In-situ construction method of self-supporting sulfided nickel water-splitting electrode adapting to fluctuating working conditions

CN122105462BActive Publication Date: 2026-11-20UNIV OF SCI & TECH BEIJING
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610257465.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-03-04
Publication Date
2026-11-20
Estimated Expiration
2046-03-04

AI Technical Summary

Technical Problem

[0004]针对上述现有技术中存在的催化剂层与基底界面结合弱、抗反向电流能力差、机械稳定性不足等问题,本发明提供了一种适应波动工况的硫化镍自支撑解水电极原位构筑方法

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122105462B_ABST
    Figure CN122105462B_ABST
Patent Text Reader

Abstract

The application discloses a sulfidized nickel self-supporting water-splitting electrode in-situ construction method suitable for fluctuant working conditions and belongs to the technical field of hydrogen production by water electrolysis. x The nickel base material is subjected to surface etching by strong oxidizing acid to form a structure state with a micro-nano scale rough surface, and then is subjected to sulfidation treatment under mild conditions to in-situ construct a Ni / NiS heterojunction with gradient change in composition and structure. The gradient interface can realize catalyst-substrate integration, avoiding problems such as active site shielding, high interface contact resistance and weak bonding force caused by dependence on polymer adhesives in traditional processes. The integrated self-supporting sulfidized nickel electrode provided by the application can realize strong and tough bonding and efficient charge transmission between the catalyst layer and the substrate, thereby significantly improving the structural integrity and redox reversibility of the electrode under severe working conditions such as reverse current impact, bubble scouring and solution flow, and finally realizing the unity of high activity and high stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water electrolysis for hydrogen production technology, specifically relating to an in-situ construction method for a nickel sulfide self-supporting water electrolysis electrode adapted to fluctuating operating conditions. Background Technology

[0002] Green hydrogen energy is an important component of the future clean energy system and is of great significance for alleviating the environmental and energy problems caused by carbon emissions. Alkaline water electrolysis for hydrogen production is considered one of the key pathways to achieving large-scale green hydrogen production due to its relatively mature process conditions and potential for large-scale application. Further breakthroughs in this technology heavily depend on the development of catalytic electrode materials that combine high activity, high stability, and low cost. Currently, nickel-based materials are widely used as electrode substrates and active material precursors due to their abundant resources, good conductivity, structural stability, and corrosion resistance in alkaline media. To further enhance the intrinsic catalytic activity of nickel-based electrodes, researchers often modify them through strategies such as anion modification (e.g., sulfidation, phosphating), elemental doping, and interface engineering. Among these, nickel sulfide (NiS) is particularly effective. x Due to its flexible electronic structure and abundant active sites, it has shown significant potential in both hydrogen evolution and oxygen evolution reactions, making it a highly active catalytic material that has attracted much attention.

[0003] However, when existing alkaline water electrolysis electrodes are coupled with fluctuating renewable energy sources (such as wind and photovoltaics), frequent start-stop operations cause drastic fluctuations in electrode potential. Especially under reverse current impact, the high-valence catalyst material at the anode is prone to reduction, while the cathode material is easily oxidized. This leads to irreversible reconstruction of the active phase structure of the catalytic electrode, chemical corrosion, and even peeling off from the substrate, resulting in rapid degradation of electrode performance. In addition, the mechanical impact caused by the continuous growth and detachment of bubbles during industrial-grade high-current-density operation, as well as the forced flow of electrolyte, further exacerbates the mechanical detachment and failure of the catalyst layer. In traditional supported electrodes, the catalyst and substrate are mostly physically attached or simply bonded, resulting in low interfacial bonding strength. Under strong mechanical and electrochemical stress, they are prone to failure and detachment, severely restricting the long-term operational stability and engineering application of water electrolysis systems under fluctuating conditions. Summary of the Invention

