A multilayer structure high bearing self-lubricating erosion-resistant coating and a preparation method and application thereof

By employing a multi-layered coating design and utilizing the columnar crystal morphology of Nb and NbC transition layers, interlayer stress is alleviated and adhesion is enhanced. This solves the problem of friction, wear, and corrosion of metal-ceramic coatings in marine environments, achieving a synergistic improvement in self-lubricating and wear-resistant properties, and extending the life of mechanical parts.

CN122147226BActive Publication Date: 2026-11-24GUANGDONG INST OF NEW MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610297759.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-03-12
Publication Date
2026-11-24
Estimated Expiration
2046-03-12

AI Technical Summary

Technical Problem

Existing metal-ceramic coatings suffer from severe friction, wear, and corrosion problems in marine environments, exhibiting risks of pore corrosion, high friction coefficients, poor wear resistance, and difficulty in meeting the requirements for long life and high reliability under dynamic friction-wear-corrosion coupling.

Method used

The coating adopts a multi-layer structure design, including a metal-ceramic support layer, a transition layer, and a DLC layer. The transition layer consists of an Nb main transition layer and an NbC transition layer. The transition layer has a columnar crystal morphology. By matching the passivation characteristics and thermal expansion coefficient of Nb, the interlayer stress is relieved, forming a mechanical interlocking mechanism and improving the bonding force.

Benefits of technology

It improves the coating's bonding strength, load-bearing capacity, corrosion resistance, and protective durability, achieving a synergistic enhancement of self-lubricating and wear-resistant properties, and extending the service life of mechanical parts and equipment safety under marine conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122147226B_ABST
    Figure CN122147226B_ABST
Patent Text Reader

Abstract

This invention discloses a multilayer high-load-bearing self-lubricating and corrosion-resistant coating, its preparation method, and its application, belonging to the field of composite coating technology. The multilayer high-load-bearing self-lubricating and corrosion-resistant coating comprises a metal-ceramic support layer, a transition layer, and a DLC layer sequentially disposed on the substrate surface; wherein, the transition layer includes an Nb main transition layer far from the DLC layer and an NbC transition layer close to the DLC layer; the transition layer has a columnar crystal morphology; the total thickness of the transition layer is 0.1μm~2μm. This multilayer high-load-bearing self-lubricating and corrosion-resistant coating, through a specific multilayer structure design, progressively alleviates the thermal / compressive stress between layers, effectively improving the coating's bonding strength, load-bearing capacity, corrosion resistance, and protective durability, achieving a synergistic improvement in the coating's self-lubricating and corrosion-resistant properties, and can improve the service life of components and equipment safety under marine working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite coating technology, and more specifically, to a multilayer high load-bearing self-lubricating wear-resistant coating, its preparation method, and its application. Background Technology

[0002] With the continuous development of the marine economy, the requirements for moving equipment components used in marine environments are also increasing. Marine engineering equipment is directly exposed to the marine environment during operation, suffering from the combined corrosive effects of chemical and electrochemical interactions in the marine atmosphere, as well as friction and wear at the interfaces caused by interactions between moving metal parts. This significantly accelerates the damage and failure of metal materials, thereby reducing service life and reliability. Since metal materials typically exhibit high coefficients of friction and poor wear resistance, and direct contact with seawater causes surface corrosion, further reducing the mechanical properties of the metal, preparing a protective functional coating that provides lubrication, wear resistance, and corrosion protection on the metal surface is an effective strategy.

[0003] Currently, many cermet coatings with excellent mechanical properties and wear and corrosion resistance are widely used for surface protection of mechanical parts, such as tungsten carbide-based and chromium carbide-based cermet coatings. However, these coatings have high porosity, making them susceptible to corrosion by corrosive media (such as Cl). - It is easy for it to penetrate through pores and reach the substrate surface, thus corroding the substrate and posing a potential risk. Furthermore, the high coefficient of friction of cermet coatings, while wear-resistant, does not reduce friction, resulting in additional energy loss. The lack of lubrication during frictional contact also leads to severe wear on the mating components. Some existing technologies use diamond-like carbon (DLC) films as surface protective coatings; however, DLC films suffer from high internal stress and a significant difference in hardness and elastic modulus compared to the metal substrate. This causes the film to collapse and peel off under heavy-load friction and wear due to plastic deformation of the substrate or high tensile stress within the film, a phenomenon known as the "eggshell effect." Other existing technologies combine DLC and WC coatings, but simply combining a hard coating with a DLC film is insufficient to meet the long lifespan and high reliability requirements of moving and transmission components under dynamic friction-wear-corrosion coupled damage in harsh marine environments.

[0004] In view of this, the present invention is proposed. Summary of the Invention

[0005] The purpose of this invention is to provide a multilayer high load-bearing self-lubricating wear-resistant coating, its preparation method and application, in order to solve or improve the above-mentioned technical problems.

[0006] This invention can be implemented as follows: In a first aspect, the present invention provides a multilayer high load-bearing self-lubricating wear-resistant coating, comprising a metal-ceramic support layer, a transition layer and a DLC layer sequentially disposed on the surface of a substrate. The transition layer includes a Nb main transition layer far from the DLC layer and an NbC transition layer close to the DLC layer; the overall transition layer has a columnar crystal morphology; the total thickness of the transition layer is 0.1 μm to 2 μm.

[0007] In an optional implementation, the total thickness of the transition layer is 0.1 μm to 1 μm.

[0008] In an optional embodiment, the metal-ceramic support layer has at least one of the following characteristics: Feature 1: The cermet support layer is a WC-based hard alloy coating; preferably, the cermet support layer comprises a WC hard phase and a NiMoCrFeCo binder phase in a mass ratio of 3:1 to 5:1; Feature 2: The thickness of the metal-ceramic support layer is 50μm~300μm; Feature 3: The surface roughness Ra of the metal-ceramic support layer is 0.05μm~0.3μm; Feature 4: The hardness of the metal-ceramic support layer is greater than that of the substrate, and the hardness of the metal-ceramic support layer is less than that of the DLC layer.

[0009] In an optional implementation, the DLC layer has at least one of the following characteristics: Feature 5: The thickness of the DLC layer is 200nm~3μm; Feature 6: DLC layers have high SP 3 Amorphous DLC film with high content.

[0010] In an optional embodiment, the multilayer high-load-bearing self-lubricating and wear-resistant coating further includes at least one of the following features: Feature 7: The total thickness of the multi-layered, high-load-bearing, self-lubricating, and wear-resistant coating is 50.3 μm to 305 μm; Feature 8: A mechanical interlocking mechanism is formed between the transition layer and the DLC layer.

[0011] In a second aspect, the present invention provides a method for preparing a multilayer high load-bearing self-lubricating wear-resistant coating as described in any of the foregoing embodiments, comprising the following steps: sequentially depositing a metal-ceramic support layer, a transition layer and a DLC layer on the surface of a substrate.

[0012] In an optional embodiment, a metal-ceramic support layer is prepared by supersonic flame spraying. The preparation conditions for the metal-ceramic support layer include: carrier gas of 5MPa~10MPa, oxygen flow rate of 750L / min~1000L / min, kerosene flow rate of 18L / h~32L / h, powder feeding rate of 50g / min~150g / min, spray distance of 100mm~200mm, and spray gun moving speed of 10mm / s~30mm / s.

