An underwater anti-dispersion composite material and a preparation method thereof

By controlling the synergistic effect of polymer bridging agents and components such as sulfoaluminate cement, the problems of insufficient anti-dispersion properties, interfacial bond strength, and toughness of underwater concrete repair materials are solved, achieving efficient repair and reinforcement in underwater environments.

CN122167112BActive Publication Date: 2026-11-24QINGDAO UNIV OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610199408.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-02-11
Publication Date
2026-11-24
Estimated Expiration
2046-02-11

AI Technical Summary

Technical Problem

Existing underwater concrete repair materials are deficient in terms of anti-dispersion properties, interfacial bond strength, material toughness, and network synergy, making it difficult to effectively bond and toughen in underwater environments, and they also have poor durability.

Method used

A controllable synthetic polymer bridging agent was used to prepare an amphiphilic block copolymer via a three-step polymerization method. Combined with sulfoaluminate cement, network reinforcing agent, and charge regulator, a multifunctional composite material was constructed to achieve the synergistic effect of strong chemical anchoring, steric hindrance, and flexible network.

Benefits of technology

It significantly improves the anti-dispersion properties, bond strength, and toughness of underwater concrete, enhances the material's durability and impermeability, and is suitable for efficient repair and reinforcement in underwater construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122167112B_ABST
    Figure CN122167112B_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of underwater engineering repair materials, and discloses an underwater anti-dispersion composite material and its preparation method. Its components include: 2-5 parts of a controllable synthetic polymer bridging agent, 0.8-1.5 parts of a network reinforcing agent, 50-65 parts of sulfoaluminate cement, 40-55 parts of fine sand, 10-18 parts of acrylamide monomer, 0.3-0.6 parts of ammonium persulfate initiator, 0.15-0.35 parts of accelerator, 0.3-0.6 parts of charge regulator, and 18-28 parts of water. The underwater anti-dispersion composite material of this invention has an underwater anti-dispersion loss rate of <5%, a bond strength to wet substrate >3.5 MPa, and significantly improved toughness, making it suitable for the repair and reinforcement of concrete structures in underwater environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of underwater engineering repair materials technology, specifically relating to an underwater anti-dispersion composite material and its preparation method, which is suitable for the repair and reinforcement of concrete structures in underwater environments (such as oceans, freshwater, and damp tunnels). Background Technology

[0002] The repair and reinforcement of underwater concrete structures is a major technical challenge in the field of civil engineering. Compared with the terrestrial environment, underwater construction faces a series of difficulties, including water erosion, material component dispersion and loss, harsh bonding environment at the interface between new and old concrete (wet or even water-bearing substrates), and demanding curing conditions. Traditional underwater non-dispersible concrete (NDC) mainly relies on high-viscosity and water-resistant admixtures (such as cellulose ethers and polyacrylamide) to improve the cohesiveness of the paste. Although this reduces dispersion loss to some extent, it generally suffers from the following bottlenecks: 1. Weak interfacial adhesion: The adhesion between traditional materials and old underwater concrete substrates mainly relies on physical adsorption and limited mechanical interlocking, lacking strong chemical bonding, resulting in low bonding strength (usually below 1.5MPa). This easily leads to the formation of a weak layer at the interface, becoming a hidden danger for long-term service.

[0003] 2. Insufficient material toughness: High-molecular-weight thickeners introduced to meet the requirements of anti-dispersion often lead to increased material brittleness, poor crack resistance, and difficulty in adapting to stress caused by dynamic loads and temperature changes, making the repair layer prone to cracking.

[0004] 3. Loose network structure: The organic thickener and inorganic cement hydration products are mostly physically blended or weakly interacted, lacking effective chemical bridging and network interpenetration, which easily leads to phase separation, resulting in uneven macroscopic properties of the material and poor durability (such as impermeability and corrosion resistance).