[0004] To address the problems of weak bonding between the catalyst layer and the substrate interface, poor resistance to reverse current, and insufficient mechanical stability in the existing technologies, this invention provides an in-situ construction method for a self-supporting nickel sulfide water-splitting electrode adapted to fluctuating operating conditions. The method involves surface etching of the nickel substrate material with a strong oxidizing acid to form a structure with a micro / nano-scale rough surface, followed by sulfidation treatment under mild conditions to in-situ construct a Ni / NiS electrode with compositional and structural gradients. xHeterogeneous interface. This gradient interface enables catalyst-substrate integration, avoiding problems such as active site shielding, high interfacial contact resistance, and weak bonding caused by reliance on polymer binders in traditional processes. The integrated self-supporting nickel sulfide electrode provided by this invention achieves strong bonding and efficient charge transport between the catalyst layer and the substrate, thereby significantly improving the structural integrity and redox reversibility of the electrode under harsh conditions such as reverse current impact, bubble scouring, and solution flow. Ultimately, it achieves a balance between high activity and high stability, meeting the high-efficiency and stable operation requirements of industrial-grade fluctuating water electrolysis systems.

[0005] To achieve the above objectives, the present invention provides the following technical solution: One of the technical solutions of this invention is to provide an in-situ construction method for a self-supporting nickel sulfide water-splitting electrode adapted to fluctuating operating conditions, comprising the following steps: The nickel substrate material is immersed in an oxidizing acid solution for etching to obtain a nickel substrate material with a micro-nano scale rough structure on the surface; the nickel substrate material with a micro-nano scale rough structure is placed in a mixed solution of sodium thiosulfate and sodium sulfide and subjected to sulfidation treatment at a temperature not exceeding 80°C to obtain the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions.

[0006] This invention utilizes a strong oxidizing mixed acid etching process to form a transition layer with micro-nano scale roughness on the surface of a nickel substrate. This structure increases the specific surface area and exposes abundant nickel atoms, facilitating the subsequent Ni / NiS sulfide formation process. x The formation of gradient interfaces provides a crystallographic basis.

[0007] This invention employs a low-temperature liquid-phase sulfidation process, where a sulfur source reacts with nickel atoms exposed after etching under mild conditions to generate a nickel sulfide layer in situ. This differs from conventional methods such as hydrothermal / solvothermal methods, electrochemical deposition, and high-temperature vapor-phase sulfidation. These methods are either unsuitable for large-area preparation due to high reaction temperatures (typically >150℃) and complex conditions, or their deposition mechanisms limit the formation of a continuous structural gradient, resulting in insufficient bonding strength between the catalyst and the substrate. The low-temperature (≤80℃) liquid-phase sulfidation strategy employed in this invention, through precise control of interfacial diffusion and reaction kinetics, promotes a gradual sulfidation reaction from the surface inwards, naturally constructing a continuous compositional and structural gradient from metallic nickel to nickel sulfide. This process achieves chemically bonded interfacial bonding strength, laying the foundation for the long-term stability of the electrode under mechanical and electrochemical stress.

[0008] The gradient heterogeneous interface constructed in this invention effectively promotes interfacial charge transport and significantly suppresses phase reconstruction, corrosion, and interlayer delamination caused by reverse current. It can maintain the integrity of the electrode structure under severe potential reversal and mechanical shock.

[0009] The size of the nickel substrate material used in this invention can be scaled up from the conventional laboratory size (e.g., 2cm × 2cm) to the industrial size (e.g., 18cm × 18cm or more) according to actual needs.

[0010] Preferably, the nickel substrate material includes nickel foam or nickel mesh.

[0011] Preferably, the nickel substrate material undergoes surface pretreatment before etching.

[0012] More preferably, the surface pretreatment step includes: ultrasonically cleaning the nickel substrate material in acetone, anhydrous ethanol and water in sequence, and then drying it.

[0013] Preferably, the oxidizing acid solution is prepared by mixing solution 1, solution 2, solution 3 and water in a volume ratio of 2:1:1:10; solution 1 is concentrated nitric acid; solution 2 is concentrated hydrochloric acid or a salt solution with a doped metal element concentration of 1 mol / L; and solution 3 is a 1 mol / L sodium hypochlorite solution.

