A high-sealing bellows based on ultrasound-assisted five-layer electrodeposition and its preparation method

By combining a five-layer nickel-cobalt alloy and copper alternating composite structure with ultrasonic vibration-assisted deposition technology, the problems of densification of deposition layers, stable interlayer bonding, uniform wall thickness and high sealing performance in multilayer electrodeposited corrugated pipes have been solved. This has enabled the fabrication of corrugated pipes with high airtightness and structural stability, which are suitable for high-end fields such as aerospace, energy equipment and precision instruments.

CN122082058APending Publication Date: 2026-05-26NORTHEASTERN UNIV CHINA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610188793.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-10
Publication Date
2026-05-26

Smart Images

  • Figure CN122082058A_ABST
    Figure CN122082058A_ABST
Patent Text Reader

Abstract

This invention discloses a five-layer electrodeposited high-sealing corrugated pipe based on ultrasound assistance and its preparation method, belonging to the technical field of metal corrugated pipe manufacturing. It aims to solve the problem that in multi-layer electrodeposited corrugated pipes, it is difficult to effectively coordinate current density, surface quality, and interfacial bonding strength, leading to insufficient densification of the deposited layer, unstable interlayer bonding, poor wall thickness uniformity, and failure to meet airtightness standards, ultimately resulting in poor overall performance stability. This invention includes a five-layer composite structure in which the pipe wall is composed of alternating nickel-cobalt alloy and copper layers. Each layer of the five-layer composite structure undergoes ultrasonic vibration treatment during deposition. The corrugated pipe prepared by this invention has a uniform and dense deposited layer with good interlayer bonding. The five-layer alternating deposition layer composite structure not only achieves uniform stress transmission and dispersion, effectively delaying crack propagation and interfacial penetration, but also improves the uniformity of wall thickness distribution, enabling the corrugated pipe to exhibit higher structural stability and long-term reliability in a sealed environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of metal bellows manufacturing, specifically to an ultrasonic-assisted five-layer electrodeposition high-sealing bellows and its preparation method. Background Technology

[0002] As flexible functional components, bellows are widely used in aerospace, energy equipment, petrochemical plants, and precision instruments, primarily serving functions such as displacement compensation, pressure transmission, vibration absorption, and sealing. In high-end equipment and complex service environments, bellows typically need to operate stably for extended periods under cyclic loading conditions, placing higher demands on their airtightness, structural stiffness, and service reliability. With the development of equipment towards miniaturization, lightweighting, and high reliability, traditional bellows manufacturing technologies are gradually showing limitations in terms of precision control and performance consistency.

[0003] Currently, bellows are mostly manufactured using machining, hydroforming, or welding. While these methods are mature and widely applicable, they suffer from low material utilization, limited forming accuracy, and the weld area being prone to leakage and fatigue failure, making it difficult to meet the demands of high-end equipment for small size, high consistency, and high sealing performance. Therefore, electrodeposition forming technology has gradually attracted attention. This technology directly deposits metal or alloy materials on the surface of a cathode mandrel through an electrochemical reduction reaction, enabling the integrated forming of complex corrugated structures. It offers advantages such as mild processing, high dimensional consistency, and good wall thickness control, making it particularly suitable for the fabrication of miniaturized and high-precision bellows.

[0004] Existing electrodeposited bellows mostly employ a single-layer nickel or nickel-cobalt alloy structure. Nickel-cobalt alloys, due to their high strength, hardness, and corrosion resistance, are widely used in the fabrication of electrodeposited bellows. However, during actual deposition, hydrogen evolution commonly occurs on the cathode surface. These bubbles easily adhere to the deposition interface and become encapsulated within the deposition layer, forming microporous defects that severely affect the airtightness of the bellows. Furthermore, single-layer deposition structures are prone to localized stress concentration and microcrack propagation under high pressure or cyclic loading, leading to reduced sealing performance and service life.

[0005] To improve the defects of single-layer structures, Chinese invention patent application CN103540981A discloses a multilayer thin-walled electrodeposited corrugated pipe and its processing method. This technology employs a three-layer structure: inner, middle, and outer layers. The inner and outer layers are pure nickel or nickel-cobalt alloy layers, and the middle layer is metallic copper. By alternately depositing different metal or alloy layers, a layered composite structure is constructed to improve stress distribution and inhibit crack propagation. During processing, copper is first flash-plated as a base, followed by the sequential deposition of a nickel / nickel-cobalt layer, a copper layer, and another nickel / nickel-cobalt layer. After demolding, the inner copper layer is removed by nitric acid cleaning. The dense crystalline structure of the copper layer fills the porosity of the nickel layer, increasing the airtightness compliance rate to 60% and the operating temperature to 300℃. This alleviates internal stress concentration to a certain extent and improves the overall density of the deposited layers, thereby enhancing the comprehensive performance of the corrugated pipe.

[0006] However, this existing technology still has the following limitations: In terms of interlayer bonding, the interlayer interface mass transfer conditions of the three-layer structure are insufficient, the difference in deposition kinetics of different metal layers leads to uneven microstructure, and the electrolyte system has poor fluidity in complex corrugated areas, which further aggravates the interlayer defects and uneven wall thickness. Under vibration, impact and other working conditions, delamination failure is likely to occur, affecting the overall performance consistency. Regarding bubble defects and mass transfer, the deposition process was controlled solely by adjusting electrochemical parameters such as current density and electrolyte composition, without addressing the localized mass transfer dead zones within the complex wavy structure (peaks / troughs). Hydrogen bubbles easily become trapped at interlayer interfaces, forming micropores, resulting in a gas tightness compliance rate of only 60% and a leakage rate of 1×10⁻⁶. -10 At the Pa³ / s level, the significant difference in deposition thickness between the crest and trough regions affects the fatigue performance of the product.