[0013] In an optional implementation, the transition layer is prepared by magnetron sputtering; The preparation of the transition layer includes: evacuating the deposition furnace to a vacuum level of 1×10⁻⁶. -3 Pa~5×10 -3 Pa, inert gas is introduced into the coating chamber at a flow rate of 50 sccm to 180 sccm and a vacuum degree of 0.1 Pa to 0.6 Pa; the bias voltage is -50 V to -300 V, the metal target is turned on, and a transition layer is deposited on the surface of the metal-ceramic support layer at a deposition power of 500 W to 2000 W and a deposition time of 10 min to 60 min.

[0014] In an optional embodiment, the DLC layer is prepared by arc ion plating; The preparation of the DLC layer includes: turning off the metal target, introducing an inert gas into the coating chamber at a flow rate of 60 sccm to 180 sccm and a vacuum of 0.1 Pa to 0.3 Pa; a bias voltage of -30 V to -200 V; turning on the carbon target; depositing the DLC layer on the surface of the transition layer at a target current of 50 A to 100 A and a deposition time of 30 min to 100 min.

[0015] In an optional embodiment, the metal-ceramic support layer is further subjected to grinding and polishing as well as ion beam cleaning before the transition layer is prepared. The polishing process includes polishing with 200-3000 mesh sandpaper at 200-1200 rpm until the surface roughness of the metal-ceramic support layer reaches Ra of 0.05 μm-0.3 μm. Ion beam cleaning includes sequential glow discharge cleaning and ion bombardment cleaning. Glow discharge cleaning includes: introducing inert gas into the coating chamber at a flow rate of 60 sccm to 200 sccm, a vacuum of 1.0 Pa to 3 Pa, a bias voltage of -1000 V to -600 V, and a glow discharge duration of 10 min to 30 min. Ion bombardment cleaning conditions include: an inert gas flow rate of 60 sccm to 160 sccm, a vacuum of 0.2 Pa to 0.8 Pa, a bias voltage of -800 V to -500 V, and a duration of 10 min to 20 min.

[0016] Thirdly, the present invention provides a mechanical component for marine applications, wherein the surface of the mechanical component for marine applications has a multi-layered, high-load-bearing, self-lubricating, wear-resistant and corrosion-resistant coating as described in any of the foregoing embodiments.

[0017] The beneficial effects of this invention include: This invention specifically employs metallic Nb to prepare the transition layer. Nb primarily forms a main Nb transition layer between the metal-ceramic support layer and the DLC layer, and reacts with C on the surface of the DLC layer to form a thinner NbC transition layer. This results in a certain degree of compositional transition among the metal-ceramic support layer, the transition layer, and the DLC layer. Furthermore, the passivation characteristics and thermal expansion coefficient of Nb are close to those of WC and DLC, which can play a superior role in the composite coating provided by this invention. The thickness of the transition layer also directly affects the performance of the composite coating; both excessively thick and thin transition layers will lead to a decrease in the overall adhesion of the coating. In this invention, the transition layer is entirely a columnar crystalline layer. The longitudinal grain boundaries of the columnar crystals provide a preferential path for stress release, reducing the risk of crack propagation perpendicular to the coating direction through grain boundary sliding or microcrack deflection. Moreover, the thermal expansion coefficient of the columnar crystal structure is closer to that of the metal and ceramic substrates, which can reduce interfacial thermal mismatch stress. In addition, the serrated structure at the top of the columnar crystals can, to some extent, form a mechanical interlock with subsequent coatings, thereby further improving the adhesion.

[0018] The multi-layer high load-bearing self-lubricating wear-resistant coating provided by this invention, through a specific multi-layer structure design, gradually alleviates the thermal / compressive stress between layers, effectively improving the coating's bonding strength, load-bearing capacity, corrosion resistance, and protective durability. It achieves a synergistic improvement in the coating's self-lubricating and wear-resistant properties, which can enhance the service life of components and the safety of equipment under marine working conditions. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 A schematic diagram of a multilayer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating provided by the present invention; Figure 2 This is an electron microscope schematic diagram of the transition layer of the multilayer high load-bearing self-lubricating wear-resistant coating prepared in Example 1 of this test example; Figure 3 for Figure 2 High-resolution TEM image of the intermediate transition layer; Figure 4This is a schematic diagram comparing the scratch test results of the coated products in Example 1 and Comparative Examples 3-6 in Experimental Example 2; Figures 5 to 7 This is a schematic diagram comparing the mechanical properties of the coating products of Example 1 and Comparative Examples 1-4 in Experimental Example 2; Figure 8 This is a schematic diagram comparing the tribological properties of the coating products of Example 1 and Comparative Examples 3-4 in seawater environment in Experimental Example 2. Figure 9 The SEM-EDS characterization results are for Example 1 and Comparative Example 4 in Experimental Example 2; Figure 10 The polarization curves are for the coating products of Example 1, Comparative Example 2 and Comparative Example 4 in Experimental Example 2.

[0021] Icons: 100 - Metal-ceramic support layer; 200 - Transition layer; 300 - DLC layer. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0023] The following is a detailed description of the multilayer high load-bearing self-lubricating wear-resistant coating, its preparation method, and its application provided by the present invention.

[0024] This invention provides a multilayer high-load-bearing, self-lubricating, wear-resistant and corrosion-resistant coating, such as... Figure 1 As shown, it includes a metal-ceramic support layer 100, a transition layer 200, and a DLC layer 300 sequentially disposed on the surface of the substrate.

[0025] The substrate can be regarded as a mechanical part. By forming a multi-layered, high-load-bearing, self-lubricating, wear-resistant and corrosion-resistant coating on certain areas of the mechanical part in a special environment, the effect of corrosion prevention and wear resistance can be achieved.

[0026] In this invention, the cermet support layer 100 is a WC-based cemented carbide coating, such as a WC-Ni-based cemented carbide coating. This WC-based cemented carbide coating contains a WC hard phase and a NiMoCrFeCo binder phase. The mass ratio of the WC hard phase to the NiMoCrFeCo binder phase can be from 3:1 to 5:1, such as 3:1, 3.5:1, 4:1, 4.5:1, or 5:1, or other values ​​within the range of 3:1 to 5:1. The tungsten carbide binder has a certain influence on the performance of the multilayer composite coating. If the binder phase is not selected appropriately, it may result in low coating density, decreased hardness and toughness, and insufficient corrosion resistance; if there is too much binder phase, it will lead to insufficient coating hardness. This invention uses Ni-based alloys such as NiMoCrFeCo as the binder phase of the WC-based coating, which can provide long-term corrosion protection and strong support for the surface layer.

[0027] In some alternative embodiments, the thickness of the metal-ceramic support layer 100 can be 50μm to 300μm, such as 50μm, 80μm, 100μm, 150μm, 200μm, 250μm or 300μm, or other values ​​within the range of 50μm to 300μm.

[0028] If the thickness of the metal-ceramic support layer 100 is less than 50 μm, it is not conducive to the load-bearing capacity of the coating; if the thickness of the metal-ceramic support layer 100 is greater than 300 μm, it is not conducive to the interfacial bonding between the coatings.

[0029] In some optional embodiments, the surface roughness Ra of the metal-ceramic support layer 100 can be 0.05 μm to 0.3 μm, such as 0.05 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm or 0.3 μm, or other values ​​in the range of 0.05 μm to 0.3 μm.