[0014] In this invention, concentrated nitric acid and concentrated hydrochloric acid are commercially available products, and their concentrations are commercially available concentrations.

[0015] In the technical solution of the present invention, solution 2 in the oxidizing acid solution can be concentrated hydrochloric acid, which is used to simply sulfide the nickel substrate material; solution 2 in the oxidizing acid solution can also be a salt solution of the metal element to be doped (such as Fe), so as to achieve in-situ doping of other metal elements in the catalyst layer and further optimize the electronic structure and catalytic activity.

[0016] Preferably, the etching time is 5 to 10 minutes.

[0017] Preferably, the concentration of S in the mixed solution of sodium thiosulfate and sodium sulfide is 0.5 mol / L, and the molar ratio of sodium thiosulfate to sodium sulfide is 1:1.

[0018] Preferably, the vulcanization treatment time is 6 to 12 hours.

[0019] The second technical solution of the present invention provides a nickel sulfide self-supporting water-splitting electrode adapted to fluctuating working conditions, which is prepared according to the above-mentioned in-situ construction method of nickel sulfide self-supporting water-splitting electrode adapted to fluctuating working conditions.

[0020] The nickel sulfide self-supporting water-splitting electrode prepared in this invention, adapted to fluctuating operating conditions, exhibits excellent full hydrolysis performance under industrial testing conditions (80℃, 30wt% KOH), requiring only 1.804V to reach 1000mA·cm. -2 The current density has met the U.S. Department of Energy's (DOE) 2026 technical target; at 1000 mA·cm⁻¹ -2It can operate stably for more than 800 hours without significant degradation; in 3600 acceleration start-stop cycle tests with simulated fluctuating energy input, the electrode performance remains stable, demonstrating excellent resistance to reverse current and mechanical durability.

[0021] The third technical solution of the present invention provides an application of the above-mentioned nickel sulfide self-supporting water electrolysis electrode adapted to fluctuating working conditions in water electrolysis.

[0022] The beneficial technical effects of the present invention are as follows: (1) This invention successfully constructs Ni / NiS in situ on the surface of a nickel substrate using a simple two-step method of acid etching and mild sulfidation. x A gradient interface was used to obtain a nickel sulfide self-supporting water-splitting electrode, which achieved a strong bond between the catalyst and the substrate, significantly improving the mechanical stability of the electrode and the interfacial charge transport efficiency.

[0023] (2) The electrode prepared by the present invention exhibits excellent catalytic activity and ultra-long stability at industrial-grade current density. In particular, its performance does not decay during repeated start-stop cycles under simulated fluctuating operating conditions, and it has outstanding resistance to reverse current impact.

[0024] (3) This invention confirms the presence of NiS by cross-sectional scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS) line scanning analysis. x - The formation of the Ni gradient interface; in-situ electrochemical Raman spectroscopy shows that the gradient interface can maintain strong structural stability and reversibility under reverse current; soft X-ray absorption spectroscopy (SXAS) further confirms the successful doping of Fe element at the catalytic interface.

[0025] (4) This invention breaks through the bottleneck of the difficulty in balancing activity and stability in traditional electrode design from the perspective of interface engineering. It provides a new idea for developing a highly durable water electrolysis electrode suitable for fluctuating renewable energy input. The preparation method provided is simple, mild and does not require complex equipment. It is suitable for industrial-grade large-area electrode preparation and has important scientific research value and engineering application prospects. Attached Figure Description

[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1The images show SEM images (a) of cleaned nickel foam, (b) of nickel foam with roughened surface, and (c) and a magnified view (d) of the nickel foam-based nickel sulfide self-supporting integrated electrode.

[0028] Figure 2 The image shows the XRD pattern of the foamed nickel-based nickel sulfide self-supporting integrated electrode prepared in Example 1.