[0007] Furthermore, existing technologies primarily improve deposition quality by controlling electrochemical parameters such as current density, voltage, solution composition, and additives. However, their effects on localized mass transfer enhancement and bubble desorption at the deposition interface are limited, making it difficult to achieve stable and uniform densification in multilayer composite structures. Although some studies have attempted to introduce ultrasonic vibrations into the electrodeposition process to enhance mass transfer and suppress porosity formation, related applications are mostly limited to simple structural components. There is insufficient synergistic control over different deposition stages and interlayer interfaces in multilayer electrodeposited corrugated pipes. On the one hand, ultrasonic action exhibits significant spatial inhomogeneity in complex corrugated structures, leading to significant differences in deposition quality at peaks, troughs, and between inner and outer walls. On the other hand, while ultrasonic cavitation promotes dehydrogenation and grain refinement, it can easily disturb the already formed multilayer interfaces, affecting the stability of interlayer bonding. Moreover, the enhanced electrochemical reactions induced by ultrasound are difficult to coordinate with layer thickness control and material switching during multilayer deposition, making it difficult to simultaneously achieve both density and sealing of the deposition layer. Existing technologies cannot solve this problem by simply adjusting ultrasonic power or through limited experimental optimization.

[0008] The stiffness of corrugated pipes made from the same material increases with increasing wall thickness, and different applications require corrugated pipes with different stiffnesses. With the total thickness remaining constant, multi-layer structures can significantly improve the airtightness of corrugated pipes compared to single-layer structures. The core challenge of expanding from 3 layers to 5 layers is not simply the addition of layers, but how to maintain uniform wall thickness and good interlayer bonding even after increasing the number of layers. This is also the key bottleneck that existing technologies have not been able to effectively overcome.

[0009] Therefore, conventional improvement approaches have limited effectiveness: simply increasing the number of layers leads to the accumulation of interlayer defects and a decrease in airtightness; simply changing the electrolyte cannot solve the problem of mass transfer dead zones; and using ultrasound alone cannot improve stress concentration in multilayer structures. Multilayer electrodeposition structures have certain advantages in improving stress distribution, inhibiting crack propagation, and enhancing airtightness, but current research is not systematic, process parameters are scattered, and mature methods are lacking. It is difficult to effectively coordinate the deposition rate, composition ratio, and interfacial bonding strength between different layers, resulting in insufficient overall performance stability, especially in the design of structures with five or more layers, which is still in its infancy.

[0010] In summary, existing technologies cannot simultaneously achieve a synergistic improvement in deposit layer densification, interlayer bonding stability, wall thickness uniformity, and high sealing performance. Therefore, there is an urgent need to further optimize the technical solutions to meet the application requirements of high-end equipment. Summary of the Invention

[0011] To address the shortcomings of existing technologies, this invention aims to solve the problem of difficulty in effectively coordinating deposition rate, composition ratio, and interfacial bonding strength in multilayer electrodeposited corrugated pipes. This leads to insufficient densification of the deposited layer, unstable interlayer bonding, poor wall thickness uniformity, and failure to meet airtightness standards, ultimately resulting in poor overall performance stability. This invention proposes a five-layer electrodeposited high-sealing corrugated pipe based on ultrasound-assisted deposition and its preparation method. Through the synergistic design of a five-layer nickel-cobalt alloy and copper alternating composite structure and ultrasound vibration-assisted deposition technology, the mass transfer conditions and bubble behavior at the deposition interface are controlled, the formation of porosity defects is suppressed, and the densification and bonding stability of the deposited layer and interlayer interfaces are improved. This optimizes airtightness, structural stiffness, and long-term service reliability. The corrugated pipe wall is a five-layer composite structure with alternating nickel-cobalt alloy and copper layers. Each layer of the five-layer composite structure undergoes ultrasonic vibration treatment during deposition, including the following steps: S1. Pre-treatment of core mold: After mechanical polishing, the core mold is assembled into a core mold assembly, and then subjected to alkaline washing, pickling, repeated alkaline washing, repeated pickling, and zinc immersion treatment in sequence. S2. Pre-plating copper treatment: The core mold assembly is placed into a special copper deposition fixture and placed in a copper deposition tank for pre-plating copper. After deposition, it is rinsed with tap water and then placed in an ultrasonic cleaner for deep cleaning with deionized water. S3. Five-layer composite structure deposition: The first nickel-cobalt alloy layer, the second copper layer, the third nickel-cobalt alloy layer, the fourth copper layer, and the fifth nickel-cobalt alloy layer are deposited sequentially. During each deposition, the core mold assembly is first loaded into the corresponding deposition tooling and then placed into the corresponding deposition tank. The corresponding deposition tanks are placed in an ultrasonic vibration tank, and tap water is used as the medium for ultrasonic vibration propagation for deposition. After each layer of deposition, the core mold assembly is first rinsed with tap water, and then placed in an ultrasonic cleaner for deep cleaning with deionized water. S4. Copper plating protection treatment: The core mold assembly is placed into a special copper deposition tooling and placed in a copper deposition tank for pre-copper plating. After deposition, it is rinsed with tap water to obtain a semi-finished corrugated pipe containing the core mold assembly. S5. Demolding process: Transfer the semi-finished corrugated pipe to the lathe, drill a hole in the center of the core mold assembly, then put it into the demolding solution to dissolve it. After the core mold assembly is completely dissolved, put it into an ultrasonic cleaner for deep cleaning with deionized water. S6. Copper Removal Treatment: The semi-finished corrugated pipe is placed in a copper removal solution to remove the protective copper layer on the inner and outer surfaces of the semi-finished corrugated pipe. After deep cleaning with deionized water in an ultrasonic cleaner, it is dried to obtain a five-layer electrodeposited high-sealing corrugated pipe.

[0012] A further feature of the present invention is that, in step S1, the core mold is made of 2A12 aluminum alloy with a surface roughness Ra ≤ 1.6 μm; The alkaline washing solution contains 10-25 g / L sodium hydroxide, 35-50 g / L sodium carbonate, and 20-30 g / L trisodium phosphate. The solution temperature is 60-80℃, and the alkaline washing time is 20-30 seconds. The pickling solution is a diluted concentrated nitric acid with a concentration of 500 ml / L and a mass fraction of 68%. Pickling is performed at room temperature for 30-60 seconds. Repeat the alkaline washing for 15-20 seconds, and repeat the acid washing for 20-30 seconds; The zinc immersion solution contains 400-550 g / L sodium hydroxide, 50-120 g / L zinc oxide, 10-50 g / L sodium potassium tartrate, 0.1-2 g / L ferric chloride, and 0.5-1.5 g / L sodium nitrate. The zinc is immersed for 40 seconds at room temperature.