[0030] By controlling the surface roughness Ra of the metal-ceramic support layer 100 to 0.05μm~0.3μm, it is beneficial to form an effective mechanical interlock between the transition layer 200 and the DLC layer 300.

[0031] In some alternative embodiments, the hardness of the cermet support layer 100 is greater than that of the substrate, and the hardness of the cermet support layer 100 is less than that of the DLC layer 300, thereby creating a hardness transition between the substrate and the DLC layer 300.

[0032] In this invention, the transition layer 200 includes a Nb main transition layer 200 that is far from the DLC layer 300 and an NbC transition layer 200 that is close to the DLC layer 300; the transition layer 200 has a columnar crystal morphology; the total thickness of the transition layer 200 is 0.1 μm to 2 μm.

[0033] The aforementioned transition layer 200 is located between the cermet support layer 100 and the DLC layer 300, and can mitigate the differences in properties between the main component materials of the cermet support layer 100 and the DLC layer 300. It should be emphasized that, in this invention, the type of transition layer 200 directly affects the corrosion resistance and adhesion of the composite coating. If the corrosion resistance of the transition layer 200 is too poor, it will accelerate the corrosion of the transition layer 200 when the corrosive medium penetrates through the DLC layer 300. If the thermal expansion coefficients of the transition layer 200, the WC base coating, and the DLC layer 300 differ significantly, it will result in poor adhesion between the multiple coating layers, leading to the peeling off of the DLC layer 300 upon wear. This invention specifically employs metallic Nb to prepare the transition layer 200. Nb primarily forms the Nb main transition layer 200 between the cermet support layer 100 and the DLC layer 300, and reacts with C on the surface of the DLC layer 300 to form a thinner NbC transition layer 200. This results in a certain degree of compositional transition among the cermet support layer 100, the transition layer 200, and the DLC layer 300. The Nb specifically used in this invention has passivation characteristics and a coefficient of thermal expansion close to those of WC and DLC, enabling it to achieve superior performance in the composite coating provided by this invention. Using commonly used metallic Ti or Cr to prepare the transition layer 200 would lead to problems such as mismatched coefficients of thermal expansion and modulus imbalance, resulting in decreased coating adhesion.

[0034] In some optional embodiments, the total thickness of the transition layer 200 can be 0.1 μm to 2 μm, such as 0.1 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, or 2 μm, or other values ​​within the range of 0.1 μm to 2 μm. In some preferred embodiments, the total thickness of the transition layer 200 is 0.1 μm to 1 μm, such as 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, or 1 μm. The thickness of the transition layer 200 directly affects the performance of the composite coating; both excessively thick and excessively thin transition layer 200 will lead to a decrease in the overall adhesion of the coating.

[0035] In this invention, the transition layer 200 is a columnar crystalline layer. Columnar crystals, as observed under a scanning electron microscope, have a crystallographic orientation that aligns along a certain direction, typically exhibiting a relatively regular columnar shape, and show certain preferred orientation growth characteristics during the growth process. The longitudinal grain boundaries of the columnar crystals in the transition layer 200 provide a preferred path for stress release, reducing the risk of crack propagation perpendicular to the coating direction through grain boundary sliding or microcrack deflection. Furthermore, the coefficient of thermal expansion of the columnar crystal structure is closer to that of metal and ceramic substrates, which can reduce interfacial thermal mismatch stress. In addition, the serrated structure at the top of the columnar crystals can, to some extent, form a mechanical interlock with subsequent coatings, thereby further enhancing the adhesion.

[0036] In this invention, the thickness of the DLC layer 300 can be 200 nm to 3 μm, such as 200 nm, 500 nm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, or 3 μm, or other values ​​within the range of 200 nm to 3 μm. In some preferred embodiments, the thickness of the DLC layer 300 can be 500 nm to 3 μm.

[0037] If the thickness of the DLC layer 300 is less than 200nm, it will wear through quickly under high load; if the thickness of the DLC layer 300 is greater than 3μm, it will cause excessive internal stress and make it easy to peel off during service.

[0038] DLC layer 300 is a high SP 3 Amorphous DLC film with high content.

[0039] In some optional embodiments, the total thickness of the multilayer high load-bearing self-lubricating and wear-resistant coating is 50.3 μm to 305 μm, preferably 100 μm to 300 μm.

[0040] In some optional embodiments, the nanohardness of the multilayer high load-bearing self-lubricating wear-resistant coating is not less than 29 GPa, such as 29.12 GPa to 32.15 GPa.

[0041] In some optional embodiments, the elastic modulus of the multilayer high load-bearing self-lubricating wear-resistant coating is not less than 330 GPa, such as 333.61 GPa to 390.46 GPa.

[0042] In some alternative implementations, the H-layer structure of the high load-bearing, self-lubricating, wear-resistant coating... 3 / E 2 The value should not be lower than 0.21 GPa, such as 0.218 GPa to 0.226 GPa.

[0043] In some alternative implementations, the normal load corresponding to the cracking of the multilayer high load-bearing self-lubricating wear-resistant coating is not less than 15N, such as 15.3N to 17.3N, and further not less than 17N.

[0044] In some alternative implementations, the wear rate of the multilayer high-load-bearing self-lubricating corrosion-resistant coating after 18,000 wear cycles does not exceed 10.5 × 10⁻⁶. -7 / mm 3 ·N -1 ·m -1 For example, 7.12×10 -7 / mm 3 ·N -1 ·m -1 ~10.06×10 -7 / mm3 ·N -1 ·m -1 Further not exceeding 7.15×10 -7 / mm 3 ·N -1 ·m -1 .

[0045] In some alternative implementations, the corrosion current density of the multilayer high-load-bearing self-lubricating corrosion-resistant coating does not exceed 1.9 A / cm². 2 For example, 1.69A / cm 2 ~1.88A / cm 2 Further not exceeding 1.7A / cm 2 .

[0046] Building upon the above, this invention, by setting the aforementioned special transition layer 200, gradually alleviates the thermal / compressive stress between layers, improves the coating's bonding strength, load-bearing capacity, corrosion resistance, and protective durability, further achieving a synergistic improvement in the coating's self-lubricating and wear-resistant properties, and mitigating the risk of diamond-like carbon (DLC) surface layer detachment during long-term service due to insufficient interfacial bonding or galvanic corrosion, ultimately improving the service life and equipment safety of components (such as bearing thrust discs, couplings, bushings, and spherical bearings) under marine operating conditions.

[0047] Accordingly, the present invention also provides a method for preparing the above-mentioned multilayer high load-bearing self-lubricating wear-resistant coating, comprising the following steps: sequentially depositing a metal-ceramic support layer 100, a transition layer 200, and a DLC layer 300 on the surface of a substrate.

[0048] In some alternative embodiments, the substrate may be degreased and deoiled first, followed by sandblasting of the spraying area, and then the metal-ceramic support layer 100 may be prepared.

[0049] Sandblasting removes the oxide layer from the substrate surface, increasing surface activity and improving the adhesion between the coating and the substrate. The abrasive material used for sandblasting can be white fused alumina, brown fused alumina, or zirconium fused alumina, with a particle size of 54# or 60#, etc. During sandblasting, the blasting pressure can be controlled between 0.2MPa and 0.6MPa, and the blasting distance can be controlled between 50mm and 350mm. The nozzle of the sandblasting machine maintains an angle of 60° to 90° with the sample surface. After sandblasting, the sample surface has a uniform roughness and no metallic luster; residual abrasive particles or dust can be blown away with compressed air.