[0029] Figure 3 The images shown are: (a) SEM image of the surface-roughened nickel mesh in Example 2; (b) SEM image of the nickel mesh-based nickel sulfide self-supporting integrated electrode; and (c) SEM image and elemental distribution EDS image of the cross-section of the nickel mesh-based nickel sulfide self-supporting integrated electrode.

[0030] Figure 4 For example, NiS in Example 2 x - Potential change trend and local magnification of Ni as the cathode in accelerated start-stop cycle test for water electrolysis.

[0031] Figure 5 For example, NiS in Example 2 x - Potential change trend and local magnified image of Ni as the anode in accelerated start-stop cycle test for water electrolysis.

[0032] Figure 6 For example, NiS in Example 2 x -Ni are in-situ electrochemical Raman spectra of the anode (a) and cathode (b) of water electrolysis under the corresponding oxidation and reduction potentials.

[0033] Figure 7 For example, NiS in Example 2 x -Diagram (a) of an electrolytic cell constructed using Ni as the cathode and anode for water electrolysis, respectively. x - Performance trends of electrolyzers using Ni as anode and anode versus using pure Ni mesh as anode (b) and NiS x -Ni is used as the stability evaluation result of the anode and cathode electrolyzer (c).

[0034] Figure 8 The soft X-ray absorption spectrum of the nickel mesh-based Fe-doped nickel sulfide self-supporting integrated electrode prepared in Example 3 is shown in Figure a, where a is the energy variation of the Ni L-edge, b is the energy variation of the Fe L-edge, and c is the energy variation of the SL-edge. Detailed Implementation

[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention. It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the present invention.

[0036] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.

[0037] Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, are also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0038] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar to or equivalent to those described herein may be used in the implementation or testing of this invention.

[0039] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0040] To address the problems of weak bonding between the catalyst layer and substrate interface, poor resistance to reverse current, and insufficient mechanical stability in existing electrolytic water electrolysis catalytic electrode materials, this invention provides an in-situ construction method for a nickel sulfide self-supporting water electrolysis electrode adapted to fluctuating operating conditions, comprising the following steps: First, the nickel substrate material is ultrasonically cleaned in acetone, anhydrous ethanol and water in sequence to remove surface organic contaminants and oxides, and then dried for later use. The pretreated nickel substrate material is then immersed in an oxidizing acid solution for etching to obtain a nickel substrate material with a micro-nano scale rough structure on the surface. This treatment significantly increases the specific surface area of ​​the nickel substrate material, which is beneficial to the uniform nucleation and interface fusion of subsequent sulfidation. The nickel substrate material with a micro-nano scale rough structure on its surface is placed in a mixed solution of sodium thiosulfate and sodium sulfide and subjected to sulfidation treatment at a temperature not exceeding 80°C. A self-supporting nickel sulfide catalytic layer with gradient interface bonding is constructed in situ on the surface of the nickel substrate material to obtain the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions.

[0041] Furthermore, the nickel substrate material includes nickel foam or nickel mesh.

[0042] Furthermore, the oxidizing acid solution is composed of solution 1, solution 2, solution 3 and water in a volume ratio of 2:1:1:10; solution 1 is concentrated nitric acid; solution 2 is concentrated hydrochloric acid or a salt solution with a doped metal element concentration of 1 mol / L; and solution 3 is a 1 mol / L sodium hypochlorite solution.

[0043] Furthermore, the etching time is 5 to 10 minutes.

[0044] Furthermore, the concentration of S in the mixed solution of sodium thiosulfate and sodium sulfide is 0.5 mol / L, and the molar ratio of sodium thiosulfate to sodium sulfide is 1:1.

[0045] Furthermore, the vulcanization treatment time is 6~12 hours.

[0046] Unless otherwise specified, room temperature in this invention refers to a temperature of 25±5℃.

[0047] All raw materials used in this invention are commercially available products.

[0048] Example 1 Fabrication of a self-supporting integrated nickel sulfide electrode based on small-sized nickel foam: (1) Place a 2cm×2cm piece of nickel foam in acetone, ethanol and deionized water for ultrasonic cleaning for 30min each, and vacuum dry at 60℃ for later use.

