A method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore

By using a roasting oxidation method and an ammonia-ethylenediaminetetraacetic acid mixed leaching system, the problem of inefficient recovery of copper and molybdenum from molybdenum ore ammonia leaching tailings was solved, achieving high leaching rates and selective recovery, simplifying the process and reducing environmental risks.

CN122081661APending Publication Date: 2026-05-26KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610375693.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-25
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the efficient and coordinated recovery of copper and molybdenum from ammonia leaching tailings in molybdenum mines, leading to resource waste and environmental pollution. Furthermore, conventional methods suffer from poor selectivity, strong corrosiveness, complex processes, and high costs.

Method used

Molybdenum ore tailings were pretreated by roasting oxidation, followed by leaching using an ammonia-ethylenediaminetetraacetic acid mixture system. The leaching process was adjusted to improve the leaching rates of copper and molybdenum.

Benefits of technology

It achieves efficient synergistic recovery of copper and molybdenum with a leaching rate of over 96%, reduces impurity content, simplifies the process, and aligns with the development direction of green metallurgy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for extracting copper and molybdenum from ammonia leaching tailings of molybdenum ore, belonging to the field of comprehensive tailings utilization. Addressing the technical problem of low copper and molybdenum leaching rates in the resource utilization of ammonia leaching tailings of molybdenum ore, this invention specifically includes the following steps: pretreating the ammonia leaching tailings of molybdenum ore using a roasting oxidation method to obtain roasted sand; leaching the roasted sand using a composite leaching system composed of ammonia water and ethylenediaminetetraacetic acid, simultaneously extracting copper and molybdenum from the roasted sand; this invention achieves a copper and molybdenum leaching rate of over 96% from ammonia leaching tailings of molybdenum ore, with a simple process flow, eliminating the need for large amounts of strong acids, strong alkalis, or other highly corrosive reagents, and enabling efficient comprehensive recovery of copper and molybdenum from the tailings, providing technical guidance for the comprehensive utilization of ammonia leaching tailings of molybdenum ore.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of tailings comprehensive utilization technology, specifically relating to a method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum mines. Background Technology

[0002] Molybdenum, a strategically important metal with high melting point, high strength, and high conductivity, is an indispensable key material in the steel industry, high-end equipment manufacturing, new energy batteries, and aerospace. Globally, my country holds approximately 39% of the world's total molybdenum reserves, ranking first in the world. my country's molybdenum ores are mostly sulfide ores (such as molybdenite MoS2), often accompanied by valuable metals such as Cu, W, Bi, Se, Pb, Zn, Ag, and Au. However, the grade of molybdenum deposits in my country is generally low, limiting the comprehensive recovery rate of molybdenum and associated valuable components such as copper during beneficiation and smelting. A large amount of valuable metals are lost with the tailings from smelting processes, and the high-value resource utilization of molybdenum smelting solid waste is still in the exploratory stage. The copper and molybdenum resources contained within these wastes possess extremely high comprehensive recovery value.

[0003] In the beneficiation and smelting of molybdenum ore, ammonia leaching is one of the main processes for processing molybdenum concentrate. Ammonia leaching can selectively dissolve molybdenum to obtain ammonium molybdate. However, this process generates a large amount of ammonia leaching tailings. The tailings not only contain unleached, insoluble molybdenum components, but also enriched with valuable metals such as copper that were associated with the original ore. Due to the complex occurrence and severe encapsulation of metals in the tailings, conventional leaching methods cannot achieve efficient and synergistic extraction of copper and molybdenum. As a result, a large amount of valuable metals end up in the tailings pond, which not only wastes resources but also increases the environmental burden.

[0004] Currently, domestic and international research and industrial explorations on the recovery of valuable metals from ammonia leaching tailings of molybdenum ore mainly focus on three categories: acid leaching, secondary flotation, and ammonia leaching. Among them, acid leaching mainly uses strong acids such as sulfuric acid and hydrochloric acid as the main leaching agents. Although it can leach some molybdenum and copper components under strong acid conditions, it has poor selectivity, high impurity dissolution rate, and strong corrosiveness to equipment. Secondary flotation can only recover residual sulfide minerals with good floatability in the tailings. It has a very poor recovery effect on oxidized molybdenum and copper species formed during ammonia leaching, and the overall recovery rate of valuable metals is generally low, making it impossible to achieve high-value utilization of tailings. The single ammonia leaching process is difficult to effectively destroy the stable phases of metals in the tailings, resulting in low leaching efficiency and failing to meet the economic and technical indicators for industrial recovery.

[0005] In summary, existing molybdenum ore ammonia leaching tailings treatment technologies all have significant technical shortcomings, failing to simultaneously meet the core requirements for industrial applications: high leaching rate, high selectivity, cleanliness and low corrosion, simple process, and controllable cost. Therefore, there is an urgent need to develop a technology for the efficient and simultaneous recovery of copper and molybdenum from molybdenum ore ammonia leaching tailings. This would improve the high-value utilization of difficult-to-treat molybdenum smelting tailings and effectively reduce the environmental risks and potential health hazards posed by tailings. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore, which addresses the shortcomings of the prior art. The method uses roasting oxidation to remove impurities from the tailings, and leaches molybdenum and copper from the roasted ore through an ammonia-ethylenediaminetetraacetic acid mixed system. By adjusting and optimizing the leaching process, the leaching rate of copper and molybdenum can reach more than 96%.