[0050] In some optional embodiments, the metal-ceramic support layer 100 can be prepared by supersonic flame spraying. The preparation conditions for the metal-ceramic support layer 100 may include: a carrier gas pressure of 5 MPa to 10 MPa (e.g., 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, or 10 MPa), an oxygen flow rate of 750 L / min to 1000 L / min (e.g., 750 L / min, 800 L / min, 850 L / min, 900 L / min, 950 L / min, or 1000 L / min), and a kerosene flow rate of 18 L / h to 32 L / h (e.g., 18 L / h, 20 L / h, 25 L / h, 3...). The powder feeding rate is 50g / min to 150g / min (e.g., 50g / min, 80g / min, 100g / min, 120g / min or 150g / min), the spray distance is 100mm to 200mm (e.g., 100mm, 120mm, 150mm, 180mm or 200mm), and the spray gun moving speed is 10mm / s to 30mm / s (e.g., 10mm / s, 15mm / s, 20mm / s, 25mm / s or 30mm / s).

[0051] The selection of parameters in thermal spraying is crucial to the performance of multilayer composite coatings. Inappropriate parameter selection can lead to uneven cooling, intermittent coating buildup, poor adhesion, and powder supply interruptions. Similarly, the selection of the tungsten carbide binder phase in thermal spraying is critical to the performance of multilayer composite coatings. An inappropriate binder phase can result in lower coating density, reduced hardness and toughness, and insufficient corrosion resistance. For example, in the above process, a spray distance of less than 100 mm can easily lead to a sharp increase in thermal stress in the coating, causing defects such as warping and cracking; a spray distance greater than 200 mm can easily lead to a significant decrease in coating adhesion strength and an increase in porosity.

[0052] In some alternative embodiments, the transition layer 200 can be prepared by magnetron sputtering. The preparation of the transition layer 200 may include: evacuating the deposition furnace to a vacuum level of 1 × 10⁻⁶. -3 Pa~5×10 -3 Pa (e.g., 1×10) -3 Pa, 2×10 -3 Pa, 3×10 - 3 Pa, 4×10 -3 Pa or 5×10 -3An inert gas is introduced into the coating chamber at a flow rate of 50 sccm to 180 sccm (e.g., 50 sccm, 80 sccm, 100 sccm, 150 sccm, or 180 sccm), with a vacuum degree of 0.1 Pa to 0.6 Pa (e.g., 0.1 Pa, 0.2 Pa, 0.3 Pa, 0.4 Pa, 0.5 Pa, or 0.6 Pa). The bias voltage is -50 V to -300 V (e.g., -50 V, -100 V, -150 V, -200 V, -250 V, or -300 V). The metal target is turned on, and a transition layer 200 is deposited on the surface of the metal-ceramic support layer 100 at a deposition power of 500 W to 2000 W (e.g., 500 W, 1000 W, 1500 W, or 2000 W) and a deposition time of 10 min to 60 min (e.g., 10 min, 20 min, 40 min, or 60 min).

[0053] In the above process, if the vacuum level is below 0.1 Pa, the difficulty of gas ionization increases sharply, making it difficult to form a continuous and uniform film layer, resulting in poor adhesion between the film and the metal-ceramic support layer 100. If the vacuum level is above 0.6 Pa, it is easy for atoms to be difficult to arrange in an orderly manner during film growth, leading to decreased crystallinity, increased roughness, and a tendency for film peeling. If the bias voltage is below -50V (e.g., -40V), it is easy for the coating porosity to be high; if the bias voltage is above -300V (e.g., -320V), it is easy for the internal stress of the coating to be too high, inducing microcracks. If the deposition time is less than 10 min, the deposited Nb layer is easy to be too thin, failing to form an effective transition; if the deposition time is more than 60 min, the Nb layer is easy to be too thick, and its low strength can easily induce DLC layer collapse under heavy load wear.

[0054] In some alternative embodiments, the metal-ceramic support layer 100 is further subjected to polishing and ion beam cleaning before the transition layer 200 is prepared.

[0055] The polishing process includes polishing with 200-3000 grit sandpaper at 200 rpm to 1200 rpm (such as 200 rpm, 500 rpm, 800 rpm, 1000 rpm or 1200 rpm, etc.) until the surface roughness of the metal-ceramic support layer 100 reaches Ra of 0.05 μm to 0.2 μm.

[0056] This invention controls the surface roughness Ra of the metal-ceramic support layer 100 within the range of 0.05 μm to 0.2 μm, which helps to achieve a balance between mechanical interlocking, chemical bonding, and stress buffering, thereby improving the bonding effect between film layers. If the roughness is too high (Ra>0.2 μm), sharp protrusions or deep grooves will cause local stress concentration in the DLC layer 300, which is prone to cracking or peeling; while if it is too smooth (Ra<0.05 μm), there is a lack of anchoring points, resulting in insufficient bonding force; the range of 0.05 μm to 0.2 μm just balances the two, ensuring uniform stress distribution.

[0057] Ion beam cleaning includes sequential glow discharge cleaning and ion bombardment cleaning. Glow discharge cleaning involves introducing an inert gas into the coating chamber at a flow rate of 60 sccm to 200 sccm (e.g., 60 sccm, 80 sccm, 100 sccm, 150 sccm, or 200 sccm), a vacuum level of 1.0 Pa to 3 Pa (e.g., 1 Pa, 2 Pa, or 3 Pa), a bias voltage of -1000V to -600V (e.g., -1000V, -900V, -800V, -700V, or -600V), and a glow discharge duration of 10 min to 30 min (e.g., 10 m). The ion bombardment cleaning conditions include: an inert gas flow rate of 60 sccm to 160 sccm (e.g., 60 sccm, 100 sccm, 120 sccm, 150 sccm, or 160 sccm), a vacuum degree of 0.2 Pa to 0.8 Pa (e.g., 0.2 Pa, 0.5 Pa, or 0.8 Pa), a bias voltage of -800 V to -500 V (e.g., -800 V, -700 V, -600 V, or -500 V), and a duration of 10 min to 20 min (e.g., 10 min, 15 min, or 20 min).

[0058] In some alternative implementations, the DLC layer 300 can be prepared by arc ion plating. The fabrication of the DLC layer 300 may include: turning off the metal target, introducing an inert gas into the coating chamber at a flow rate of 60 sccm to 180 sccm (e.g., 60 sccm, 80 sccm, 100 sccm, 120 sccm, 150 sccm, or 180 sccm), maintaining a vacuum level of 0.1 Pa to 0.3 Pa (e.g., 0.1 Pa, 0.2 Pa, or 0.3 Pa), a bias voltage of -30 V to -200 V (e.g., -30 V, -50 V, -100 V, -150 V, or -200 V), turning on the carbon target, depositing the DLC layer 300 on the surface of the transition layer 200, using a target current of 50 A to 100 A (e.g., 50 A, 60 A, 70 A, 80 A, 90 A, or 100 A), and a deposition time of 30 min to 100 min (e.g., 30 min, 50 min, 80 min, or 100 min).