[0013] A further provision of the present invention is as follows: In step S3, when depositing the first, third, and fifth nickel-cobalt alloy layers, the anode material is a low-sulfur nickel bead with a diameter of 10 mm. The corresponding electrolyte in the nickel deposition tank is an aminosulfonate system, comprising 500-650 g / L nickel aminosulfonate, 7-19 g / L cobalt aminosulfonate, 10-15 g / L nickel chloride, 35-40 g / L boric acid, and 0.15-0.20 g / L sodium dodecyl sulfate. The deposition parameters are: anode-cathode spacing of 365 mm, temperature of 60 °C, pH adjusted to 4 with potassium hydroxide, and current density of 0.4 A / dm³. 2 The circulation flow rate is 5400 ml / min.

[0014] A further provision of the present invention is as follows: In steps S2-S4, when depositing the pre-plated copper layer, the second copper layer, and the fourth copper layer, the anode material is a phosphorus-containing copper ball with a diameter of 25 mm. The corresponding electrolyte in the copper deposition tank is an organic polyphosphoric acid system containing 50-60 g / L of hydroxyethylidene diphosphonic acid, 10-20 g / L of copper sulfate, and 40-60 g / L of potassium carbonate. The deposition parameters are: anode-cathode spacing of 365 mm, temperature of 50 °C, pH adjusted to 9 with potassium hydroxide, and current density of 0.4 A / dm³. 2 The circulation flow rate is 5400 ml / min.

[0015] A further provision of the present invention is that, in step S3, the deposition times for each layer are as follows: 2 hours for the first nickel-cobalt alloy layer, 6 hours for the second copper layer, 4 hours for the third nickel-cobalt alloy layer, 8 hours for the fourth copper layer, and 4 hours for the fifth nickel-cobalt alloy layer. The total wall thickness of the five-layer composite structure is 0.03-0.15 mm. Specifically, the thickness of the first nickel-cobalt alloy layer accounts for 18-22% of the total wall thickness, the thickness of the second copper layer accounts for 15-18% of the total wall thickness, the thickness of the third nickel-cobalt alloy layer accounts for 25-30% of the total wall thickness, the thickness of the fourth copper layer accounts for 18-22% of the total wall thickness, and the thickness of the fifth nickel-cobalt alloy layer accounts for 18-22% of the total wall thickness.

[0016] A further feature of the present invention is that, in step S5, the demolding solution is a potassium hydroxide solution with a concentration of 180 g / L and a temperature of 90 °C.

[0017] A further provision of the present invention is that, in step S6, the copper removal solution contains 12.5 ml / L of concentrated sulfuric acid and 63 g / L of chromium trioxide, with the concentrated sulfuric acid having a mass fraction of 98%.

[0018] A further feature of the present invention is that the electrodeposition power supply is a high-frequency pulse power supply, the output waveform of the high-frequency pulse power supply is a square wave, the output frequency of the high-frequency pulse power supply is 30KHz, the ultrasonic power range of the ultrasonic vibration tank is 300-400W, and the deposition tank is made of PP material.

[0019] A further feature of the present invention is: a five-layer electrodeposited high-sealing bellows.

[0020] The beneficial technical effects of this invention are as follows: 1. The deposition layer is uniform and dense, and the high airtightness index meets the standard: The corrugated pipe deposition layer prepared by this invention has the characteristics of uniform density and good interlayer interface bonding, which can be achieved by attaching... Figure 4 The results are clearly visible; after multiple batches of airtightness tests, the product's airtightness is consistently less than 1.0 × 10⁻⁶. -13 Pa・m³ / s meets the high airtightness requirements of high-end applications. The copper layer, as an intermediate interlayer, can effectively fill or block the micropores of the nickel-cobalt alloy layer, blocking gas permeation channels and further improving the overall leak tightness, ensuring the reliability of the bellows in vacuum, precision instruments, or high-pressure applications.

[0021] 2. Controllable wall thickness uniformity: The zinc immersion treatment on the surface of the aluminum alloy core mold can increase the active sites on the core mold surface and form a transition layer, laying the foundation for obtaining a copper deposition layer with uniform thickness in the future. Combined with the effect of ultrasonic vibration to enhance the fluidity of the electrolyte, it further optimizes the deposition consistency of complex corrugated structures. Moreover, the zinc immersion layer can be dissolved synchronously with the core mold during the demolding process, with no residue affecting subsequent processes.

[0022] 3. The process is equipped with a comprehensive protective design to effectively ensure the integrity of the product molding: During the deposition process, copper is plated on the inner and outer surfaces of the corrugated pipe. The inner copper layer can isolate the zinc immersion layer from the first nickel-cobalt alloy layer, and at the same time prevent the black precipitate formed by the dissolution of the core mold during demolding from contaminating the inner layer; the outer copper layer can protect the outer layer of the corrugated pipe during the demolding process and prevent the demolding liquid from causing corrosion damage to the deposition layer; and the copper layer can be precisely removed with a copper stripping solution in the future without affecting the core structural performance of the corrugated pipe.

[0023] 4. The five-layer alternating sequence design is reasonable, irreplaceable, and achieves complementary performance optimization: The alternation sequence of the nickel-cobalt alloy layer and the copper layer in this invention is the optimal design and cannot be replaced. On the one hand, the nickel-cobalt alloy layer, as the main structural layer, provides high strength, high elasticity, fatigue resistance, and corrosion resistance, adapting to the service requirements of cyclic loads and high temperatures; the copper layer has a low modulus and good ductility, which can reduce the overall spring rate, improve flexibility, and fill the pores of the nickel-cobalt layer as an interlayer, improving sealing performance. On the other hand, this sequence avoids the problems of reduced corrosion resistance and fatigue life caused by the copper layer being exposed, while ensuring the welding or brazing compatibility of the bellows, taking into account both structural performance and application adaptability.