[0049] (2) Preparation of mixed oxidizing acid solution: Measure 8 mL of concentrated nitric acid, 4 mL of concentrated hydrochloric acid and 4 mL of sodium hypochlorite solution (1 mol / L), and mix them evenly with 40 mL of deionized water. Immerse the pretreated nickel foam in the acid solution, let it stand at room temperature for 5 min, take it out and rinse it with a large amount of deionized water to obtain surface roughened nickel foam.

[0050] (3) Preparation of sulfide solution: Weigh a certain amount of sodium thiosulfate (Na2S2O3·5H2O) and sodium sulfide (Na2S·9H2O), dissolve them in deionized water, and prepare a mixed solution with a total sulfur concentration of 0.5 mol / L and a molar ratio of Na2S2O3 to Na2S of 1:1. Place the mixed solution in a beaker, and then immerse the surface-roughened nickel foam into the mixed solution and react in an 80℃ water bath for 6 hours. After the reaction is completed, remove the electrode, wash it thoroughly with deionized water, and dry it under vacuum at 60℃ to obtain a nickel foam-based nickel sulfide self-supporting integrated electrode.

[0051] SEM images (a) of cleaned nickel foam, SEM image (b) of surface-roughened nickel foam, and SEM image (c) and a magnified view (d) of the nickel foam-based nickel sulfide self-supporting integrated electrode are shown in Example 1. Figure 1 .

[0052] from Figure 1 As can be seen, the surface of the nickel foam skeleton after acid etching exhibits a micro-nano scale rough structure (see reference). Figure 1 (a, b) After mild sulfidation, the rough surface is transformed in situ into a uniform catalytic layer composed of different micro- and nanoparticles, maintaining continuous connection with the substrate (see reference). Figure 1 (c, d)

[0053] The XRD pattern of the foamed nickel-based nickel sulfide self-supporting integrated electrode prepared in Example 1 is shown in Figure 1. Figure 2 .

[0054] Figure 2 The XRD pattern of the nickel foam-based nickel sulfide self-supporting integrated electrode shows strong diffraction peaks of metallic nickel at 44.5°, 51.8°, and 76.4°, and characteristic diffraction peaks of nickel sulfide (Ni3S2) at approximately 21.7°, 31.1°, 37.8°, 49.7°, and 55.2°, confirming the presence of Ni3S2. x Successful synthesis.

[0055] Example 2 Fabrication of a self-supporting integrated nickel sulfide electrode based on a medium-sized nickel mesh: (1) Place a 10cm×10cm nickel mesh in acetone, ethanol and deionized water for ultrasonic cleaning for 30min each, and vacuum dry at 60℃ for later use.

[0056] (2) Preparation of mixed oxidizing acid solution: Measure 200 mL of concentrated nitric acid, 100 mL of concentrated hydrochloric acid and 100 mL of sodium hypochlorite solution (1 mol / L), and mix them evenly with 1000 mL of deionized water. Immerse the pretreated nickel mesh in the acid solution, let it stand at room temperature for 5 min, take it out and rinse it with a large amount of deionized water to obtain a roughened nickel mesh.

[0057] (3) Preparation of sulfidation solution: Weigh a certain amount of sodium thiosulfate (Na2S2O3·5H2O) and sodium sulfide (Na2S·9H2O), dissolve them in deionized water, and prepare a mixed solution with a total sulfur concentration of 0.5 mol / L and a molar ratio of Na2S2O3 to Na2S of 1:1. Place the mixed solution in a beaker, and then immerse the roughened nickel mesh in the mixed solution and react in an 80℃ water bath for 6 hours. After the reaction is complete, remove the mesh, wash it thoroughly with deionized water, and dry it under vacuum at 60℃ to obtain a nickel mesh-based nickel sulfide self-supporting integrated electrode (labeled as NiS). x -Ni).