[0059] In the above process, if the vacuum level is below 0.1 Pa, the difficulty of gas ionization will increase sharply, making it difficult to form a continuous and uniform film layer, resulting in poor adhesion between the film and the metal transition layer 200. If the vacuum level is above 0.3 Pa, the film growth may not be able to fully fill the pores during the film growth process, failing to meet the corrosion resistance requirements. If the target current is less than 50 A, it may lead to difficulties in arc initiation and ineffective film deposition. If the target current is greater than 100 A, it may lead to a sharp increase in the surface roughness of the coating, resulting in obvious defects such as particle protrusions and pinholes.

[0060] In the above preparation process, a carbon source is provided by a carbon target, and a negative bias voltage enhances the ion bombardment energy to break the orderly arrangement of carbon chains, forming a high sp2+ carbon chain. 3 The amorphous DLC film with a diamond-like carbon content is densified under high bias to reduce porosity. The DLC layer 300 serves as the final functional layer, providing surface protection for the coating system through ultra-low friction, high hardness, and chemical inertness.

[0061] In addition, the present invention also provides a mechanical component for marine applications, the surface of which has the above-mentioned multi-layered high load-bearing, self-lubricating, wear-resistant and corrosion-resistant coating.

[0062] In some alternative implementations, mechanical components used in marine applications may, by way of example but not limitation, include bearing thrust discs, couplings, bushings, spherical bearings, and other similar components.

[0063] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0064] Example 1 This embodiment provides a multilayer high load-bearing self-lubricating wear-resistant coating, which includes a metal-ceramic support layer 100, a transition layer 200 and a DLC layer 300 sequentially disposed on the surface of a substrate (TC4 substrate).

[0065] The cermet support layer 100 comprises a WC hard phase and a NiMoCrFeCo binder phase in a mass ratio of 4:1, with a thickness of 150 μm and a surface roughness Ra of 0.1 μm. The transition layer 200 includes a Nb main transition layer 200 located away from the DLC layer 300 and an NbC transition layer 200 located close to the DLC layer 300. The transition layer 200 exhibits a columnar crystal morphology and has a total thickness of 0.2 μm. The DLC layer 300 has a thickness of 2 μm and is a high sp3 phase. 3The amorphous DLC film layer has a high content of [missing information]. The total thickness of the multilayer high load-bearing, self-lubricating, and wear-resistant coating is 152.2 μm. A mechanical interlocking mechanism is formed between the transition layer 200 and the DLC layer 300; the hardness of the transition layer 200 is less than that of the metal-ceramic support layer 100, and the hardness of the transition layer 200 is greater than that of the DLC layer 300.

[0066] The preparation method of the above-mentioned multilayer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating includes: S1: Degrease and remove oil from the substrate, and sandblast the spraying area.

[0067] The abrasive material (white corundum) used for sandblasting has a particle size of 54#, the sandblasting pressure is 0.3MPa, and the sandblasting distance is 150mm.

[0068] S2: Deposit a metal-ceramic support layer 100 on the substrate surface.

[0069] The substrate surface, after sandblasting and preheating to 150°C, was sprayed using a supersonic flame device. The preparation conditions included: the raw material was WC-NiMoCrFeCo powder (mass ratio 4:1); the carrier gas was 8 MPa, the oxygen flow rate was 850 L / min, the kerosene flow rate was 25 L / h, the powder feeding rate was 100 g / min, the spray distance was 150 mm, and the spray gun moving speed was 20 mm / s.

[0070] S3: Polish the metal-ceramic support layer 100.

[0071] The diamond grinding wheel rotates at 600 rpm. The diamond grinding wheel is then polished sequentially using 400-grit, 800-grit, 1000-grit, 1500-grit, and 3000-grit sandpaper. After polishing, the surface roughness Ra of the cermet support layer 100 is 0.1 μm. The thickness of the polished cermet support layer 100 is 150 μm.

[0072] S4: Ion beam cleaning is performed on the polished support layer.

[0073] Glow discharge cleaning: Open the Ar gas cylinder, the gas flow rate is 180 sccm, the vacuum degree is 1.5 Pa, the bias voltage is -800 V, and the glow discharge duration is 20 min.

[0074] Ion bombardment cleaning: inert gas flow rate of 120 sccm, vacuum degree of 0.5 Pa, bias voltage of -600 V, duration of 15 min.

[0075] S5: Deposit a transition layer 200 containing Nb on the cermet support layer 100.

[0076] The vacuum level of the deposition furnace was evacuated to 1×10⁻⁶. -3After Pa, Ar gas was introduced into the coating chamber at a flow rate of 120 sccm, and the vacuum degree was 0.5 Pa. The bias voltage was -100 V, the Nb target was turned on, and a transition layer of 200 was deposited on the surface of the support layer at a deposition power of 1600 W for a deposition time of 20 min.

[0077] S6: Prepare DLC layer 300 on transition layer 200.

[0078] Turn off the metal target, introduce inert gas into the coating chamber at a flow rate of 100 sccm and a vacuum of 0.2 Pa; and set the bias voltage to -100 V. Turn on the carbon target and deposit the DLC layer 300 on the surface of the transition layer 200 at a target current of 80 A and a deposition time of 60 min.

[0079] Example 2 This embodiment provides a multilayer high load-bearing self-lubricating wear-resistant coating, which includes a metal-ceramic support layer 100, a transition layer 200 and a DLC layer 300 sequentially disposed on the surface of a substrate (TC4 substrate).

[0080] The cermet support layer 100 comprises a WC hard phase and a NiMoCrFeCo binder phase in a mass ratio of 3:1. The thickness of the cermet support layer 100 is 50 μm, and its surface roughness Ra is 0.05 μm. The transition layer 200 includes a Nb main transition layer 200 located away from the DLC layer 300 and an NbC transition layer 200 located close to the DLC layer 300. The transition layer 200 exhibits a columnar crystal morphology, and its total thickness is 0.5 μm. The DLC layer 300 has a thickness of 200 nm and is a high sp3 phase. 3 The amorphous DLC film layer has a high content of [missing information]. The total thickness of the multilayer high load-bearing, self-lubricating, and wear-resistant coating is 50.7 μm. A mechanical interlocking mechanism is formed between the transition layer 200 and the DLC layer 300; the hardness of the transition layer 200 is less than that of the metal-ceramic support layer 100, and the hardness of the transition layer 200 is greater than that of the DLC layer 300.

[0081] The preparation method of the above-mentioned multilayer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating includes: S1: Degrease and remove oil from the substrate, and sandblast the spraying area.

[0082] The abrasive material (white corundum) used for sandblasting has a particle size of 54#, the sandblasting pressure is 0.2MPa, and the sandblasting distance is 50mm.

[0083] S2: Deposit a metal-ceramic support layer 100 on the substrate surface.

[0084] The substrate surface, after sandblasting and preheating to 150°C, was sprayed using a supersonic flame device. The preparation conditions included: the raw material was WC-NiMoCrFeCo powder; the carrier gas was 5MPa, the oxygen flow rate was 750L / min, the kerosene flow rate was 18L / h, the powder feeding rate was 50g / min, the spray distance was 100mm, and the spray gun moving speed was 10mm / s.

[0085] S3: Polish the metal-ceramic support layer 100.