[0024] 5. The five-layer alternating thickness ratio design is reasonable: The gradient multilayer structure of nickel-cobalt alloy layer and copper layer with progressively thicker layers from the inside out ensures that the total wall thickness remains unchanged (without changing the core stiffness properties of the bellows, adapting to the target application scenario). The increased thickness of the outer nickel-cobalt alloy layer effectively improves the tensile, bending and fatigue resistance of the bellows crest region. The thinner inner deposition layer is more likely to obtain a dense and uniform structure, ensuring the stability of interlayer bonding and achieving a smooth transition of interlayer stiffness, thereby significantly reducing the risk of interface stress concentration and through-through failure. This gradient layer thickness design synergistically solves the core problems of wall thickness uniformity and interlayer bonding in multilayer structures, greatly improving the structural stability and long-term service reliability of multilayer electrodeposited bellows.

[0025] 6. Stable interlayer bonding, improving service reliability: The cavitation and acoustic flow effects generated by ultrasonic vibration with a power of 300-400W can achieve dynamic cleaning and activation of the interlayer interface, overcome interfacial bonding barriers, promote metallurgical bonding of different deposition layers, and coordinate the deposition rate and composition ratio of each layer; the five-layer alternating composite structure further enhances the interlayer synergistic stress-bearing capacity, inhibits microcrack propagation, optimizes stress distribution, avoids the risk of delamination failure, and significantly improves the corrugated pipe's resistance to cyclic loading.

[0026] 7. Strong process controllability and engineering application value: The controlled ultrasonic-assisted parameters of this invention are precisely matched with the electrolyte system and deposition process to form a stable and controllable preparation process, avoiding the limitations of simply relying on electrochemical parameter regulation or simple multilayer superposition; moreover, the process is easy to integrate into existing production lines without large-scale modification, providing a reliable technical path for the domestic mass production of high-sealing and high-performance corrugated pipes, which can meet the application needs of high-end fields such as aerospace, energy equipment, and precision instruments. Attached Figure Description

[0027] Figure 1 The image shows a product after the copper layer of the present invention has been deposited.

[0028] Figure 2 The image shows a product after the nickel-cobalt alloy layer of the present invention has been deposited.

[0029] Figure 3 A product image of the present invention after demolding is shown.

[0030] Figure 4 The diagram shows the distribution of the nickel-cobalt alloy layer and copper layer in the cross-section of the deposited layer of the present invention.

[0031] Figure 5 A comparison diagram of the corrugated pipe crest surfaces of Example 1 and Comparative Example 1 is shown.

[0032] Figure 6 A comparison diagram of the corrugated pipe cross-sections of Example 1 and Comparative Example 1 is shown.

[0033] Figure 7 A comparison diagram of the corrugated pipe sidewall cross-sections of Example 1 and Comparative Example 1 is shown.

[0034] Figure 8 Comparative examples 3 and 4 show a comparison of the corrugated pipe cross sections. Detailed Implementation

[0035] The following is a reference to the appendix. Figure 1-8 The preferred embodiments of the present invention will be described below. Those skilled in the art should understand that these embodiments are merely illustrative of the technical principles of the present invention and are not intended to limit the scope of protection of the present invention.

[0036] Example 1 A 30L electrodeposition tank is used. The 30L electrodeposition tank is made of PP and has a length, width and depth of 474mm, 254mm and 290mm respectively. The ultrasonic vibration tank needs to be able to hold the 30L electrodeposition tank. The power of the ultrasonic vibration tank is 0-540W. This application prefers to use 300-400W. The electrodeposition power supply is a high-frequency pulse power supply. The output waveform of the high-frequency pulse power supply is a square wave and the output frequency is 30KHz.

[0037] S1. Core mold pretreatment: The core mold is made of 2A12 aluminum alloy with a surface roughness Ra=1.2μm. After mechanical polishing, the core mold is assembled into a core mold component and then subjected to the following treatments in sequence: alkaline washing (alkaline washing solution contains 17.5g / L sodium hydroxide, 42.5g / L sodium carbonate, and 25g / L trisodium phosphate, solution temperature 60℃, time 20s), acid washing (acid washing solution contains 500ml / L diluted concentrated nitric acid with a mass fraction of 68%, temperature room temperature, time 45s), repeated alkaline washing (same as above, time 15s), repeated acid washing (same as above, time 25s), and zinc immersion (zinc immersion solution contains 480g / L sodium hydroxide, 80g / L zinc oxide, 30g / L potassium sodium tartrate, 2g / L ferric chloride, and 1g / L sodium nitrate, temperature room temperature, time 40s).

[0038] S2. Pre-plating copper treatment: The core mold assembly is installed in a copper deposition fixture and placed in a copper deposition tank for pre-plating copper. The anode material is a phosphorus-containing copper ball with a diameter of 25 mm. The electrolyte in the copper deposition tank is an organic polyphosphate system, i.e., the HEDP system, containing 55 g / L hydroxyethylidene diphosphonic acid, 15 g / L copper sulfate, and 50 g / L potassium carbonate. Deposition parameters: anode-cathode spacing 365 mm, temperature 50℃, pH adjusted to 9 with potassium hydroxide, current density 0.4 A / dm³. 2 The circulation flow rate is 5400 ml / min, and the deposition time is 2 min (without ultrasound). After deposition, the sample is rinsed with tap water and then placed in an ultrasonic cleaner for deep cleaning with deionized water.

[0039] S3. Five-layer composite structure deposition: First layer of nickel-cobalt alloy: The mandrel assembly is installed into a nickel deposition fixture, and then placed in a nickel deposition tank for nickel-cobalt alloy deposition. The anode material is low-sulfur nickel beads with a diameter of 10 mm. The electrolyte in the nickel deposition tank is an aminosulfonate system, containing 575 g / L nickel aminosulfonate, 13 g / L cobalt aminosulfonate, 12.5 g / L nickel chloride, 37.5 g / L boric acid, and 0.20 g / L sodium dodecyl sulfate. The nickel deposition tank is placed in an ultrasonic vibration tank, using tap water as the ultrasonic propagation medium, with a power setting of 350 W. Deposition parameters: anode-cathode distance 365 mm, temperature 60℃, pH adjusted to 4 with potassium hydroxide, current density 0.4 A / dm³. 2 The circulation flow rate was 5400 ml / min, and the deposition time was 2 hours. After the deposition time was reached, the core mold assembly was removed. The residual nickel deposit on the surface of the core mold assembly was first rinsed with tap water, and then placed in deionized water for deep cleaning using an ultrasonic cleaner.

