Lithium foil direct contact-based lithium ion capacitor anode material pre-lithiation method
By using a direct contact pre-lithiation method with lithium foil, the area and thickness of the lithium foil are calculated. After covering the anode sheet, the foil is rolled and allowed to stand for reaction. This method solves the problems of complexity and non-uniformity in the pre-lithiation of the anode in existing lithium-ion capacitors, and improves production efficiency and the cycle performance of the capacitor.
Patent Information
- Application Number
- CN202610412105.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-31
- Publication Date
- 2026-05-26
AI Technical Summary
Existing methods for pre-lithiation of the anode in lithium-ion capacitors suffer from complex processes, low production efficiency, and insufficient uniformity and controllability of pre-lithiation. In particular, direct contact pre-lithiation technology requires high standards for lithium source distribution control and operating environment.
A pre-lithiation method based on direct contact with lithium foil is adopted. By calculating the area and thickness of the lithium foil, it is covered on the surface of the anode sheet, rolled and electrolyte is added, allowed to stand for reaction, and finally cleaned to obtain the pre-lithiation anode. This simplifies the operation and controls the degree of pre-lithiation.
It simplifies the operation process, improves production efficiency, ensures uniformity and controllability of lithiation, reduces production costs, and enhances the cycle performance of lithium-ion capacitors without compromising the stability of the anode structure.
Smart Images

Figure CN122091408A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical technology, and in particular to a method for pre-lithiation of anode materials for lithium-ion capacitors based on direct contact with lithium foil. Background Technology
[0002] With the rapid development of renewable energy and electric vehicles, the demand for high-efficiency energy storage systems is constantly increasing, and lithium-ion capacitors (LICs) have become a research hotspot due to their unique performance. LICs are energy storage devices that combine the characteristics of lithium-ion batteries and capacitors, utilizing a battery-type negative electrode and a capacitor-type positive electrode to achieve a balance between high energy density and high power density.
[0003] Despite the significant advantages of lithium-ion intercalation / deintercalation (LICs), their widespread application is still limited by the irreversible lithium-ion consumption resulting from the intercalation / deintercalation process at the anode. Simultaneously, irreversible side reactions within the anode and the formation of the surface SEI film also consume a large amount of lithium ions during the first cycle. This substantial irreversible lithium-ion consumption significantly reduces the capacity and cycle life of LICs. Therefore, supplementing with an additional lithium source to compensate for the irreversible consumption of active lithium ions is crucial for improving the performance of LICs.
[0004] Anode pre-lithiation technology has proven to be a viable approach. By introducing an additional lithium source into the anode beforehand, the impact of lithium-ion consumption on the performance of LICs can be reduced. This technology can be implemented in various ways, including chemical pre-lithiation, electrochemical pre-lithiation, and direct contact pre-lithiation, each aimed at improving the lithium storage capacity of energy storage materials while maintaining structural stability and extending the lifespan of LICs.
[0005] As a key step in improving the performance of lithium phosphate electrodes (LICs), there are many methods to achieve pre-lithiation of the LIC anode. Currently, there are two traditional laboratory pre-lithiation methods: electrochemical pre-lithiation (EC-Pr) and external short-circuit pre-lithiation (ESC-Pr). The EC-Pr method is complex and the lithiated electrode and active material are easily separated, while the ESC-Pr method is cumbersome and causes unnecessary waste of manpower and resources. In contrast, direct contact pre-lithiation (DC-Pr) can achieve a membrane-free lithiated electrode through a self-discharge process, which is a simple, practical, and scalable pre-lithiation method. DC-Pr induces electron migration through the potential difference between the anode and metallic lithium, allowing lithium ions in the metallic lithium to be released into the anode through the electrolyte, ultimately obtaining a lithiated anode. At the same time, DC-Pr not only produces an SEI on the anode surface that is very similar to other pre-lithiation technologies, but also achieves stable cycling performance without sacrificing the stability of the anode structure. In addition, DC-Pr technology can simplify the complex disassembly and assembly process and control the degree of pre-lithiation by adjusting the contact time. This strategy has the potential to be widely compatible with electrode manufacturing processes.
[0006] CN114788037A discloses a method for pre-lithiating multiple anodes. This method involves stacking anode sheets and lithium-containing sheets in an electrolyte as a jelly roll or stack, achieving pre-lithiation of the anodes through direct contact or by transferring lithium ions via discharge / charge. However, this method still suffers from drawbacks such as complex processes, low production efficiency, and issues with the uniformity and controllability of pre-lithiation.