[0086] The diamond grinding wheel rotates at 200 rpm, and the diamond grinding wheel is polished with sandpaper of 400 grit, 800 grit, 1000 grit, 1500 grit and 3000 grit in sequence.

[0087] S4: Ion beam cleaning is performed on the polished support layer.

[0088] Glow discharge cleaning: Open the Ar gas cylinder, the gas flow rate is 60 sccm, the vacuum degree is 1 Pa, the bias voltage is -1000 V, and the glow discharge duration is 10 min.

[0089] Ion bombardment cleaning: inert gas flow rate of 60 sccm, vacuum degree of 0.2 Pa, bias voltage of -800 V, duration of 10 min.

[0090] S5: Deposit a transition layer 200 containing Nb on the cermet support layer 100.

[0091] The vacuum level of the deposition furnace was evacuated to 3×10⁻⁶. -3 After Pa, Ar gas is introduced into the coating chamber at a flow rate of 50 sccm, and the vacuum degree is 0.1 Pa. The bias voltage is -50 V, the Nb target is turned on, and a transition layer of 200 is deposited on the surface of the support layer at a deposition power of 500 W and a deposition time of 60 min.

[0092] S6: Prepare DLC layer 300 on transition layer 200.

[0093] Turn off the metal target, introduce inert gas into the coating chamber at a flow rate of 60 sccm and a vacuum of 0.1 Pa; set the bias voltage to -30 V, turn on the carbon target, and deposit the DLC layer 300 on the surface of the transition layer 200 at a target current of 50 A and a deposition time of 100 min.

[0094] Example 3 This embodiment provides a multilayer high load-bearing self-lubricating wear-resistant coating, which includes a metal-ceramic support layer 100, a transition layer 200 and a DLC layer 300 sequentially disposed on the surface of a substrate (TC4 substrate).

[0095] The cermet support layer 100 comprises a WC hard phase and a NiMoCrFeCo binder phase in a mass ratio of 5:1. The thickness of the cermet support layer 100 is 300 μm, and its surface roughness Ra is 0.3 μm. The transition layer 200 includes a Nb main transition layer 200 located away from the DLC layer 300 and an NbC transition layer 200 located close to the DLC layer 300. The transition layer 200 exhibits a columnar crystal morphology, and its total thickness is approximately 0.2 μm. The DLC layer 300 has a thickness of 2 μm and is a high sp3 phase. 3 The amorphous DLC film layer has a high content of [missing information]. The total thickness of the multilayer high load-bearing, self-lubricating, and wear-resistant coating is 302.2 μm. A mechanical interlocking mechanism is formed between the transition layer 200 and the DLC layer 300; the hardness of the transition layer 200 is less than that of the metal-ceramic support layer 100, and the hardness of the transition layer 200 is greater than that of the DLC layer 300.

[0096] The preparation method of the above-mentioned multilayer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating includes: S1: Degrease and remove oil from the substrate, and sandblast the spraying area.

[0097] The abrasive material (brown corundum) used for sandblasting has a particle size of 60#, the sandblasting pressure is 0.6MPa, and the sandblasting distance is 350mm.

[0098] S2: Deposit a metal-ceramic support layer 100 on the substrate surface.

[0099] The substrate surface, after sandblasting and preheating to 150°C, was sprayed using a supersonic flame device. The preparation conditions included: the raw material was WC-NiMoCrFeCo powder; the carrier gas was 10MPa, the oxygen flow rate was 1000L / min, the kerosene flow rate was 32L / h, the powder feeding rate was 150g / min, the spray distance was 200mm, and the spray gun moving speed was 30mm / s.

[0100] S3: Polish the metal-ceramic support layer 100.

[0101] The diamond grinding wheel rotates at 1200 rpm, and the diamond grinding wheel is polished with sandpaper of 200 grit, 400 grit, 800 grit, 1000 grit, 1500 grit and 3000 grit in sequence.

[0102] S4: Ion beam cleaning is performed on the polished support layer.

[0103] Glow discharge cleaning: Open the Ar gas cylinder, the gas flow rate is 200 sccm, the vacuum degree is 3 Pa, the bias voltage is -600 V, and the glow discharge duration is 30 min.

[0104] Ion bombardment cleaning: inert gas flow rate of 160 sccm, vacuum degree of 0.8 Pa, bias voltage of -500 V, duration of 20 min.

[0105] S5: Deposit a transition layer 200 containing Nb on the cermet support layer 100.

[0106] The vacuum level of the deposition furnace was evacuated to 5×10⁻⁶. -3 After Pa, Ar gas is introduced into the coating chamber at a flow rate of 180 sccm, and the vacuum degree is 0.6 Pa. The bias voltage is -300 V, the Nb target is turned on, and a transition layer of 200 is deposited on the surface of the support layer at a deposition power of 2000 W for a deposition time of 10 min.

[0107] S6: Prepare DLC layer 300 on transition layer 200.

[0108] Turn off the metal target, introduce inert gas into the coating chamber at a flow rate of 180 sccm and a vacuum of 0.3 Pa; set the bias voltage to -200 V, turn on the carbon target, and deposit the DLC layer 300 on the surface of the transition layer 200 at a target current of 100 A and a deposition time of 30 min.

[0109] Comparative Example 1 This comparative example uses an untreated TC4 matrix.

[0110] Comparative Example 2 The difference between this comparative example and Example 1 is that a metal-ceramic support layer 100 is deposited only on the substrate surface.

[0111] Comparative Example 3 The difference between this comparative example and Example 1 is that no metal-ceramic support layer 100 was deposited on the substrate surface, that is, there were no steps S100 and S200.

[0112] Comparative Example 4 The difference between this comparative example and Example 1 is that no transition layer 200 containing Nb was deposited on the cermet support layer 100, i.e., step S5 was omitted.

[0113] The remaining steps and conditions are the same as in Example 1.

[0114] Comparative Example 5 The difference between this comparative example and Example 1 is that Nb is replaced with an equal amount of Ti.

[0115] Comparative Example 6 The difference between this comparative example and Example 1 is that Nb is replaced with an equal amount of Cr.

[0116] Comparative Example 7 The difference between this comparative example and Example 1 is that the mass ratio of the WC hard phase and the NiMoCrFeCo binder phase in the cermet support layer 100 is 2:1.

[0117] Comparative Example 8 The difference between this comparative example and Example 1 is that the surface roughness Ra of the metal-ceramic support layer 100 is 0.05 μm.

[0118] Comparative Example 9 The difference between this comparative example and Example 1 is that the surface roughness Ra of the metal-ceramic support layer 100 is 0.4 μm.

[0119] Comparative Example 10 The difference between this comparative example and Example 1 is that the total thickness of the transition layer 200 is 0.05 μm.

[0120] Comparative Example 11 The difference between this comparative example and Example 1 is that the total thickness of the transition layer 200 is 2.5 μm.

[0121] Comparative Example 12 The difference between this comparative example and Example 1 is that the spray distance is 50 mm during the preparation of the metal ceramic support layer 100.

[0122] Comparative Example 13 The difference between this comparative example and Example 1 is that the spray distance is 250 mm during the preparation of the metal ceramic support layer 100.

[0123] Comparative Example 14 The difference between this comparative example and Example 1 is that the vacuum degree is 0.05 Pa during the preparation of the transition layer 200.