[0058] SEM images (a) of the surface-roughened nickel mesh, (b) of the nickel mesh-based nickel sulfide self-supporting integrated electrode, and (c) of the cross-section and elemental distribution EDS diagram of the nickel mesh-based nickel sulfide self-supporting integrated electrode are shown in Example 2. Figure 3 .

[0059] Figure 3 As shown, the electrode surface obtained in Example 2 is uniformly covered with a nickel sulfide catalyst layer, and SEM results show that a multi-level micro-nano sulfide structure is formed on the surface of the nickel mesh electrode (see reference). Figure 3 (a, b) Cross-sectional SEM and elemental X-ray energy dispersive spectroscopy (EDS mapping) further revealed that the Ni signal intensity remained continuous from the inside to the surface of the nickel mesh skeleton, while the S signal gradually increased from the inside to the outside, directly confirming the NiS... x - Formation of the Ni gradient interface (see reference) Figure 3 (c) further demonstrates the applicability of the in-situ construction method provided by the present invention to nickel mesh substrates and medium-sized samples.

[0060] NiS in Example 2 x Ni was used as the cathode and anode for water electrolysis, respectively, and NiS was subjected to simulated conditions. x The performance of -Ni was tested.

[0061] The constructed three-electrode electrolytic cell was subjected to 3600 accelerated start-stop cycles, with the cathode repeatedly starting and stopping under a condition of -500 mA·cm⁻¹. -2 Hold for 60 seconds, then hold at 0.8V (vs. RHE) for 60 seconds, repeat 3600 times; the anode start-stop condition is 500 mA·cm. -2 Hold for 60 seconds, then hold at 0.3V (vs. RHE) for 60 seconds, repeat 3600 times.

[0062] The potential change trend and local magnified image during the repeated start-up and shutdown of the cathode are shown below. Figure 4 The potential change trend and local magnified diagram during the repeated start-up and shutdown of the anode are shown in the figure. Figure 5 .

[0063] Figure 4 and Figure 5 As shown, NiS in Example 2 x -Ni, used as both the cathode and anode in water electrolysis, maintained stable performance during 3600 accelerated start-stop cycles under simulated fluctuating conditions, demonstrating its excellent resistance to reverse current and mechanical durability.

[0064] NiS in Example 2 x The in-situ electrochemical Raman spectra of Ni as the anode (a) and cathode (b) in water electrolysis under the corresponding oxidation and reduction potentials are shown below. Figure 6 .

[0065] Figure 6 In-situ electrochemical Raman results show that NiS x The Ni electrode exhibits stable surface structure during repeated cathode start-up and shutdown, maintaining its Ni3S2 structural state within a reverse potential range of 0.2V~0.8V (vs. RHE); NiS x - The Ni anode can be effectively reconstructed into the corresponding oxide active structure during oxygen evolution service, and can maintain between Ni(OH)2 and NiOOH during repeated start-up and shutdown, thus maintaining good reversibility.

[0066] Diagram (a) of the constructed electrolytic cell, NiS x - Performance trends of electrolyzers using Ni as anode and anode versus using pure Ni mesh as anode (b) and NiS x The stability evaluation results of Ni as an anode and cathode electrolyzer are shown in [the table]. Figure 7 .

[0067] Figure 7 The results showed that, when tested in a 30 wt% KOH solution at 80 °C, the total hydrolysis performance required only 1.804 V to drive 1000 mA·cm. -2 Current density (refer to) Figure 7 (b) The system operates at 1000 mA·cm -2 After 800 hours of continuous operation at current density, the voltage decay was only 0.11% (for reference). Figure 7 (c)

[0068] Example 3 Fabrication of Fe-doped nickel sulfide self-supporting integrated electrode based on large-size nickel mesh: (1) Place a 18cm×18cm nickel mesh in acetone, ethanol and deionized water for ultrasonic cleaning for 30min each, and vacuum dry at 60℃ for later use.