[0005] In recent years, biomimetic adhesive materials (such as catechol-based mussel adhesive proteins) have provided new ideas for developing strong underwater adhesive materials: catechol groups can form strong coordination bonds with various metal ions underwater. However, how to effectively combine such biomimetic groups with cement-based materials while simultaneously addressing multiple requirements such as anti-dispersion and toughening remains a technical challenge. Simple physical incorporation of biomimetic molecules often has limited effects and may interfere with cement hydration.

[0006] On the other hand, introducing in-situ polymeric monomers (such as acrylamide) into polymer-cement composites is an effective way to improve toughness. However, the compatibility and synergy between the polymeric network and the cement hydration network are poor, especially in the construction kinetics in underwater environments, where fine control is lacking. If polymerization is too fast, it may hinder cement hydration; if it is too slow, it will lead to insufficient early strength of the material. In addition, if the flexible network formed by acrylamide polymerization cannot form a strong bond with the rigid inorganic phase and interface, its toughening effect will be greatly reduced, and it may fail due to interfacial debonding.

[0007] Therefore, there is an urgent need to develop a new type of underwater repair composite material that can be constructed from molecular design and through controllable synthesis technology to create a multifunctional polymer bridging agent, thereby achieving an integrated improvement in underwater anti-dispersion, strong interfacial adhesion, high toughness and excellent durability. Summary of the Invention

[0008] The purpose of this invention is to provide an underwater anti-dispersion composite material and its preparation method, so as to help overcome the shortcomings of existing underwater repair materials in terms of anti-dispersion, interfacial bonding strength, material toughness or network synergy.

[0009] To achieve the above objectives, the present invention provides the following technical solution: An underwater anti-dispersion composite material, by weight, comprises the following components: 2-5 parts of a controllable synthetic polymer bridging agent, 0.8-1.5 parts of a network reinforcing agent, 50-65 parts of sulfoaluminate cement, 40-55 parts of fine sand, 10-18 parts of acrylamide monomer, 0.3-0.6 parts of ammonium persulfate initiator, 0.15-0.35 parts of accelerator, 0.3-0.6 parts of charge regulator, and 18-28 parts of water; The controllable synthetic polymer bridging agent is an amphiphilic block copolymer prepared by a sequentially controllable three-step polymerization method, and its molecular structure is as follows: ; In this molecule, the R1 group at one end is a catechol anchoring group, the S2 segment in the middle is a hydrophilic segment of polyethylene oxide, and the S3 segment at the other end is a hydrophobic segment of polycaprolactone; n is an integer between 40 and 100, m is an integer between 10 and 60, and the mass ratio of the hydrophobic segment of polycaprolactone to the hydrophilic segment of polyethylene oxide is (0.8~1.5):1.

[0010] Furthermore, the three-step polymerization method for the controllable synthesis of the polymer bridging agent includes the following preparation steps: S1. Terminal functionalization: Starting with 3,4-dihydroxybenzoic acid, an active bromoalkyl terminus is introduced through esterification to obtain a catechol functionalization initiator. S2. Hydrophilic segment controlled polymerization: Using the product obtained in step S1 as an initiator, in the presence of an alkaline catalyst, the ring-opening polymerization of ethylene oxide monomer is initiated. The polymerization temperature is 80~110℃ and the reaction time is 6~12h to obtain catechol-polyethylene oxide intermediate. S3. Controllable chain extension of hydrophobic segments: Using the intermediate obtained in step S2 as a macromolecular initiator, under the action of an organometallic catalyst, the ε-caprolactone monomer is initiated to undergo ring-opening polymerization at a polymerization temperature of 100~130℃ and a reaction time of 8~16h to obtain catechol-polyethylene oxide-polycaprolactone copolymer. S4. Purification and characterization: The product obtained in step S3 is precipitated, washed, and vacuum dried to obtain the controllable synthetic polymer bridging agent, and characterized by 1H NMR spectroscopy.