[0007] The above-mentioned technical objective of the present invention is achieved through the following technical solution: (1) Grind the ammonia leaching tailings of molybdenum ore into fine powder, roast it, and then let it cool naturally to room temperature after roasting to obtain roasted sand; (2) The calcined sand obtained in step (1) is further ground and added to the mixed leachate I. After stirring and leaching, liquid-solid separation and washing, ammonia leaching residue and ammonia leaching filtrate containing molybdenum and copper are obtained. The mixed leachate I is prepared by ammonia water and ethylenediaminetetraacetic acid.

[0008] Preferably, in step (1) of the present invention, the particles with a particle size of no more than 75µm in the finely ground molybdenum ore ammonia leaching tailings account for more than 80% of the total mass.

[0009] Preferably, the calcination conditions in step (1) of the present invention are: 450~600℃, calcination for 1~6h.

[0010] Preferably, in step (2) of the present invention, the calcined sand is further ground until the particles with a particle size of no more than 75µm account for more than 90% of the total mass.

[0011] Preferably, in step (2) of the present invention, the mass of the added calcined sand and the liquid-solid ratio of the leachate I are (2~6):1, in mL:g.

[0012] Preferably, in step (2) of the present invention: the concentration of ammonia in the mixed leachate I is 2~10 mol / L and the mass percentage concentration of ethylenediaminetetraacetic acid is 3~10%.

[0013] Preferably, in step (2) of the present invention, the stirring and leaching time is 2~12h.

[0014] The beneficial effects of this invention are as follows: (1) The present invention pretreats molybdenum tailings by roasting oxidation, which effectively destroys the encapsulation structure of gangue minerals on metal components in the tailings, changes the occurrence form of copper and molybdenum, and promotes the subsequent dissolution of copper and molybdenum.

[0015] (2) The present invention uses ammonia-ethylenediaminetetraacetic acid (EDTA) to form a leaching system for the synergistic leaching of copper and molybdenum in calcined sand, which significantly improves the leaching efficiency of copper and molybdenum in the leaching system; the leaching rate of copper and molybdenum can reach more than 96%, realizing the efficient synergistic recovery of the two.

[0016] (3) The present invention uses a weakly alkaline leaching system composed of ammonia and EDTA, which has excellent leaching selectivity for copper and molybdenum, and has almost no leaching effect on gangue impurities such as iron, calcium, aluminum and silicon in the tailings, effectively reducing the impurity content in the leachate; at the same time, it can further enrich valuable metals such as gold in the leaching tailings, reduce the burden of subsequent separation and purification, and also create favorable conditions for the cascade recovery of valuable metals such as gold in the tailings, thus improving the overall economic efficiency of the process.

[0017] (4) The process of this invention is simple, easy to operate, and the leaching system has low corrosivity, which is in line with the development direction of green metallurgy and has good application prospects. Detailed Implementation

[0018] To gain a deeper understanding and effective implementation, and to verify the significant role of the process optimization proposed in the treatment of molybdenum mine tailings, this invention is described in detail with specific implementation examples. It should also be noted that this invention is not limited to the examples listed below.

[0019] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased on the market or prepared by existing methods.

[0020] The elemental contents of the molybdenum ore ammonia leaching tailings treated in the following examples and comparative examples are shown in Table 1 below.

[0021] Example 1 (1) Grind the molybdenum ore ammonia leaching tailings until the particles with a size not greater than 75µm account for more than 80% of the total mass, and carry out roasting oxidation pretreatment under the conditions of roasting temperature of 600℃ and roasting time of 1h.

[0022] (2) Grind the calcined sand obtained in step (1) until the particles with a size not greater than 75µm account for more than 90% of the total mass. Add the ground calcined sand to the mixed leaching solution I according to the liquid-solid ratio (mL:g) of 2:1. Stir and leach at room temperature for 6 hours. After filtration and washing, the ammonia leaching residue and the ammonia leaching solution containing copper and molybdenum are obtained after liquid-solid separation. Leaching solution I is prepared by ammonia water and EDTA. The concentration of ammonia water in leaching solution I is 10.0mol / L and the mass concentration of EDTA is 3%. At this time, the copper leaching rate is measured to be 91.33% and the molybdenum leaching rate is 88.49%.

[0023] Example 2 (1) Grind the molybdenum ore ammonia leaching tailings until the particles with a size not greater than 75µm account for more than 80% of the total mass, and carry out roasting oxidation pretreatment under the conditions of roasting temperature of 450℃ and roasting time of 5h.