[0040] Second copper layer: The mandrel assembly is transferred into a copper deposition fixture, and then placed in a copper deposition tank for copper deposition. The anode material is a 25mm diameter copper-containing phosphorus ball. The electrolyte in the copper deposition tank is an organic polyphosphate system, i.e., HEDP system, containing 55g / L hydroxyethylidene diphosphonic acid, 15g / L copper sulfate, and 50g / L potassium carbonate. The copper deposition tank is placed in an ultrasonic vibration tank, using tap water as the ultrasonic propagation medium, with a power setting of 350W. Deposition parameters: anode-cathode distance 365mm, temperature 50℃, pH adjusted to 9 with potassium hydroxide, current density 0.4A / dm³. 2 The circulation flow rate was 5400 ml / min, and the deposition time was 6 hours (with ultrasound). The rinsing and cleaning steps were the same as before.

[0041] Third layer of nickel-cobalt alloy: repeat the deposition process of the first layer, deposition time 4 hours; rinsing and cleaning steps are the same as before.

[0042] Fourth copper layer: Repeat the second layer deposition process for 8 hours; the rinsing and cleaning steps are the same as before.

[0043] Fifth layer of nickel-cobalt alloy: Repeat the deposition process of the first layer, deposition time 4 hours; rinsing and cleaning steps are the same as before.

[0044] S4. Copper plating protection treatment: Repeat step S2 deposition process. After deposition, rinse with tap water to obtain a semi-finished corrugated pipe containing the core mold assembly. S5. Demolding process: Transfer the semi-finished corrugated pipe to the lathe, drill a hole at the center of the core mold assembly according to the drawing requirements, remove as much excess part as possible, and then dissolve it in the demolding solution. The demolding solution is potassium hydroxide solution with a concentration of 180g / L and a temperature of 90℃. After the core mold assembly is completely dissolved, take out the semi-finished corrugated pipe and put it into an ultrasonic cleaner for deep cleaning with deionized water. S6. Copper Removal Treatment: The semi-finished corrugated pipe is placed in a copper removal solution containing 12.5 ml / L of concentrated sulfuric acid and 63 g / L of chromium trioxide. The concentrated sulfuric acid has a mass fraction of 98%. The protective copper layer on the inner and outer surfaces of the semi-finished corrugated pipe is removed. After deep cleaning with deionized water in an ultrasonic cleaner, it is dried to obtain a five-layer electrodeposited high-sealing corrugated pipe.

[0045] Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, peak wall thickness 0.062mm, trough wall thickness 0.05mm, peak-to-trough thickness ratio 1.24; thickness percentage of each layer: first layer nickel-cobalt alloy 15%, second layer copper 12%, third layer nickel-cobalt alloy 29%, fourth layer copper 18%, fifth layer nickel-cobalt alloy 26%.

[0046] Example 2 The preparation method is the same as in Example 1, except that: S1. Pretreatment of the core mold: The surface roughness of the core mold Ra=1.2μm, and it is subjected to alkaline washing (alkaline washing solution contains 25g / L sodium hydroxide, 45g / L sodium carbonate, and 30g / L trisodium phosphate, solution temperature is 80℃, time is 30s), acid washing (time is 60s), repeated alkaline washing (time is 20s), repeated acid washing (time is 30s), and zinc immersion (zinc immersion solution contains 550g / L sodium hydroxide, 120g / L zinc oxide, 40g / L potassium sodium tartrate, 1.5g / L ferric chloride, and 1.2g / L sodium nitrate).

[0047] S2. Pre-plating copper treatment: 60g / L hydroxyethylidene diphosphonic acid, 18g / L copper sulfate, 55g / L potassium carbonate.

[0048] S3. Five-layer composite structure deposition: The first layer of nickel-cobalt alloy: the electrolyte in the nickel deposition tank is 650 g / L nickel sulfamate, 19 g / L cobalt sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.20 g / L sodium dodecyl sulfate; the power of the ultrasonic vibration tank is set to 400W.

[0049] The second copper layer consists of an electrolyte in a copper deposition tank containing 60 g / L hydroxyethylidene diphosphonic acid, 18 g / L copper sulfate, and 55 g / L potassium carbonate; the ultrasonic vibration tank is set to a power of 400 W.

[0050] Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, wave crest wall thickness 0.070mm, wave trough wall thickness 0.0545mm, peak-to-trough thickness ratio 1.28; thickness percentage of each layer: first layer nickel-cobalt alloy 16%, second layer copper 10%, third layer nickel-cobalt alloy 30%, fourth layer copper 16%, fifth layer nickel-cobalt alloy 28%.

[0051] Example 3 The preparation method is the same as in Example 1, except that: S1. Pretreatment of the core mold: The surface roughness of the core mold Ra=1.2μm, and it is subjected to the following treatments in sequence: alkaline washing (alkaline washing solution contains 10g / L sodium hydroxide, 35g / L sodium carbonate, and 20g / L trisodium phosphate, solution temperature is 60℃, time is 20s), acid washing (time is 30s), repeated alkaline washing (time is 15s), repeated acid washing (time is 20s), and zinc immersion (zinc immersion solution contains 400g / L sodium hydroxide, 50g / L zinc oxide, 10g / L potassium sodium tartrate, 0.1g / L ferric chloride, and 0.8g / L sodium nitrate); S2. Pre-plating copper treatment: 50 g / L hydroxyethylidene diphosphonic acid, 12 g / L copper sulfate, 42 g / L potassium carbonate; S3. Five-layer composite structure deposition: The first layer of nickel-cobalt alloy: The nickel-cobalt alloy electrolyte consists of 500 g / L nickel sulfamate, 7 g / L cobalt sulfamate, 11 g / L nickel chloride, 36 g / L boric acid and 0.16 g / L sodium dodecyl sulfate; the ultrasonic vibration tank power is set to 300W.

