oxidation, including the following steps: Lithium iron phosphate black powder was mixed with water to form a slurry with a solid content of 40 g / L. Lithium formate (lithium formate to black powder mass ratio 1:4) was then added. The slurry was flowed through the electron beam region at a depth of 2 cm and a flow rate of 60 m / min. The electron beam irradiation energy was 2 MeV, the dose was 200 kGy, and the process was repeated three times. Carbon dioxide was introduced into the electron-irradiated slurry at a flow rate of 20 L / min, and then the slurry was filtered in a filter press at a pressure of 1 MPa. The main component of the filtrate was lithium bicarbonate. The solid obtained from the filter press was mixed with water again to form a slurry with a solid content of 40 g / L. This slurry was then irradiated again under the same conditions and filtered to obtain insoluble matter. The filtrates from the two filtrations were combined.
[0022] Example 3 This embodiment provides a highly efficient leaching method for waste lithium battery cathode materials based on rapid electron beam oxidation, including the following steps: Lithium iron phosphate black powder was mixed with water to form a slurry with a solid content of 30 g / L. Ferric formate (mass ratio of ferric formate to black powder was 1:10) was then added. The slurry was flowed through the electron beam region at a depth of 3 cm and a flow rate of 50 m / min. The electron beam irradiation energy was 3 MeV, the dose was 300 kGy, and the process was repeated three times. Carbon dioxide was introduced into the electron-irradiated slurry at a flow rate of 15 L / min, and then the slurry was filtered in a filter press at a pressure of 1 MPa. The main component of the filtrate was lithium bicarbonate. The solid obtained from the filter press was mixed with water again to form a slurry with a solid content of 30 g / L. This slurry was then irradiated again under the same conditions and filtered to obtain insoluble matter. The filtrates from the two filtrations were combined.
[0023] Comparative Example 1 The difference between this comparative example and Example 1 is that sodium formate is not added to the slurry, while all other conditions are the same.
[0024] Comparative Example 2 This comparative example provides a leaching method for waste lithium battery cathode materials, including the following steps: Lithium iron phosphate black powder and sulfuric acid were mixed at a mass ratio of 1:8, with a sulfuric acid molar concentration of 2 mol / L. Hydrogen peroxide with a molar concentration of 30% (the amount of hydrogen peroxide was 30% of the mass of lithium iron phosphate black powder) was added, and the solution was heated to 70°C and reacted for 1 hour. The slurry obtained by wet leaching was then put into a filter press for filtration. The solid obtained by filtration was then mixed with sulfuric acid again in the above ratio to prepare a slurry. After acid leaching at 70°C for 1 hour, the slurry was filtered again to obtain insoluble matter. The filtrates from the two filtrations were combined.
[0025] Test case The insoluble matter and filtrate of each embodiment and comparative example were tested, and the results are shown in Table 1 below. The insoluble matter included ferric phosphate, PVDF binder, conductive carbon black, and graphite; slag content = m 不溶物 / m 磷酸铁锂黑粉 *100%; The mass m of lithium element in lithium iron phosphate black powder was determined by its composition. Li The lithium concentration c in the filtrate Li The lithium recovery rate was obtained from ICP measurements and then calculated as c. Li *V 滤液 / m Li *100%.
[0026] As shown in the table below, the lithium recovery rate of Comparative Example 1 is relatively low. This is because Comparative Example 1 does not add carboxylates, thus failing to promote lithium ion leaching. Comparative Example 2, using conventional acid leaching, achieves a lithium recovery rate close to that of the examples, but this requires heating and consumes a certain amount of hydrogen peroxide. Furthermore, ferric phosphate does not leach during the treatment described in the examples, while it does during the treatment in Comparative Example 2, affecting subsequent ferric phosphate recovery and lithium purification.
[0027] Table 1
[0028] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.
Claims
1. A method for leaching lithium battery cathode material, characterized in that, Includes the following steps: S1: Mix black powder with water and carboxylates to prepare the first slurry; S2: After electron beam irradiation of the first slurry, carbon dioxide is introduced, and solid-liquid separation is performed to obtain the first lithium bicarbonate solution.
2. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S1, the black powder is selected from lithium iron phosphate black powder.
3. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S1, the solid-liquid ratio of the black powder to water is (30~50) g: 1 L.
4. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S1, the carboxylate is selected from at least one of sodium carboxylate, lithium carboxylate, or iron carboxylate; and / or, the mass of the carboxylate is 10% to 30% of the mass of the black powder.
5. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S2, the first slurry is irradiated with an electron beam in the form of a thin layer, the thickness of the thin layer is 1~4cm, and the flow rate of the slurry is 50~100m / min.
6. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S2, the energy of the electron beam irradiation is 1~10MeV, and the dose is 100~1000kGy.
7. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S2, the carbon dioxide flow rate is 15~20 L / min.
8. The lithium battery cathode material leaching method according to claim 1, characterized in that, In step S2, the solid-liquid separation is achieved by pressure filtration, and the pressure of the pressure filtration is 0.8~1.5MPa.
9. The lithium battery cathode material leaching method according to claim 1, characterized in that, It also includes the following steps: S3: Mix the solid obtained after solid-liquid separation in step S2 with water to prepare a second slurry, and repeat step S2 with the second slurry to obtain a second lithium bicarbonate solution.
10. The application of the lithium battery cathode material leaching method according to any one of claims 1-9 in the recycling of waste lithium-ion batteries.