[0011] Further, in step S1, the molar ratio of 3,4-dihydroxybenzoic acid to bromoalkyl alcohol is 1:(1.1~1.3); the molar ratio of the dehydrating agent N,N'-dicyclohexylcarbodiimide used in the esterification reaction to 3,4-dihydroxybenzoic acid is (1.0~1.2):1; and the amount of the catalyst 4-dimethylaminopyridine used in the esterification reaction is 5%~15% of the molar amount of 3,4-dihydroxybenzoic acid.

[0012] Furthermore, in step S2, the molar ratio of the initiator to the ethylene oxide monomer is 1:(40~100), the amount of alkaline catalyst is 1%~5% of the mass of the initiator, and the alkaline catalyst is sodium methoxide or potassium tert-butoxide.

[0013] Furthermore, in step S3, the molar ratio of the macromolecular initiator to the ε-caprolactone monomer is 1:(10~60), the amount of organometallic catalyst is 0.05%~0.2% of the total mass of the monomer, and the organometallic catalyst is stannous octoate or aluminum triisopropoxy.

[0014] Preferably, the network reinforcing agent is sodium carboxymethyl cellulose with a degree of substitution of 0.6 to 0.9.

[0015] Preferably, the accelerator is a compound system of sodium bisulfite and triethanolamine, with a mass ratio of sodium bisulfite to triethanolamine of (2~4):1.

[0016] Preferably, the charge regulator is a dimethyl diallyl ammonium chloride-acrylamide copolymer with a cationic charge density of 3.5~5.0 meq / g.

[0017] Preferably, the specific surface area of ​​sulfoaluminate cement is 380~450 m². 2 / kg, initial setting time not earlier than 15 minutes; fine sand is quartz sand with a fineness modulus of 1.8~2.2 and a mud content of less than 0.5%.

[0018] The above-mentioned method for preparing underwater anti-dispersion composite materials includes the following steps: P1. Preparation of premix: Dissolve the controllable synthetic polymer bridging agent in 60% of the formulation water, stir until completely dissolved, add the network reinforcing agent, and continue stirring to form a uniform and viscous premix; P2, Inorganic phase composite: The premixed liquid obtained in step P1 is added to sulfoaluminate cement, fine sand and charge regulator, and mechanically stirred to mix evenly to obtain an inorganic reinforced slurry matrix; P3. Preparation of polymerization initiator solution: Dissolve the acrylamide monomer, ammonium persulfate initiator and accelerator in the remaining 40% of the formulation water, stir evenly to form the acrylamide in-situ polymerization initiator solution; P4. In-situ composite and casting: The polymerization initiator liquid obtained in step P3 is added to the slurry matrix obtained in step P2 and stirred for 30-60 seconds to obtain the composite material slurry, which is then cast underwater.

[0019] Beneficial effects: 1. Excellent underwater anti-dispersion performance: This invention constructs a triple synergistic anti-dispersion mechanism of "steric hindrance, electrostatic stability, and viscosity encapsulation" by introducing a controllable synthetic polymer bridging agent with a clearly defined amphiphilic block structure, along with a charge regulator and a network enhancer. The long chains of polyethylene oxide (PEO) in the controllable synthetic polymer bridging agent fully extend in the aqueous phase, forming a thick hydration layer on the surface of solid particles, generating a strong steric hindrance effect that fundamentally inhibits particle approach and loss. Simultaneously, the high-cationic-density charge regulator (dimethyl diallyl ammonium chloride-acrylamide copolymer, i.e., DMDAAC-AM copolymer) adsorbs onto the surface of cement particles, increasing the stability of the slurry structure through charge neutralization and bridging flocculation. The network enhancer (sodium carboxymethyl cellulose, i.e., CMC) significantly increases the viscosity of the aqueous phase, providing physical encapsulation. This triple synergistic effect allows the anti-dispersion loss rate of the material during underwater casting to be controlled below 5%, far superior to traditional underwater non-dispersible concrete (typically with a loss rate >10%), ensuring the molding quality and material utilization rate of underwater construction.