[0007] In summary, the direct contact pre-lithiation method has significant advantages in achieving anode pre-lithiation, improving LIC performance, and controlling production steps, but it also faces limitations such as the need for precise control of lithium source distribution and high requirements for the operating environment.
[0008] Therefore, the aforementioned problems faced by direct contact prelithiation technology still need to be addressed by developing suitable process routes and appropriate lithium sources. Summary of the Invention
[0009] The purpose of this invention is to overcome at least one of the defects of the prior art, such as complex process, low production efficiency, and uneven and controllable pre-lithiation, and to provide a pre-lithiation method for lithium-ion capacitor anode materials based on direct contact with lithium foil.
[0010] The objective of this invention can be achieved through the following technical solutions: This invention provides a method for pre-lithiation of anode materials for lithium-ion capacitors based on direct contact with lithium foil, comprising the following steps: S1: Calculate the required area of lithium foil based on the type of anode material, lithium intercalation capacity, and thickness of the lithium foil in the lithium-ion capacitor; S2: Cut the lithium foil to the required area and completely cover the surface of the anode sheet with the lithium foil; S3: Roll the anode sheet covered with lithium foil to ensure that the lithium foil is completely adhered to the surface of the anode sheet; S4: Add a predetermined amount of electrolyte to the rolled anode sheet and seal it; S5: Allow the sealed anode sheet to stand for a while to ensure that the lithium foil reacts completely and is fully pre-lithiated; S6: Clean the pre-lithiated anode sheet to finally obtain the pre-lithiated lithium-ion capacitor anode.
[0011] Furthermore, in step S1, the anode material of the lithium-ion capacitor is any one of graphite, hard carbon, or silicon-based materials.
[0012] Furthermore, in step S1, the thickness of the lithium foil ranges from 5 to 50 μm.
[0013] Furthermore, in step S1, the types of lithium foil include single-layer lithium foil with a substrate and double-layer lithium foil with a substrate.
[0014] Further, in step S1, the formula for calculating the required area of the lithium foil is as follows: A = Q / (t × ρ × F) In the formula, A The area required for lithium foil, Q For lithium intercalation capacity, t The thickness of the lithium foil used, ρ The density of lithium, F is the Faraday constant for lithium.
[0015] Furthermore, the lithium intercalation capacity is preset by multiplying the mass of the anode material of the lithium-ion capacitor by the pre-lithiation capacity, and the value of the pre-lithiation capacity ranges from 50 to 300 mAh / g.
[0016] Furthermore, the operations in steps S2, S3, and S4 are all performed in an inert gas atmosphere.
[0017] Furthermore, the inert gas atmosphere is any one or a mixture of helium and argon.
[0018] Furthermore, in step S2, the lithium foil is covered by a single layer or a multilayer covering.
[0019] Furthermore, when the required area of the lithium foil is smaller than the anode area, a single layer of lithium foil is uniformly spread outward from the center of the anode sheet.
[0020] Furthermore, when the required area of the lithium foil is greater than the area of the anode, the bottom lithium foil is covered on the surface of the anode sheet in a single-layer manner, and the excess superimposed layers are uniformly covered on the bottom lithium foil from the center outward according to the same principle.
[0021] Furthermore, in step S3, the roller spacing of the rolling process is 80% to 90% of the total thickness of the electrode after covering the lithium foil.
[0022] Furthermore, in step S3, the rolling is performed in a non-heated, ambient temperature double-roll press.
[0023] Furthermore, in step S4, the electrolyte includes lithium salt, organic solvent, and additives.
[0024] Furthermore, the lithium salt includes any one or a combination of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0025] Furthermore, the organic solvent includes any one or more combinations of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), propylene carbonate (PC), dimethoxyethane (DME), 1,3-dioxane (DOL), methyl formate (MF), and ethyl acetate (EA).
[0026] Furthermore, the additives include any one or a combination of flame retardants, overcharge protection additives, and conductive salt additives.
[0027] Furthermore, the flame retardant includes any one or a combination of triphenyl phosphate (TPP) and diphenyl phosphate (DPB).
[0028] Furthermore, the overcharge protection additive includes lithium bis(fluorosulfonyl)imide (LiDFSI).