[0124] Comparative Example 15 The difference between this comparative example and Example 1 is that the bias voltage is -40V during the preparation of the transition layer 200.

[0125] Comparative Example 16 The difference between this comparative example and Example 1 is that the bias voltage during the preparation of the transition layer 200 is -320V.

[0126] Comparative Example 17 The difference between this comparative example and Example 1 is that the bias voltage during the preparation of the DLC layer 300 is -320V.

[0127] Comparative Example 18 The difference between this comparative example and Example 1 is that the target current is 40A during the preparation of the DLC layer 300.

[0128] Comparative Example 19 The difference between this comparative example and Example 1 is that the target current is 120A during the fabrication of the DLC layer 300.

[0129] Experimental Example 1 Taking the multilayer high load-bearing self-lubricating wear-resistant coating prepared in Example 1 as an example, structural tests were performed on it.

[0130] The cross-sectional morphology of the multilayer high load-bearing self-lubricating wear-resistant coating obtained in Example 1 is as follows: Figure 2 As shown, by Figure 2 It can be seen that there are no obvious gaps or defects at the interfaces between each layer and the coating and the substrate surface, indicating that the bonding state between the interfaces of this multi-layer high load-bearing self-lubricating wear-resistant coating is good. Among them, there are no defects between the columnar crystal growth transition layer 200 and the DLC, and there is a mechanical interlocking effect. This interlocking structure causes the pinholes inside the transition layer 200 and the DLC film to be arranged alternately, thereby making the films tightly bonded together.

[0131] Furthermore, combined Figure 3 As can be seen, the transition layer 200 includes the Nb main transition layer 200 which is far from the DLC layer 300 and the NbC transition layer 200 which is close to the DLC layer 300.

[0132] Experimental Example 2 The coating products prepared in Example 1 and Comparative Examples 1-4 were subjected to performance tests.

[0133] (1) The coatings of Comparative Examples 3-6 and Example 1 were compared in terms of adhesion and crack resistance using the scratch test method. The results are as follows: Figure 4 As shown.

[0134] Depend on Figure 4 It can be seen that, due to material mismatch, the DLC coating of Comparative Example 3 cracked under a normal load of 2.5N, and the DLC coating of Comparative Example 4 cracked under a normal load of 10.4N. The coatings peeled off as the cracks propagated. In contrast, the multilayer high load-bearing self-lubricating wear-resistant coating of Example 1 only began to peel off when the normal load reached 17.3N. The higher bonding strength of the multilayer high load-bearing self-lubricating wear-resistant coating undoubtedly indicates that this composite coating is less prone to cracking and peeling under friction and wear under high loads. The fact that the peeling debris around the DLC film on top of the multilayer high load-bearing self-lubricating wear-resistant coating was significantly less than that of the other DLC coatings further illustrates this point.

[0135] The above results indicate that the improved adhesion strength can be attributed to the fact that when the DLC film is subjected to external force, the WC coating hardly undergoes plastic deformation, while the DLC coating is prone to interfacial shear stress due to deformation mismatch. The metal transition layer 200 can undergo plastic flow through slippage, absorb deformation energy, alleviate the peak value of interfacial shear stress, prevent the coating from peeling off from the substrate, and reduce interfacial thermal mismatch stress, thereby further improving the toughness and adhesion of the multilayer coating.

[0136] (2) A comparative schematic diagram of the mechanical properties (including nanohardness and elastic modulus, etc.) of the coating products of Example 1 and Comparative Examples 1-4 is shown below. Figures 5 to 7 As shown.

[0137] Depend on Figures 5 to 7 It can be seen that the hardness and elastic modulus of Examples 1 and Comparative Examples 2-4 are much higher than those of Comparative Example 1, indicating that the prepared metal-ceramic support layer 100 and DLC film can effectively improve the mechanical properties of the metal substrate. Although the hardness of the metal-ceramic support layer 100 in Comparative Example 2 is higher than that of the metal substrate in Comparative Example 1, it is lower than that of the DLC layer 300 in Comparative Examples 3-4 and Example 4. This indicates that the hardness of the metal-ceramic support layer 100 is in a moderate range between the softer metal substrate and the high-hardness DLC film. This gradient hardness matching can effectively alleviate the sudden change in interfacial stress between the substrate and the film, thereby making the transition of material properties from the metal substrate to the DLC film more stable.

[0138] The nanohardness of the coating products corresponding to Comparative Example 4 and Example 1 were 27.34 GPa and 31.74 GPa, respectively, and the elastic modulus were 325.84 GPa and 378.17 GPa, respectively. The results show that compared with the DLC coating without transition layer 200 in Comparative Example 4, the nanohardness and elastic modulus of the multilayer high load-bearing self-lubricating wear-resistant coating with transition layer 200 in Example 1 are improved, indicating that transition layer 200 can effectively reduce the defect density of DLC layer 300.

[0139] Nanoscale hardness is not the only factor affecting wear resistance; H / E and H 3 / E 2 It is also an effective method for predicting wear resistance, where H and E correspond to hardness and elastic modulus, respectively; H / E and H 3 / E 2 These represent the coating's resistance to plastic deformation and its impact resistance, respectively. Generally, coating characteristic values ​​are proportional to wear resistance and crack resistance. The H value of the multilayer high-load-bearing self-lubricating wear-resistant coating in Example 1... 3 / E 2 The value is higher than that of the DLC coating in Comparative Examples 3-4, indicating that the transition layer 200 can effectively improve the toughness and wear resistance of the composite coating.

[0140] (3) The friction coefficient and wear rate of the coating products of Comparative Examples 3-4 and Example 1 were studied in an artificial seawater environment using a needle-disc friction testing machine. The results are as follows: Figure 8 As shown in the figure. The friction pair consists of Al2O3 balls with a diameter of 5 mm and a load of 40 N.

[0141] Depend on Figure 8 As can be seen in (a), after the initial running-in stage, the S values ​​of both composite coatings gradually decreased from approximately 0.26 at the beginning of friction to approximately 0.06, demonstrating the good lubricity of the DLC film. This is because, as the friction process progresses, due to the accumulation of contact stress and the increase in local temperature, some SP... 3 Carbon bonds may break or rearrange, transforming into sp bonds. 2 Bonds are formed to create graphite friction layers, which reduce frictional resistance through interlayer sliding. Ultimately, the coefficient of friction of the DLC layer 300 in Comparative Example 3 and Example 1 is stabilized at around 0.06, exhibiting excellent anti-friction properties.

[0142] Figure 8 As can be seen in Figure (b), under a reciprocating friction and wear test with a load of 40 N in an artificial seawater environment, the wear rate of the coating of Comparative Example 4 was 12.46 × 10⁻⁶ after only 3000 friction cycles in Comparative Example 3. -7 mm 3 ·N -1 ·m -1 The wear rate of the coating in Example 1 was 7.12 × 10⁻⁶. -7 mm 3 ·N -1 ·m -1 This indicates that the wear mark width and depth of the multilayer high load-bearing self-lubricating wear-resistant coating of Example 1 are both smaller than those of Comparative Example 3.