[0020] 2. Superior adhesion to underwater wet substrates: The core innovation of this invention lies in the controlled synthesis of a catechol group, inspired by mussel adhesive proteins, introduced into one end of a polymer bridging agent molecule. This group can react underwater with the hydration products of inorganic cementitious materials (such as Ca). 2+ Al 3+The material forms high-strength, hydrolysis-resistant multiple metal chelate bonds with metal oxides / hydroxides on the surface of the old concrete substrate. This molecular-level chemical anchoring overcomes the limitations of traditional bonding, which relies on physical adsorption and limited mechanical interlocking, achieving direct chemical bonding across the interface between the old and new layers. Combined with the mechanical interlocking formed by the excellent permeability of the material slurry (due to its superior anti-dispersion properties and suitable rheological properties), and the interpenetration and interweaving of the polymer network and inorganic phase in the interface region, the bonding strength between this material and the underwater wet substrate is consistently higher than 3.5 MPa, solving the core problem of weak interfaces in underwater repair.

[0021] 3. Significantly improved toughness and crack resistance: This invention constructs a unique composite reinforcement and toughening system of "rigid inorganic network - flexible organic network - reversible physical crosslinking points". The sulfoaluminate cement hydration network provides stiffness and early strength; the flexible long-chain polyacrylamide (PAM) network formed by in-situ polymerization of acrylamide is tightly bound to the inorganic phase through multiple hydrogen bonds (with CMC and cement hydration products), and dissipates energy under stress through segment slip and reversible hydrogen bond breakage. More importantly, the hydrophobic polycaprolactone (PCL) segments at the ends of the controllably synthesized polymer bridging agent form nanocrystalline microregions after material curing, serving as highly efficient physical crosslinking points and energy dissipation centers. When the material is loaded, these crystalline microregions can absorb a large amount of energy through destruction and recombination. Tests show that the flexural strength (reflecting toughness) of this material can be increased by more than 180% compared to ordinary underwater concrete, and the increased toughness significantly enhances impact resistance and crack propagation inhibition.

[0022] 4. Excellent impermeability and durability: The underwater anti-dispersion composite material of this invention forms a highly dense and uniform organic-inorganic network structure through the mediation of a controllably synthesized polymer bridging agent and the integration of a network reinforcing agent. Acrylamide polymer gel and cement hydration products synergistically fill the capillary pores, and polycaprolactone (PCL) segments themselves readily form nanocrystalline microregions. The presence of these nanocrystalline microregions further refines the pore structure, making most pores closed micropores. This dense structure effectively blocks moisture and corrosive ions (such as Cl-). - SO4 2- The material exhibits excellent impermeability (low chloride ion diffusion coefficient) and good resistance to sulfate and seawater corrosion, making it suitable for harsh marine and other corrosive underwater environments. Simultaneously, the strong chelating effect of the catechol groups with metal ions stabilizes the interface and reduces the porosity of the interfacial transition zone. Therefore, this material demonstrates excellent impermeability (low chloride ion diffusion coefficient) and good resistance to sulfate and seawater corrosion, making it suitable for harsh marine and other corrosive underwater environments.

[0023] 5. Excellent construction performance and wide applicability: The preparation method of the underwater anti-dispersion composite material of this invention is simple and the process is controllable. Through a stepwise mixing process, the full dispersion and reactivity of each component are ensured. The final slurry exhibits good fluidity and thixotropy, facilitating underwater casting and construction while resisting water erosion. The material system uses water as the dispersion medium, making it environmentally friendly and safe. The early-strength characteristics of sulfoaluminate cement are matched with the rapid polymerization of acrylamide, enabling the material to quickly build strength underwater, meeting the engineering requirements for rapid repair. This material is suitable for the repair, reinforcement, and protection of various underwater concrete structures such as reservoir dams, cross-sea bridge piers, subsea tunnels, and docks and ports. Attached Figure Description

[0024] The accompanying drawings, which form part of this specification, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. Wherein: Figure 1 The 1H NMR spectrum of the controllable synthetic polymer bridging agent prepared in Example 1 of this invention; wherein ①: catechol functionalization initiator; ②: catechol-polyethylene oxide intermediate; ③: catechol-polyethylene oxide-polycaprolactone amphiphilic block copolymer (controllable synthetic polymer bridging agent).