[0029] Furthermore, the conductive salt additive includes lithium nitrate (LiNO3).
[0030] Furthermore, in step S5, the temperature for settling is 0-50 ℃, preferably 15-35 ℃.
[0031] Furthermore, in step S5, the total duration of the resting period is not less than 36 hours.
[0032] Based on the direct contact pre-lithiation method of this invention, lithium foil is covered on the anode sheet and an appropriate amount of electrolyte is added. Electron migration is induced by the potential difference between the anode and metallic lithium, causing the lithium foil to react and generate lithium ions. These ions then migrate through the electrolyte to the anode surface and gradually embed into the anode, ultimately obtaining a lithiated anode. Furthermore, this pre-lithiation method not only produces an SEI on the anode surface very similar to other pre-lithiation technologies, but also achieves stable cycling performance without sacrificing the stability of the anode structure.
[0033] Compared with the prior art, the present invention has the following technical advantages: (1) Compared with the traditional electrochemical prelithiation (EC-Pr) method and external short-circuit prelithiation (ESC-Pr) method in the laboratory, the present invention can achieve diaphragm-free anode prelithiation by direct contact prelithiation without sacrificing the stability of the LIC anode structure, using lithium foil as an additional lithium source, and achieving diaphragm-free anode prelithiation through self-discharge process, simplifying the complicated disassembly and assembly process.
[0034] (2) The present invention adopts the method of directly covering the anode surface with lithium foil to achieve pre-lithiation of the anode. The process steps are simple and highly operable. The degree of pre-lithiation can be controlled by adjusting parameters such as lithium foil thickness, area, and resting time in real time. It has good compatibility with current electrode manufacturing processes.
[0035] (3) The pre-lithiation method used in this invention does not require additional energy consumption and has a simple process route, which is conducive to controlling and reducing the production cost of electrode pre-lithiation. Attached Figure Description
[0036] Figure 1 This is a schematic flowchart of the pre-lithiation method of the present invention.
[0037] Figure 2 This is a schematic diagram of the rolling pressing method used in Embodiments 1, 2, 3, 4 and 5 of the present invention.
[0038] Figure 3 This is a schematic diagram of the pre-lithiation mechanism in Examples 1 and 2 of the present invention.
[0039] Figure 4 These are SEM scan images of Embodiment 1 of the present invention before and after pre-lithiation. Figure 4 (a) Figure 4 (b) is a SEM scan image of the electrode surface before pre-lithiation of the graphite anode in Example 1; Figure 4 (c) Figure 4 (d) is a SEM scan image of the electrode surface after pre-lithiation of the graphite anode in Example 1.
[0040] Figure 5XPS analysis image of the film-like material on the surface of the graphite anode after pre-lithiation in Example 1 of this invention.
[0041] Figure 6 The first charge-discharge curves of the assembled half-cells before and after pre-lithiation in Example 1 and Comparative Example 1 of the present invention are shown.
[0042] Figure 7 Images showing the long-cycle test results of half-cells assembled before and after pre-lithiation in Example 1 and Comparative Example 1 of the present invention at a rate of 0.05 C.
[0043] Figure 8 This is an example of the distribution of lithium foil on the electrode surface during the pre-lithiation process in Embodiment 1 of the present invention at different pre-lithiation times. Detailed Implementation
[0044] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.
[0045] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available.
[0046] This invention provides a method for pre-lithiation of anode materials in lithium-ion capacitors based on direct contact with lithium foil, aiming to achieve better electrode pre-lithiation and improve battery performance.
[0047] like Figure 1 As shown, the pre-lithiation method of the present invention specifically includes the following steps: S1: Calculate the required area of lithium foil based on the type of LICs anode active material, lithium intercalation capacity, and lithium foil thickness.
[0048] Based on the type of LIC anode active material selected and its theoretical lithium intercalation capacity, calculate the required lithium foil thickness and area. Single-layer lithium foil is preferred to meet the lithium intercalation capacity requirements, avoiding the use of multilayer structures. The calculation formula can be based on the lithium foil density and lithium intercalation capacity formula to ensure accurate results. Determine the lithium foil thickness (t) and area (A) to meet the required lithium intercalation capacity (Q) using the following formula: Q = t × A × ρ × F In the formula, t The thickness of the lithium foil used, A The area required for lithium foil, ρ The density of lithium, F is the Faraday constant for lithium.