[0069] (2) Preparation of mixed oxidizing acid solution containing doped elements: Replace the concentrated hydrochloric acid in Example 2 with ferric chloride solution (1 mol / L), and then scale up the process proportionally. Immerse the pretreated nickel mesh in the acid solution, let it stand at room temperature for 6 minutes, and then rinse it with a large amount of deionized water to obtain a roughened Fe-doped nickel mesh.

[0070] (3) Preparation of sulfide solution: Weigh a certain amount of sodium thiosulfate (Na2S2O3·5H2O) and sodium sulfide (Na2S·9H2O), dissolve them in deionized water, and prepare a mixed solution with a total sulfur concentration of 0.5 mol / L and a molar ratio of Na2S2O3 to Na2S of 1:1. Place the mixed solution in a beaker, and then immerse the roughened Fe-doped nickel mesh in the mixed solution and react in an 80℃ water bath for 6 hours. After the reaction is complete, remove the mesh, wash it thoroughly with deionized water, and dry it under vacuum at 60℃ to obtain a nickel mesh-based Fe-doped nickel sulfide self-supporting integrated electrode.

[0071] Example 3 shows the soft X-ray absorption spectrum of the nickel mesh-based Fe-doped nickel sulfide self-supporting integrated electrode. Figure 8 Where a is the energy variation diagram of Ni L-edge, b is the energy variation diagram of Fe L-edge, and c is the energy variation diagram of SL-edge.

[0072] Figure 8 Soft X-ray absorption spectroscopy (SXAS) analysis confirmed the successful incorporation of Fe into the nickel sulfide lattice (featured absorption edge peaks of Fe L3 and L2 at 706.5 eV and 720 eV, respectively, see reference). Figure 8 (b) This demonstrates the flexibility and superiority of the method provided by this invention in fabricating large-size electrodes and controlling elemental doping, offering a feasible path for customizing electrode performance for industrial applications.

[0073] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for in-situ construction of a nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions, characterized in that, Includes the following steps: The nickel substrate material is immersed in an oxidizing acid solution for etching to obtain a nickel substrate material with a micro-nano scale rough structure on the surface; the nickel substrate material with a micro-nano scale rough structure is placed in a mixed solution of sodium thiosulfate and sodium sulfide and subjected to sulfidation treatment at a temperature not exceeding 80°C to obtain the nickel sulfide self-supporting water-dissolving electrode adapted to fluctuating operating conditions. The concentration of S in the mixed solution of sodium thiosulfate and sodium sulfide is 0.5 mol / L, and the molar ratio of sodium thiosulfate to sodium sulfide is 1:

1. The vulcanization treatment takes 6 to 12 hours.

2. The in-situ construction method of the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions according to claim 1, characterized in that, The nickel substrate material includes nickel foam or nickel mesh.

3. The in-situ construction method of the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions according to claim 1, characterized in that, The nickel substrate material undergoes surface pretreatment before etching.

4. The in-situ construction method of the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions according to claim 1, characterized in that, The oxidizing acid solution is composed of solution 1, solution 2, solution 3 and water in a volume ratio of 2:1:1:10; solution 1 is concentrated nitric acid; solution 2 is concentrated hydrochloric acid or a salt solution with a doped metal element concentration of 1 mol / L; solution 3 is a 1 mol / L sodium hypochlorite solution.

5. The in-situ construction method of the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions according to claim 1, characterized in that, The etching time is 5-10 minutes.

6. A nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions, prepared by the in-situ construction method of the nickel sulfide self-supporting water-splitting electrode adapted to fluctuating operating conditions according to any one of claims 1 to 5.

7. The application of the nickel sulfide self-supporting water electrolysis electrode adapted to fluctuating operating conditions as described in claim 6 in water electrolysis.

Citation Information

Patent Citations

  • Surface modification method of transition metal-based water electrolysis catalytic material and catalytic material

    CN116463669A

  • Catalyst for producing hydrogen by electrolyzing seawater under fluctuating working condition and preparation method of catalyst

    CN120556070A