[0025] Figure 2 SEM image of the microstructure of the underwater anti-dispersion composite material prepared in Example 1 of this invention.

[0026] Figure 3 The image shows the microstructure of the underwater anti-dispersion composite material prepared in Comparative Example 1 of this invention, as shown in the SEM image. Detailed Implementation

[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention are within the scope of protection of the present invention.

[0028] This invention provides an underwater anti-dispersion composite material. Its core lies in constructing a multifunctional polymer bridging agent that integrates "anchoring-bridging-toughening" through precise molecular structure design and controllable synthesis. The synchronous formation and interpenetration of the sulfoaluminate cement hydration network and the acrylamide in-situ polymerization network mediated by the controllable synthesized polymer bridging agent ultimately yields an underwater repair material with excellent performance.

[0029] An underwater anti-dispersion composite material, by weight, comprises the following components: 2-5 parts (e.g., 2, 3, 4, or 5 parts) of a controllable synthetic polymer bridging agent; 0.8-1.5 parts (e.g., 0.8, 1, 1.2, 1.4, or 1.5 parts) of a network reinforcing agent; 50-65 parts (e.g., 50, 55, 60, or 65 parts) of sulfoaluminate cement; 40-55 parts (e.g., 40, 45, 50, or 55 parts) of fine sand; and 10-18 parts (e.g., 10...). The composition includes: 12, 14, 16, or 18 parts of ammonium persulfate initiator (e.g., 0.3, 0.4, 0.5, or 0.6 parts), 0.15 to 0.35 parts of accelerator (e.g., 0.15, 0.2, 0.25, 0.3, or 0.35 parts), 0.3 to 0.6 parts of charge regulator (e.g., 0.3, 0.4, 0.5, or 0.6 parts), and 18 to 28 parts of water (e.g., 18, 20, 22, 24, 26, or 28 parts). The controllable synthetic polymer bridging agent is the core innovative component of this invention. It is an amphiphilic block copolymer prepared by a sequentially controllable three-step polymerization method, and its molecular structure is as follows: ;

[0030] The R1 group at one end of the molecule is a catechol anchoring group, derived from 3,4-dihydroxybenzoic acid. This group can chelate with Ca in the hydration products of sulfoaluminate cement. 2+ Al 3+ Plasma, along with metal oxides / hydroxides on the surface of the underwater old concrete substrate, forms high-strength, hydrolysis-resistant coordination bonds, achieving molecular-level chemical anchoring.

[0031] The S2 segment in the middle is a hydrophilic segment of polyethylene oxide with a number average molecular weight of 2000~4000. This segment has extremely strong hydration capacity and can form a thick hydration protective layer on the surface of cement particles and aggregates, generating a strong steric hindrance effect. This effectively prevents solid particles from approaching, agglomerating, and being lost under the scouring of water flow, which is the key to ensuring the underwater anti-dispersion properties of the material.

[0032] The S3 segment at the other end of the molecule is a hydrophobic segment of polycaprolactone: the mass ratio of the hydrophobic polycaprolactone segment to the hydrophilic polyoxyethylene segment is (0.8~1.5):1 (e.g., 0.8:1, 1:1, 1.2:1, 1.4:1, or 1.5:1). During the curing and drying process of the composite material, the hydrophobic polycaprolactone segment can crystallize, forming nano / micron-scale physically cross-linked microregions. These crystalline microregions, acting as "reversible cross-linking points," effectively lock the polymer chains. Under external force, the destruction and recombination of these crystalline regions dissipate a large amount of energy, significantly improving the material's toughness and crack resistance.