[0052] The second copper layer consists of an electrolyte in a copper deposition tank containing 50 g / L hydroxyethylidene diphosphonic acid, 11 g / L copper sulfate, and 41 g / L potassium carbonate; the ultrasonic vibration tank power is set to 300 W.

[0053] Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, wave crest wall thickness 0.056mm, wave trough wall thickness 0.0465mm, peak-to-trough thickness ratio 1.20; thickness percentage of each layer: first layer nickel-cobalt alloy 15%, second layer copper 12%, third layer nickel-cobalt alloy 28%, fourth layer copper 18%, fifth layer nickel-cobalt alloy 27%.

[0054] Comparative Example 1 S1. Pretreatment of mandrel: Conventional electrodeposited corrugated pipe mandrel, after degreasing and zinc immersion (at least twice).

[0055] S2. Flash-plating copper undercoat: Copper deposition electrolyte (copper sulfate 200g / L, sulfuric acid 60g / L, 2-tetrahydrothiazothione 0.0015g / L, polyethylene glycol 0.035g / L), temperature 41℃, pH=8.8, cathode current density 0.8A / dm³2 The thickness of the flash-plated copper layer is 0.004mm.

[0056] S3. Three-layer deposition: First layer of nickel-cobalt alloy: Electrodeposition solution of nickel-cobalt (nickel sulfamate 400 g / L, nickel chloride 14.5 g / L, boric acid 35 g / L, sodium dodecyl sulfate 1.5 g / L, cobalt sulfamate 30 g / L), temperature 48.5℃, pH=4.2, cathode current density 2.5 A / dm³ 2 The deposits reached 41% of the total wall thickness.

[0057] Copper layer: The same electrolyte system as the flash copper plating is used to deposit copper up to 18% of the total wall thickness.

[0058] The second nickel-cobalt alloy layer: the same as the first nickel-cobalt alloy deposition system, deposited to account for 41% of the total wall thickness.

[0059] S4. Demolding and post-treatment: Demold after the total wall thickness reaches 0.062mm. Clean the inner copper layer with nitric acid solution (60ml / L nitric acid, 4ml / L sulfuric acid) at room temperature for 1.5s.

[0060] Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, crest wall thickness 0.062mm, trough wall thickness 0.021mm, peak-to-trough thickness ratio 3.00.

[0061] Comparative Example 2 S1. Pretreatment of mandrel: Conventional electrodeposited corrugated pipe mandrel, after degreasing and zinc immersion (at least twice).

[0062] S2. Flash copper plating undercoat: Copper deposition electrolyte (copper sulfate 210g / L, sulfuric acid 65g / L, 2-tetrahydrothiazothione 0.0018g / L, polyethylene glycol 0.038g / L), temperature 42℃, pH=8.9, cathode current density 0.9A / dm³ 2 The thickness of the flash-plated copper layer is 0.0045mm.

[0063] S3. Three-layer deposition: First layer of nickel-cobalt alloy: Electrodeposition solution of nickel-cobalt (nickel sulfamate 400 g / L, nickel chloride 15 g / L, boric acid 36 g / L, sodium dodecyl sulfate 1.8 g / L, cobalt sulfamate 30 g / L), temperature 49℃, pH=4.3, cathode current density 2.5 A / dm³ 2 The sediment deposited up to 42% of the total wall thickness.

[0064] Copper layer: The same electrolyte system as the flash copper plating is used to deposit copper up to 17% of the total wall thickness.

[0065] The second nickel-cobalt alloy layer: the same as the first nickel-cobalt alloy deposition system, deposited to account for 41% of the total wall thickness.

[0066] S4. Demolding and post-treatment: Demold after the total wall thickness reaches 0.05mm. Clean the inner copper layer with nitric acid solution (70ml / L nitric acid and 4.5ml / L sulfuric acid) at room temperature for 1.8s.

[0067] Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, crest wall thickness 0.070mm, trough wall thickness 0.023mm, peak-to-trough thickness ratio 3.04.

[0068] Comparative Example 3 The preparation method is the same as in Example 1, except that: S3. Five-layer composite structure deposition: power set to 250W; Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, crest wall thickness 0.084mm, trough wall thickness 0.051mm, peak-to-trough thickness ratio 1.65.

[0069] Comparative Example 4 The preparation method is the same as in Example 1, except that: S3. Five-layer composite structure deposition: power set to 450W; Finished product specifications: outer diameter 25mm × inner diameter 17mm × total length 15mm × wave number 7, crest wall thickness 0.066mm, trough wall thickness 0.048mm, peak-to-trough thickness ratio 1.38.

[0070] Under the same preparation conditions, the core performance of electrodeposited corrugated pipes prepared with and without ultrasonic treatment, and with ultrasonic power exceeding 300-400W, was tested, and the leakage rate was less than 1.0 × 10⁻⁶. -9 Pa·m 3 The airtightness was determined to be acceptable by / s. Due to the special structure of the bellows, the interlayer bonding force is difficult to measure. Generally, if no obvious delamination is observed after cutting along the central axis, it is considered acceptable. The test results are as follows: Table 1 Core performance test data

[0071] Examples 2 and 3 can achieve similar technical effects to Example 1. Taking Example 1 as an example, a comparative analysis of core performance test data is conducted with Comparative Example 1: See appendix Figure 5In the figure, (ad) represents the corrugated surface of an electrodeposited corrugated tube without ultrasound (Comparative Example 1), and (eh) represents the corrugated surface of an electrodeposited corrugated tube with ultrasound (Example 1). Without ultrasound, hydrogen bubbles generated by the cathode hydrogen evolution reaction tend to remain on the corrugated tube surface and are covered by the subsequent deposition layer, thus forming hydrogen pores. After applying ultrasonic vibration, ultrasonic cavitation and acoustic flow effects significantly enhance the desorption and escape capabilities of hydrogen bubbles, while improving the mass transfer conditions at the cathode interface and reducing the degree of hydrogen evolution side reactions, thereby effectively suppressing the formation of hydrogen pores and making the surface of the electrodeposited corrugated tube more dense and smooth.