[0049] LICs (Lithium Alloy Chemicals) anodic active materials include graphite, hard carbon, and silicon-based materials (such as silicon carbide, SiC).
[0050] The thickness of the lithium foil ranges from 5 to 50 μm, specifically including lithium foil with a thickness of 5 μm, 10 μm, 20 μm and 50 μm.
[0051] Lithium foils come in two types: single-layer lithium foil with a substrate and double-layer lithium foil with a substrate.
[0052] S2: Lithium foil in contact with the anode surface.
[0053] Under an inert atmosphere (such as argon), the cut lithium foil is evenly and completely covered on the anode plate surface. Ensure the lithium foil is undamaged and wrinkled during installation; use specialized tools if necessary. Apply a certain amount of mechanical pressure beforehand to ensure tight contact between the lithium foil and the anode plate. The pressure level needs to be determined based on the characteristics of the anode material and the lithium foil.
[0054] The lithium foil covering method on the anode surface includes single-layer covering and multi-layer covering. When the required lithium foil area calculated according to S1 is smaller than the anode area, the lithium foil should be placed in the center of the anode, ensuring no significant gaps at the edges, and the single-layer lithium foil should be evenly applied outwards from the center of the anode. When the calculated required lithium foil area is larger than the anode area, the center of the lithium foil is aligned with the center of the anode, the bottom layer of lithium foil is applied to the anode surface in a single-layer manner, and any excess multi-layers are evenly applied outwards from the center onto the bottom layer of lithium foil using the same principle.
[0055] S3: Rolled lithium foil and anode sheet.
[0056] like Figure 2 As shown, in an argon atmosphere, the anode sheet covered with lithium foil is fed into a roller press for rolling. The roller press is a non-heated, room-temperature double-roller press. The roller spacing of the roller press is adjusted to be slightly less than the sum of the anode sheet thickness and the total thickness of the lithium foil, approximately 80% to 90% of the total electrode thickness after covering with lithium foil, to ensure good contact. Rolling is repeated multiple times to ensure complete adhesion between the lithium foil and the anode sheet surface, preventing the lithium foil from detaching during subsequent operations. The rolling process should be carried out at appropriate speed and pressure to prevent excessive compression that could damage the material.
[0057] S4: Add electrolyte and seal.
[0058] Under argon protection, a predetermined amount of electrolyte is added to the rolled anode sheet. The volume of electrolyte should be calculated based on the lithium intercalation capacity to ensure sufficient electrolyte for lithium-ion migration. The anode sheet containing the electrolyte is then sealed with a special membrane to ensure no leakage.
[0059] The electrolyte consists of lithium salts, organic solvents, and additives.
[0060] Specifically, lithium salts include the following types: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), etc.
[0061] Organic solvents include the following types: carbonates (such as ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), propylene carbonate (PC), etc.), ethers (such as dimethoxyethane (DME), 1,3-dioxane (DOL), etc.), and esters (such as methyl formate (MF), ethyl acetate (EA), etc.).
[0062] Additives include the following types: flame retardants (such as triphenyl phosphate (TPP), diphenyl phosphate (DPB), etc.), overcharge protection additives (such as lithium difluorosulfonyl imide (LiDFSI), etc.), and conductive salt additives (such as lithium nitrate (LiNO3), etc.).
[0063] S5: The anode is covered by a static lithium foil.
[0064] Allow the sealed anode sheet to stand for a sufficient period of time, determined by the lithium intercalation capacity, generally no less than 36 hours. The larger the capacity, the longer the standing time should be. During the standing process, ensure environmental stability and avoid temperature and pressure fluctuations. The sealed anode sheet is placed in a set temperature environment (usually room temperature or slightly above room temperature) and left to stand for a period of time to promote lithium-ion diffusion. The sealing method is molten sealing by heating under normal pressure in an argon atmosphere. The standing temperature includes the following temperatures: 0 ℃, 15 ℃, 25 ℃ (or room temperature) and 50 ℃, preferably 25 ℃.
[0065] S6: Fully pre-lithiated.
[0066] Observe the surface of the anode plate to confirm that the lithium foil has completely reacted and disappeared. Continue to let it stand for a period of time to ensure that the lithium ions are evenly distributed in the anode material and to avoid local concentration differences. The additional standing time depends on the specific reaction situation and is generally several hours to a day.