[0143] Combined Figure 9 The SEM-EDS characterization results showed that the DLC film of Comparative Example 4 was completely worn through in the center, with only the two sides remaining, while the DLC film of Example 1 remained intact, demonstrating the effect of Nb on improving wear resistance. Figure 9 (a1) is an enlarged view of the boxed area in (a), and (a2) is the EDS result image of the boxed area in (a); (b1) is an enlarged view of the boxed area in (b), and (b2) is the EDS result image of the boxed area in (b).

[0144] (4) Figure 10The figures show the polarization curves of the coating products in Example 1 and Comparative Example 2, where the horizontal axis represents the potential (relative to a saturated calomel electrode) and the vertical axis represents the current density, which has been logarithmically calculated. The test environment was artificial seawater solution, and the test range was -0.5V to 1.0V relative to the open circuit. The corrosion resistance data of each coating were obtained by calculating the corrosion current density.

[0145] Compared to the coating in Comparative Example 2, the current density of the multilayer composite coatings in Comparative Example 4 and Example 1 decreased by an order of magnitude. This indicates that the DLC film provides good corrosion protection for the underlying WC-Ni-based coating and the substrate. Furthermore, the composite coating in Example 1, which incorporates the transition layer 200, exhibits the best corrosion resistance, with a corrosion current density of 1.69 × 10⁻⁶. -8 A / cm 2 .

[0146] Experimental Example 3 Based on the test methods of Experimental Example 1 and Experimental Example 2, the performance results of the coating products obtained in Examples 1-3 and Comparative Examples 1-19 are summarized in Table 1.

[0147] Table 1 Performance Comparison Table

[0148] As can be seen from Table 1, the multilayer high load-bearing self-lubricating and wear-resistant coating prepared in the embodiments of the present invention has superior bonding strength, load-bearing capacity, corrosion resistance and protective durability, effectively achieving a synergistic improvement in the coating's self-lubricating and wear-resistant properties.

[0149] In summary, this invention significantly improves the mechanical, tribological, and corrosion resistance of metal substrates by depositing an Nb-DLC composite film on the surface of an oxide ceramic coating and a WC-based hard coating, and by designing a transition layer 200 with specific composition and structure. Compared to WC-DLC coatings without the transition layer 200, the composite coating incorporating Nb not only achieves breakthroughs in single properties but also exhibits superior comprehensive performance under various complex working conditions and environments. This fully demonstrates that the composite coating in this invention can form a good composite structure with coatings on different substrates, exerting a synergistic effect and optimizing the overall performance of the coating. This provides a more reliable technical solution for the application of coating materials in fields such as machinery manufacturing and marine engineering, possessing significant innovation and practical value.

[0150] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A multi-layered, high-load-bearing, self-lubricating, wear-resistant, and corrosion-resistant coating, characterized in that, It includes a metal-ceramic support layer, a transition layer, and a DLC layer sequentially disposed on the surface of the substrate; The transition layer includes a Nb main transition layer away from the DLC layer and an NbC transition layer close to the DLC layer; the transition layer has a columnar crystal morphology; the total thickness of the transition layer is 0.1 μm to 2 μm. The metal-ceramic support layer is a WC-based hard alloy coating; the metal-ceramic support layer includes a WC hard phase and a NiMoCrFeCo binder phase in a mass ratio of 3:1 to 5:1; a mechanical interlocking mechanism is formed between the transition layer and the DLC layer.

2. The multi-layer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating according to claim 1, characterized in that, The total thickness of the transition layer is 0.1 μm to 1 μm.

3. The multi-layer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating according to claim 1, characterized in that, The thickness of the metal-ceramic support layer is 50μm~300μm; The surface roughness Ra of the metal-ceramic support layer is 0.05 μm to 0.3 μm; The hardness of the metal-ceramic support layer is greater than that of the substrate, and the hardness of the metal-ceramic support layer is less than that of the DLC layer.

4. The multi-layer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating according to claim 1, characterized in that, The thickness of the DLC layer is 200nm~3μm; The DLC layer is of high sp 3 Amorphous DLC film with high content.

5. The multi-layer high load-bearing self-lubricating wear-resistant and corrosion-resistant coating according to claim 1, characterized in that, The total thickness of the multi-layer high load-bearing self-lubricating wear-resistant coating is 50.3μm~305μm.

6. A method for preparing a multilayer high-load-bearing, self-lubricating, wear-resistant and corrosion-resistant coating as described in any one of claims 1 to 5, characterized in that, Includes the following steps: The metal-ceramic support layer, the transition layer, and the DLC layer are sequentially disposed on the surface of the substrate.

7. The preparation method according to claim 6, characterized in that, The metal-ceramic support layer was prepared by supersonic flame spraying. The preparation conditions of the metal-ceramic support layer include: carrier gas of 5MPa~10MPa, oxygen flow rate of 750L / min~1000L / min, kerosene flow rate of 18L / h~32L / h, powder feeding rate of 50g / min~150g / min, spray distance of 100mm~200mm, and spray gun moving speed of 10mm / s~30mm / s.

8. The preparation method according to claim 6, characterized in that, The transition layer was prepared by magnetron sputtering. The preparation of the transition layer includes: evacuating the deposition furnace to a vacuum level of 1×10⁻⁶. -3 Pa~5×10 -3 Pa, inert gas is introduced into the coating chamber at a flow rate of 50 sccm to 180 sccm and a vacuum degree of 0.1 Pa to 0.6 Pa; the bias voltage is -50 V to -300 V, the metal target is turned on, and a transition layer is deposited on the surface of the metal-ceramic support layer at a deposition power of 500 W to 2000 W and a deposition time of 10 min to 60 min.

9. The preparation method according to claim 8, characterized in that, The DLC layer was prepared by arc ion plating. The preparation of the DLC layer includes: turning off the metal target, introducing an inert gas into the coating chamber at a flow rate of 60 sccm to 180 sccm and a vacuum of 0.1 Pa to 0.3 Pa; a bias voltage of -30 V to -200 V; turning on the carbon target; depositing the DLC layer on the surface of the transition layer at a target current of 50 A to 100 A and a deposition time of 30 min to 100 min.

10. The preparation method according to claim 6, characterized in that, Before preparing the transition layer, the process also includes grinding, polishing, and cleaning the metal-ceramic support layer; The polishing process includes polishing with 200-3000 mesh sandpaper at 200-1200 rpm until the surface roughness of the metal-ceramic support layer reaches Ra of 0.05 μm-0.3 μm. The cleaning process includes sequential glow discharge cleaning and ion bombardment cleaning. The glow discharge cleaning process involves introducing inert gas into the coating chamber at a flow rate of 60 sccm to 200 sccm, a vacuum level of 1.0 Pa to 3 Pa, a bias voltage of -1000 V to -600 V, and a glow discharge duration of 10 min to 30 min. The ion bombardment cleaning process involves an inert gas flow rate of 60 sccm to 160 sccm, a vacuum level of 0.2 Pa to 0.8 Pa, a bias voltage of -800 V to -500 V, and a duration of 10 min to 20 min.

11. A mechanical component for marine applications, characterized in that, The surface of the mechanical components used in marine applications has a multi-layered, high-load-bearing, self-lubricating, wear-resistant coating as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Super wear-resistant and corrosion-resistant gradient composite coating and preparation method thereof

    CN118256864A

  • Self-lubricating anti-corrosion wear-resistant coating and preparation method thereof

    CN120174378A

  • High adhesion carbon film forming material and its production

    JP2000087218A