[0072] See appendix Figure 6 In the figure, (a) shows the peak of the electrodeposited bellows without ultrasonic treatment, (b) shows the trough of the electrodeposited bellows without ultrasonic treatment, (c) shows the peak of the electrodeposited bellows with ultrasonic treatment, and (d) shows the trough of the electrodeposited bellows with ultrasonic treatment. The wall thickness of the peak and trough of the electrodeposited bellows without ultrasonic treatment is significantly different and relatively uneven. The uneven deposition wall thickness seriously affects the fatigue performance of the electrodeposited bellows. The electrodeposited bellows obtained after ultrasonic treatment have more uniform peak and trough wall thicknesses, which improves the fatigue performance of the electrodeposited bellows.

[0073] See appendix Figure 7 Figure (a) shows the sidewall of an electrodeposited bellows without ultrasonic treatment, and (b) shows the sidewall of an electrodeposited bellows with ultrasonic treatment. Without ultrasonic treatment, the sidewall region of the multilayer electrodeposited bellows is limited by the electric field and mass transfer conditions, and the interlayer interfaces are prone to contain bubbles and impurities, resulting in insufficient bonding force and obvious delamination. After ultrasonic vibration is applied, ultrasonic cavitation and acoustic flow effects significantly improve the sidewall interface state and mass transfer conditions, achieving dynamic cleaning and activation of the interlayer interfaces, promoting continuous growth and metallurgical bonding between different deposition layers, thereby significantly improving the interlayer bonding quality of the sidewall and suppressing delamination defects.

[0074] See appendix Figure 8 In the figure, (a) is the peak of Comparative Example 3, (b) is the trough of Comparative Example 3, (c) is the peak of Comparative Example 4, and (d) is the trough of Comparative Example 4. After ultrasonic treatment, the porosity defects and densification degree of the bellows are significantly improved, and the results are comparable to those of the attached... Figure 5 The effect of (ch) is similar, so no attached diagram is provided; only the uniformity of wall thickness is shown.

[0075] Comparative Examples 1 and 2 used a traditional three-layer structure and a copper sulfate-sulfuric acid electrolyte system without ultrasonic assistance. This resulted in insufficient interlayer mass transfer efficiency, uneven microstructure due to differences in the deposition kinetics of different metals, difficulty in eliminating mass transfer dead zones at peaks and troughs, and easy retention of hydrogen bubbles forming micropores, leading to a leakage rate of only 1.0 × 10⁻⁶. -10 Pa・m 3 / s level, the airtightness qualification rate is less than 70%; on the other hand, the peak-to-valley thickness ratio of the three-layer structure is as high as about 3.0, the wall thickness uniformity is extremely poor, and fatigue failure is easily caused by stress concentration under cyclic load. Moreover, impurities are easily trapped at the interlayer interface, and there is a risk of delamination during long-term service.

[0076] Although Comparative Examples 3 and 4 follow the five-layer structure and process framework of this application, the ultrasonic power deviates from the optimal range of 300-400W: Comparative Example 3 (250W) has insufficient power, weak ultrasonic cavitation and acoustic flow effects, and cannot effectively enhance electrolyte flow and bubble desorption, resulting in increased porosity of the deposited layer. The peak-to-valley thickness ratio (1.65) is still significantly worse than that of the example, and the airtightness qualification rate is only 80.6%; Comparative Example 4 (450W) has excessive power. The excessive cavitation effect not only destroys the stability of the aminosulfonate electrolyte, but also causes impact disturbance to the already deposited interlayer interface, resulting in microcracks in some areas. Although the wall thickness uniformity is improved, the interlayer bonding stability decreases, the long-term resistance to cyclic load is weakened, and it is difficult to meet the stringent service requirements of high-end equipment.

[0077] Comparing the test results of Examples 1-3 with those of Comparative Examples 1-4, it can be seen that the present invention, through its innovative design of "a five-layer nickel-cobalt alloy and copper alternating composite structure, 300-400W controlled ultrasonic assistance, and a HEDP and aminosulfonate synergistic electrolyte system," effectively solves the core pain points of the prior art. 1. The comparative example used a three-layer structure without ultrasonic assistance, relying solely on conventional electrochemical parameter control. This resulted in uneven mass transfer at peaks / troughs, bubble retention, and a leakage rate as high as 1.0 × 10⁻⁶. -10 The airtightness compliance rate of previous systems was only 69.4%; however, this invention, through ultrasonic-enhanced mass transfer and bubble desorption, combined with a five-layer alternating densification structure, reduces the leakage rate to 1.0 × 10⁻⁶. -13 The pass rate has increased to 94.4%, achieving a qualitative leap in airtightness.

[0078] 2. The comparative example uses a copper sulfate and sulfuric acid system, which has poor fluidity in complex corrugated areas and a wall thickness uniformity of only 3.04. The HEDP system of this invention, combined with ultrasonic vibration, optimizes the wall thickness uniformity to 1.24, effectively avoiding the risk of fatigue failure.

[0079] In summary, the technical solution of this invention overcomes the limitations of existing technologies. The optimized process effectively suppresses the generation of pores and microcracks during the formation of the deposited layer, improves the density and uniformity of the deposited layer, and strengthens the bonding stability of the interlayer interface, fundamentally solving the problem of easy failure of single-layer systems under high pressure or cyclic loading environments. The five-layered alternating deposition layered composite structure not only achieves uniform stress transmission and dispersion, effectively delaying crack propagation and interfacial penetration, but also improves the uniformity of wall thickness distribution, enabling the bellows to exhibit higher structural stability and long-term reliability in a sealed environment. The finally prepared five-layer electrodeposited bellows achieves a synergistic improvement in deposited layer densification, interlayer bonding stability, wall thickness uniformity, and high sealing performance, significantly extending its service life. It fully meets the stringent application requirements of sealing elements in high-end fields such as aerospace, energy equipment, and precision instruments, and has significant engineering application prospects and promotional value.