[0067] S7: Cleaning and preparing pre-lithiated anodes.
[0068] Remove the pre-lithiated anode from the sealed packaging. Thoroughly clean the anode surface with a suitable solvent (such as ethylene carbonate) to remove residual electrolyte and reaction byproducts. Place the cleaned anode in a vacuum drying oven and dry at low temperature, ensuring no solvent residue remains. Check the integrity and lithium intercalation uniformity of the anode; once confirmed to meet the expected requirements, the pre-lithiated LIC anode is obtained.
[0069] Based on the direct contact pre-lithiation method of this invention, lithium foil is covered on the anode sheet and an appropriate amount of electrolyte is added. Electron migration is induced by the potential difference between the anode and metallic lithium, causing the lithium foil to react and generate lithium ions. These ions then migrate through the electrolyte to the anode surface and gradually embed into the anode, ultimately obtaining a lithiated anode. Furthermore, this pre-lithiation method not only produces an SEI on the anode surface very similar to other pre-lithiation technologies, but also achieves stable cycling performance without sacrificing the stability of the anode structure.
[0070] Figure 3 This is a schematic diagram illustrating the pre-lithiation mechanism of the present invention. The diagram illustrates the migration paths of lithium ions and electrons, and the solvation and desolvation processes of lithium ions when lithium foil is covered on the surface of a graphite anode.
[0071] Example 1: This embodiment provides a method for pre-lithiation of anode materials in lithium-ion capacitors based on direct contact with lithium foil, including the following steps: Step 1: Select graphite as the anode active material for lithium-ion capacitor batteries. Multiply the mass of the active material by the pre-lithiation capacity (60 mAh / g) to obtain the lithium foil capacity, and cut a fixed amount of 20 μm thick lithium foil.
[0072] Step 2: In an argon atmosphere, the lithium foil is evenly and completely covered on the surface of the graphite anode, and a certain pressure is applied in advance to ensure close contact between the lithium foil and the graphite electrode.
[0073] Step 3: In an argon atmosphere, the graphite electrode sheet covered with lithium foil is fed into a roller press for repeated rolling to further compact the contact between the lithium foil and the anode sheet, ensuring that the lithium foil will not detach from the surface of the anode sheet during subsequent operations.
[0074] Step 4: In an argon atmosphere, add 100 μl of electrolyte (1 MLiTFSI in EC:DMC=1:1) to the anode sheet that has been rolled and covered with lithium foil, and then seal it with a special membrane.
[0075] Step 5: Place the sealed special film at 25 ℃ and let it stand for 36 h.
[0076] Step 6: After the lithium foil reaction on the graphite electrode surface has completely disappeared, continue to let it stand for 36 hours to ensure uniform reaction inside the anode.
[0077] Step 7: Remove the lithium-intercalated anode sheet, clean it thoroughly, and finally obtain the pre-lithiated graphite anode of LICs.
[0078] Example 2: This embodiment provides a method for pre-lithiation of anode materials in lithium-ion capacitors based on direct contact with lithium foil, including the following steps: Step 1: Select SiC as the anode active material for lithium-ion capacitor batteries. Multiply the mass of the active material by the pre-lithiation capacity (300 mAh / g) to obtain the lithium foil capacity. Cut a fixed amount of 50 μm thick lithium foil.
[0079] Step 2: In an argon atmosphere, lithium foil is uniformly and completely covered on the surface of the SiC anode, and a certain pressure is applied in advance to ensure close contact between the lithium foil and the SiC electrode.
[0080] Step 3: In an argon atmosphere, the SiC electrode sheet covered with lithium foil is fed into a roller press for repeated rolling to further compact the contact between the lithium foil and the anode sheet, ensuring that the lithium foil will not detach from the surface of the anode sheet during subsequent operations.
[0081] Step 4: In an argon atmosphere, add 200 μl of electrolyte (1 M LiTFSI in EC:DMC=1:1) to the rolled SiC anode sheet covered with lithium foil, and then seal it with a special membrane.
[0082] Step 5: Place the sealed special film at 25 ℃ and let it stand for 72 h.
[0083] Step 6: After the lithium foil on the SiC electrode surface has completely disappeared from the reaction, continue to let it stand for 36 hours to ensure that the reaction inside the anode is uniform.
[0084] Step 7: Remove the lithium-intercalated anode sheet, clean it thoroughly, and finally obtain the pre-lithiated SiC anode of LICs.