[0024] (2) Grind the calcined sand obtained in step (1) until the particles with a size not greater than 75µm account for more than 90% of the total mass. Add the ground calcined sand to the mixed leaching solution I according to the liquid-solid ratio (mL:g) of 6:1. Stir and leach at room temperature for 4 hours. After filtration and washing, the ammonia leaching residue and the ammonia leaching solution containing copper and molybdenum are obtained after liquid-solid separation. Leaching solution I is prepared by ammonia water and EDTA. The concentration of ammonia water in leaching solution I is 6.0mol / L and the mass concentration of EDTA is 5%. At this time, the copper leaching rate is measured to be 92.25% and the molybdenum leaching rate is 93.63%.

[0025] Example 3 (1) Grind the molybdenum ore ammonia leaching tailings until the particles with a size not greater than 75µm account for more than 80% of the total mass, and carry out roasting oxidation pretreatment under the conditions of roasting temperature of 550℃ and roasting time of 5h.

[0026] (2) Grind the calcined sand obtained in step (1) until the particles with a size of no more than 75µm account for more than 90% of the total mass. Add the ground calcined sand to the mixed leaching solution I according to the liquid-solid ratio (mL:g) of 4:1. Stir and leach at room temperature for 4 hours. After filtration and washing, the ammonia leaching residue and the ammonia leaching solution containing copper and molybdenum are obtained after liquid-solid separation. Leaching solution I is prepared by ammonia water and EDTA. The concentration of ammonia water in leaching solution I is 2.0mol / L and the mass concentration of EDTA is 10%. At this time, the copper leaching rate is measured to be 97.52% and the molybdenum leaching rate is 96.65%.

[0027] The specific embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.

[0028] Comparative Example 1 Compared with Example 1, this comparative example has the same other conditions, except that the concentration of ammonia in leachate I is 6.0 mol / L and the mass concentration of EDTA is 0%. Under these conditions, the copper leaching rate is 80.67% and the molybdenum leaching rate is 73.13%.

[0029] Comparative Example 2 Compared with Example 1, this comparative example has the same other conditions, except that the concentration of ammonia in leachate I is 0 mol / L and the mass concentration of EDTA is 5.0%. Under these conditions, the copper leaching rate is 50.67% and the molybdenum leaching rate is 58.43%.

[0030] In a standalone ammonia system, ammonia can react directly with copper to form a stable, soluble copper-ammonia complex [Cu(NH3)4]. 2+ Therefore, the copper leaching rate is relatively high (90.67%); molybdenum can form soluble ammonium molybdate (NH4)2MoO4 with ammonia, but the molybdenum leaching rate is low (80.13%), mainly because of sparingly soluble molybdates such as CaMoO4; the Ca in these minerals... 2+ It hardly forms stable complexes with NH3, and ammonia water has difficulty disrupting its crystal structure, thus preventing the effective release of molybdate.

[0031] In the ethylenediaminetetraacetic acid (EDTA) system alone, EDTA is a strong chelating agent, capable of forming highly stable 1:1 chelates with various metal ions. However, due to the large size of the EDTA molecule, its diffusion rate is limited, and for metal minerals with negatively charged surfaces or those encapsulated by other minerals, the direct chelation efficiency is relatively low, with copper leaching rates of 50.67% and molybdenum leaching rates of 58.43%.

[0032] In the ammonia-EDTA combined system, the coexistence of the two significantly alters the leaching equilibrium, primarily due to the formation of mixed complexes. These mixed complexes typically exhibit higher stability constants or better solubility than single-ligand complexes. For sparingly soluble molybdates such as CaMoO4 in tailings, ammonia alone cannot achieve effective decomposition, while EDTA can react with Ca... 2+ It forms a stable Ca-EDTA complex, which disrupts the mineral lattice and releases molybdate.

Claims

1. A method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore, characterized in that, Specifically, the following steps are included: (1) Grind the ammonia leaching tailings of molybdenum ore into fine powder, roast it, and then let it cool naturally to room temperature after roasting to obtain roasted sand; (2) The calcined sand obtained in step (1) is further ground and added to the mixed leachate I. After stirring and leaching, liquid-solid separation and washing, ammonia leaching residue and ammonia leaching filtrate containing molybdenum and copper are obtained. The mixed leachate I is prepared by ammonia water and ethylenediaminetetraacetic acid.

2. The method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore according to claim 1, characterized in that: In step (1), the particles with a particle size of no more than 75µm in the ammonia leaching tailings of molybdenum ore are ground to account for more than 80% of the total mass.

3. The method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore according to claim 1, characterized in that: The calcination conditions in step (1) are: 450~600℃, calcination for 1~6 hours.

4. The method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore according to claim 1, characterized in that: In step (2), the calcined sand is further ground until particles with a size of no more than 75µm account for more than 90% of the total mass.

5. The method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore according to claim 1, characterized in that: In step (2): the mass of calcined sand added and the liquid-solid ratio of leachate I are (2~6):1, in mL:g.

6. The method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore according to claim 1, characterized in that: In step (2): the concentration of ammonia in mixed leachate I is 2~10 mol / L and the mass percentage concentration of ethylenediaminetetraacetic acid is 3~10%.

7. The method for leaching copper and molybdenum from ammonia leaching tailings of molybdenum ore according to claim 1 or 6, characterized in that: In step (2): the stirring and leaching time is 2~12h.