[0080] The above description is merely a preferred embodiment of the present invention, and the scope of protection of the present invention is not limited to the above embodiments. For those skilled in the art, any modifications, equivalent substitutions, or improvements made without departing from the technical concept of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for fabricating a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition, characterized in that: The wall of the corrugated pipe is a five-layer composite structure with alternating layers of nickel-cobalt alloy and copper. Each layer of the five-layer composite structure is subjected to ultrasonic vibration treatment during deposition, including the following steps: S1. Pre-treatment of core mold: After mechanical polishing, the core mold is assembled into a core mold assembly, and then subjected to alkaline washing, pickling, repeated alkaline washing, repeated pickling, and zinc immersion treatment in sequence. S2. Pre-plating copper treatment: The core mold assembly is placed into a special copper deposition fixture and placed in a copper deposition tank for pre-plating copper. After deposition, it is rinsed with tap water and then placed in an ultrasonic cleaner for deep cleaning with deionized water. S3. Five-layer composite structure deposition: The first nickel-cobalt alloy layer, the second copper layer, the third nickel-cobalt alloy layer, the fourth copper layer, and the fifth nickel-cobalt alloy layer are deposited sequentially. During each deposition, the core mold assembly is first loaded into the corresponding deposition tooling and then placed into the corresponding deposition tank. The corresponding deposition tanks are placed in an ultrasonic vibration tank, and tap water is used as the medium for ultrasonic vibration propagation for deposition. After each layer of deposition, the core mold assembly is first rinsed with tap water, and then placed in an ultrasonic cleaner for deep cleaning with deionized water. S4. Copper plating protection treatment: The core mold assembly is placed into a special copper deposition tooling and placed in a copper deposition tank for pre-copper plating. After deposition, it is rinsed with tap water to obtain a semi-finished corrugated pipe containing the core mold assembly. S5. Demolding process: Transfer the semi-finished corrugated pipe to the lathe, drill a hole in the center of the core mold assembly, then put it into the demolding solution to dissolve it. After the core mold assembly is completely dissolved, put it into an ultrasonic cleaner for deep cleaning with deionized water. S6. Copper Removal Treatment: The semi-finished corrugated pipe is placed in a copper removal solution to remove the protective copper layer on the inner and outer surfaces of the semi-finished corrugated pipe. After deep cleaning with deionized water in an ultrasonic cleaner, it is dried to obtain a five-layer electrodeposited high-sealing corrugated pipe.

2. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: In step S1, the core mold is made of 2A12 aluminum alloy with a surface roughness Ra≤1.6μm; The alkaline washing solution contains 10-25 g / L sodium hydroxide, 35-50 g / L sodium carbonate, and 20-30 g / L trisodium phosphate. The solution temperature is 60-80℃, and the alkaline washing time is 20-30 seconds. The pickling solution is a diluted concentrated nitric acid with a concentration of 500 ml / L and a mass fraction of 68%. Pickling is performed at room temperature for 30-60 seconds. Repeat the alkaline washing for 15-20 seconds, and repeat the acid washing for 20-30 seconds; The zinc immersion solution contains 400-550 g / L sodium hydroxide, 50-120 g / L zinc oxide, 10-50 g / L sodium potassium tartrate, 0.1-2 g / L ferric chloride, and 0.5-1.5 g / L sodium nitrate. The zinc is immersed for 40 seconds at room temperature.

3. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: In step S3, when depositing the first, third, and fifth nickel-cobalt alloy layers, the anode material is a low-sulfur nickel bead with a diameter of 10 mm. The corresponding electrolyte in the nickel deposition tank is an aminosulfonate system, containing 500-650 g / L nickel aminosulfonate, 7-19 g / L cobalt aminosulfonate, 10-15 g / L nickel chloride, 35-40 g / L boric acid, and 0.15-0.20 g / L sodium dodecyl sulfate. The deposition parameters were: anode-cathode spacing 365 mm, temperature 60 °C, pH adjusted to 4 with potassium hydroxide, and current density 0.4 A / dm³. 2 The circulation flow rate is 5400 ml / min.

4. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: In steps S2-S4, when depositing the pre-plated copper layer, the second copper layer, and the fourth copper layer, the anode material is a phosphorus-containing copper ball with a diameter of 25 mm. The corresponding electrolyte in the copper deposition tank is an organic polyphosphoric acid system containing 50-60 g / L of hydroxyethylidene diphosphonic acid, 10-20 g / L of copper sulfate, and 40-60 g / L of potassium carbonate. The deposition parameters are: anode-cathode spacing of 365 mm, temperature of 50 °C, pH adjusted to 9 with potassium hydroxide, and current density of 0.4 A / dm³. 2 The circulation flow rate is 5400 ml / min.

5. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: In step S3, the total wall thickness of the five-layer composite structure is 0.03-0.15 mm; wherein, the thickness of the first nickel-cobalt alloy layer accounts for 18-22% of the total wall thickness, the thickness of the second copper layer accounts for 15-18% of the total wall thickness, the thickness of the third nickel-cobalt alloy layer accounts for 25-30% of the total wall thickness, the thickness of the fourth copper layer accounts for 18-22% of the total wall thickness, and the thickness of the fifth nickel-cobalt alloy layer accounts for 18-22% of the total wall thickness.

6. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: In step S5, the release solution is a potassium hydroxide solution with a concentration of 180 g / L and a temperature of 90 °C.

7. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: In step S6, the copper removal solution contains 12.5 ml / L of concentrated sulfuric acid and 63 g / L of chromium trioxide, with the concentrated sulfuric acid having a mass fraction of 98%.

8. The method for preparing a high-sealing bellows based on ultrasound-assisted five-layer electrodeposition according to claim 1, characterized in that: The electrodeposition power supply is a high-frequency pulse power supply, the output waveform of the high-frequency pulse power supply is a square wave, the output frequency of the high-frequency pulse power supply is 30KHz, the ultrasonic power range of the ultrasonic vibration tank is 300-400W, and the deposition tank is made of PP material.

9. A five-layer electrodeposited high-sealing bellows prepared by the method for preparing an ultrasonically assisted five-layer electrodeposited high-sealing bellows according to any one of claims 1-8.

Citation Information

Patent Citations

  • Multi-layer thin-wall electro-deposition corrugated pipe and processing method thereof