[0085] Example 3: This embodiment provides a method for pre-lithiation of anode materials in lithium-ion capacitors based on direct contact with lithium foil, including the following steps: Step 1: Select SiC as the anode active material for lithium-ion capacitor batteries. Multiply the mass of the active material by the pre-lithiation capacity (300 mAh / g) to obtain the lithium foil capacity. Cut a fixed amount of 25 μm thick lithium foil.
[0086] Step 2: In an argon atmosphere, lithium foil is uniformly and completely covered on the surface of the SiC anode in a stacked manner, and a certain pressure is applied in advance to ensure close contact between the lithium foil and the SiC electrode.
[0087] Step 3: In an argon atmosphere, the SiC electrode sheet covered with lithium foil is fed into a roller press for repeated rolling to further compact the contact between the lithium foil and the anode sheet, ensuring that the lithium foil will not detach from the surface of the anode sheet during subsequent operations.
[0088] Step 4: In an argon atmosphere, add 200 μl of electrolyte (1 M LiTFSI in EC:DMC=1:1) to the rolled SiC anode sheet covered with lithium foil, and then seal it with a special membrane.
[0089] Step 5: Place the sealed special film at 25 ℃ and let it stand for 72 h.
[0090] Step 6: After the reaction of lithium foil on the surface of SiC electrode has completely disappeared, continue to let it stand for 72 hours to ensure uniform reaction inside the anode.
[0091] Step 7: Remove the lithium-intercalated anode sheet, clean it thoroughly, and finally obtain the pre-lithiated SiC anode of LICs.
[0092] Example 4: This embodiment provides a method for pre-lithiation of anode materials in lithium-ion capacitors based on direct contact with lithium foil, including the following steps: Step 1: Select hard carbon as the anode active material for lithium-ion capacitor batteries. Multiply the mass of the active material by the pre-lithiation capacity (100 mAh / g) to obtain the lithium foil capacity, and cut a fixed amount of 25 μm thick lithium foil.
[0093] Step 2: In an argon atmosphere, the lithium foil is evenly and completely covered on the surface of the hard carbon anode, and a certain pressure is applied in advance to ensure close contact between the lithium foil and the hard carbon electrode.
[0094] Step 3: In an argon atmosphere, the hard carbon electrode sheet covered with lithium foil is fed into a roller press for repeated rolling to further compact the contact between the lithium foil and the anode sheet, ensuring that the lithium foil will not detach from the surface of the anode sheet during subsequent operations.
[0095] Step 4: In an argon atmosphere, add 500 μl of electrolyte (1M LiTFSI in EC:DMC=1:1) to the rolled hard carbon electrode covered with lithium foil, and then seal it with a special membrane.
[0096] Step 5: Place the sealed special film at 25 ℃ and let it stand for 36 h.
[0097] Step 6: After the lithium foil reaction on the surface of the hard carbon electrode has completely disappeared, continue to let it stand for 36 hours to ensure that the reaction inside the anode is uniform.
[0098] Step 7: Remove the lithium-intercalated anode sheet, clean it thoroughly, and finally obtain the pre-lithiated hard carbon anode of LICs.
[0099] Example 5: This embodiment provides a method for pre-lithiation of anode materials in lithium-ion capacitors based on direct contact with lithium foil, including the following steps: Step 1: Select hard carbon as the anode active material for lithium-ion capacitor batteries. Multiply the mass of the active material by the pre-lithiation capacity (200 mAh / g) to obtain the lithium foil capacity. Cut a fixed amount of 20 μm thick lithium foil.
[0100] Step 2: In an argon atmosphere, the lithium foil is evenly and completely covered on the surface of the hard carbon anode, and a certain pressure is applied in advance to ensure close contact between the lithium foil and the hard carbon electrode.
[0101] Step 3: In an argon atmosphere, the hard carbon electrode sheet covered with lithium foil is fed into a roller press for repeated rolling to further compact the contact between the lithium foil and the anode sheet, ensuring that the lithium foil will not detach from the surface of the anode sheet during subsequent operations. Step 4: In an argon atmosphere, add 200 μl of electrolyte (1 M LiTFSI in EC:DMC=1:1) to the rolled hard carbon anode sheet covered with lithium foil, and then seal it with a special membrane.
[0102] Step 5: Place the sealed special film at 25 ℃ and let it stand for 60 h.
[0103] Step 6: After the lithium foil reaction on the surface of the hard carbon electrode has completely disappeared, continue to let it stand for 30 hours to ensure that the reaction inside the anode is uniform.
[0104] Step 7: Remove the lithium-intercalated anode sheet, clean it thoroughly, and finally obtain the pre-lithiated hard carbon anode of LICs.
[0105] Comparative Example 1: This comparative example is a graphite anode prepared based on wet coating technology, including the following steps: Step 1: Based on the type of active material, select a suitable active material with a ratio of graphite: PVDF binder: SuperP conductive agent of 96%:2%:2% as the electrode powder material.
[0106] Step 2: Add the electrode powder material to a small amount of NMP solvent and disperse it evenly by ball milling to obtain a wet-coated electrode slurry.
[0107] Step 3: The electrode slurry is fed into a wet coating apparatus for coating to prepare a 50 μm graphite electrode, which is then dried in a 60 ℃ oven.
[0108] Step 4: Take out the dried electrode, punch it into a circular electrode, transfer it to an 80 ℃ vacuum oven, and vacuum dry it for 10 h to obtain an unlithiated graphite anode.
[0109] Comparative Example 2: This comparative example is a SiC anode prepared based on wet coating technology, including the following steps: Step 1: Based on the type of active material, select a suitable ratio of SiC (active material): PVDF (binder): SuperP (conductive agent) of 95%:2%:3% as the electrode powder material. Step 2: Add the electrode powder material to NMP solvent and disperse it evenly by ball milling to obtain a wet-coated electrode slurry.
[0110] Step 3: The electrode slurry is fed into a wet coating apparatus for coating to prepare a 50 μm SiC electrode, and then sent to a 60 ℃ oven for drying.
[0111] Step 4: Take out the dried electrode, punch it into a circular electrode, transfer it to an 80 ℃ vacuum oven, and vacuum dry it for 10 h to obtain an unlithiated SiC anode.
[0112] Figure 4 These are SEM scan images of the graphite anode surfaces of Example 1 (after pre-lithiation) and Comparative Example 1 (before pre-lithiation) of the present invention. Before pre-lithiation, as shown... Figure 4 (a) Figure 4 As shown in (b), the surface of the graphite anode exhibits a loose and porous structure, allowing for complete observation of the graphite particle structure, with clear boundary lines between the particles. This indicates that the graphite particles and electrode morphology can be clearly and completely observed on the surface of the un-lithiated graphite anode. After pre-lithiation, as shown... Figure 4 (c) Figure 4 As shown in (d), a film-like substance can be clearly observed on the surface of the graphite anode covering the graphite particles. At this time, the anode surface becomes smoother than before pre-lithiation, and the graphite particles cannot be clearly distinguished. The boundaries between the graphite particles are covered by the film-like substance.
[0113] Figure 5 This is the XPS analysis result of the film-like material on the surface of the pre-lithiated graphite electrode in Example 1 of the present invention. Figure 5 As shown, the main components of the film-like material are lithium carbonate, lithium hydroxide, lithium oxide, and lithium fluoride. XPS results confirm that the film-like material on the anode surface is an SEI film generated during the pre-lithiation process, and that the SEI film uniformly and completely covers the surface of the graphite particles. This indicates that the pre-lithiation of the graphite anode achieved a satisfactory result, proving the feasibility of the pre-lithiation method of this invention.
[0114] Figure 6 These are the first charge-discharge curves of the half-cells assembled in Example 1 (after pre-lithiation) and Comparative Example 1 (before pre-lithiation) of the present invention. Figure 5It is evident that before pre-lithiation, the formation of the SEI film on the graphite anode surface and the generation of side reactions within the graphite electrode lead to the consumption of a large number of active lithium ions. During the first charge-discharge cycle, the content of active lithium ions extracted from the anode is significantly less than the content of active lithium ions inserted into the anode. After pre-lithiation, the lithium foil acts as an additional lithium source, providing extra lithium ions for the pre-formation of the SEI film at the anode and to counteract side reactions. Therefore, during the first charge-discharge cycle, the content of active lithium ions that can be extracted from the anode is not significantly different from the content of inserted active lithium ions. Calculations show that after pre-lithiation, the first-cycle coulombic efficiency (ICE) of the half-cell increases from 86.7% to 95%.
[0115] Figure 7 Images show the long-cycle test results of half-cells assembled in Example 1 (after pre-lithiation) and Comparative Example 1 (before pre-lithiation) at a 0.05 C rate. It can be seen that, due to the pre-introduction of additional active lithium ions to compensate for the continuous consumption of active lithium ions by irreversible reactions during discharge cycling, the half-cell assembled with the pre-lithiated electrode exhibits a significantly improved long-cycle life compared to the un-lithiated half-cell. At the same number of long cycles (300 cycles), the specific capacity of the pre-lithiated half-cell reaches 341.47 mAh / g, representing a 14.7% increase compared to the un-lithiated battery.
[0116] Figure 8 This illustrates the distribution of lithium foil on the electrode surface during different pre-lithiation times in Embodiment 1 of the present invention. Figure 8 It can be seen that at 25 °C, the residual area of the lithium foil covering the graphite anode surface decreases significantly with the advancement of pre-lithiation time. By 36 h, no obvious lithium foil structure can be observed on the electrode surface, indicating that most of the lithium foil has been converted into lithium ions and embedded inside the electrode through the reaction. In order to ensure sufficient and uniform diffusion of lithium ions inside the electrode, it is allowed to stand for another 36 h, finally obtaining a relatively uniform pre-lithiated graphite anode.
[0117] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A method for pre-lithiation of anode material in lithium-ion capacitors based on direct contact with lithium foil, characterized in that, Includes the following steps: S1: Calculate the required area of lithium foil based on the type of anode material, lithium intercalation capacity, and thickness of the lithium foil in the lithium-ion capacitor; S2: Cut the lithium foil to the required area and completely cover the surface of the anode sheet with the lithium foil; S3: Roll the anode sheet covered with lithium foil to ensure that the lithium foil is completely adhered to the surface of the anode sheet; S4: Add a predetermined amount of electrolyte to the rolled anode sheet and seal it; S5: Allow the sealed anode sheet to stand for a while to ensure that the lithium foil reacts completely and is fully pre-lithiated; S6: Clean the pre-lithiated anode sheet to finally obtain the pre-lithiated lithium-ion capacitor anode.
2. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S1, the anode material of the lithium-ion capacitor is any one of graphite, hard carbon, and silicon-based materials; The thickness of the lithium foil ranges from 5 to 50 μm.
3. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S1, the formula for calculating the required area of the lithium foil is as follows: A = Q / (t × ρ × F) ; In the formula, A The area required for lithium foil, Q For lithium intercalation capacity, t The thickness of the lithium foil used, ρ The density of lithium, F is the Faraday constant for lithium.
4. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 3, characterized in that, The lithium intercalation capacity is preset by multiplying the mass of the anode material of the lithium-ion capacitor by the pre-lithiation capacity, and the value of the pre-lithiation capacity ranges from 50 to 300 mAh / g.
5. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S2, the lithium foil is covered by a single layer or a multilayer covering. When the required area of the lithium foil is smaller than the area of the anode, a single layer of lithium foil is uniformly covered outward from the center of the anode sheet. When the required area of the lithium foil is greater than the area of the anode, the bottom lithium foil is covered on the surface of the anode sheet in a single-layer manner, and the excess superimposed layers are uniformly covered on the bottom lithium foil from the center outward according to the same principle.
6. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S3, the roller spacing of the rolling process is 80% to 90% of the total thickness of the electrode after covering the lithium foil.
7. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S4, the electrolyte includes lithium salt, organic solvent and additives; The lithium salt includes any one or a combination of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, and lithium bis(trifluoromethanesulfonyl)imide; The organic solvent includes any one or more combinations of ethylene carbonate, dimethyl carbonate, diethyl carbonate, propylene carbonate, dimethoxyethane, 1,3-dioxane, methyl formate, and ethyl acetate. The additives include any one or a combination of flame retardants, overcharge protection additives, and conductive salt additives.
8. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 7, characterized in that, The flame retardant includes any one or more combinations of triphenyl phosphate and diphenyl phosphate; The overcharge protection additive includes lithium difluorosulfonylimide salt; The conductive salt additive includes lithium nitrate.
9. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S5, the temperature for settling is 0-50 ℃.
10. The method for pre-lithiation of anode material in a lithium-ion capacitor based on direct contact with lithium foil according to claim 1, characterized in that, In step S5, the total duration of the resting period shall not be less than 36 hours.