[0033] In a preferred embodiment of the underwater anti-dispersion composite material of the present invention, the controllable synthetic polymer bridging agent is prepared by a sequentially controllable three-step polymerization method, including the following steps: S1. Terminal Functionalization: Using 3,4-dihydroxybenzoic acid as the starting material, an active bromoalkyl terminus is introduced via esterification to obtain a catechol functionalization initiator; wherein the molar ratio of 3,4-dihydroxybenzoic acid to bromoalkyl alcohol is 1:(1.1~1.3) (e.g., 1:1.1, 1:1.15, 1:1.2, 1:1.25 or 1:1.3); the esterification reaction is carried out at 0~5℃ for 2~4h (e.g., 2h, 3h or 4h), followed by raising the temperature to room temperature (25℃) and continuing the reaction for 12~1h. 8 h (e.g., 12 h, 14 h, 16 h, or 18 h); the molar ratio of the dehydrating agent DCC (N,N'-dicyclohexylcarbodiimide) to 3,4-dihydroxybenzoic acid used in the esterification reaction is (1.0~1.2):1 (e.g., 1:1, 1.25:1, 1.5:1, 1.75:1, or 1.2:1); the amount of the catalyst DMAP (4-dimethylaminopyridine) used in the esterification reaction is 5%~15% (e.g., 5%, 10%, or 15%) of the molar amount of 3,4-dihydroxybenzoic acid. The chemical reaction principle involved in this step is represented by the following structural formula: ; ; in It is undecylbromoethanol.

[0034] S2. Controlled polymerization of hydrophilic segments: Using the product obtained in step S1 as an initiator, in the presence of an alkaline catalyst (such as sodium methoxide or potassium tert-butoxide), ring-opening polymerization of ethylene oxide monomer is initiated at 80-110°C (e.g., 80°C, 90°C, 100°C, or 110°C) for 6-12 hours (e.g., 6 hours, 8 hours, 10 hours, or 12 hours) to obtain a catechol-polyethylene oxide intermediate; wherein, the molar ratio of the product obtained in step S1 (catechol functionalized initiator) to ethylene oxide monomer is 1:(40-100) (e.g., 1:40, 1:60, 1:80, or 1:100) to control the degree of polymerization (n) of the hydrophilic segments of polyethylene oxide between 40 and 100; the amount of alkaline catalyst is 1%-5% (e.g., 1%, 2%, 3%, 4%, or 5%) of the initiator mass.

[0035] The chemical reaction principle involved in this step is represented by the following structural formula: ; ; in It is ethylene oxide.

[0036] S3. Controllable chain extension of hydrophobic segments: Using the intermediate obtained in step S2 as a macromolecular initiator, under the action of an organometallic catalyst (such as stannous octoate or aluminum triisopropoxy), the ε-caprolactone monomer is initiated to undergo ring-opening polymerization at 100~130℃ (e.g., 100℃, 110℃, 120℃ or 130℃) for 8~16h (e.g., 8h, 10h, 12h, 14h or 16h) to obtain a catechol-polyethylene oxide-polycaprolactone copolymer with an amphiphilic block structure; wherein, the intermediate (macromolecular initiator) obtained in step S2 and the ε-caprolactone monomer... The molar ratio of the monomers is 1:(10~60) (e.g., 1:10, 1:30, 1:50 or 1:60) to control the degree of polymerization (m) of the hydrophobic segments of polycaprolactone between 10 and 60, and to ensure that the mass ratio of hydrophobic segments to hydrophilic segments meets the design requirement of (0.8~1.5):1 (e.g., 0.8:1, 1.0:1, 1.2:1, 1.4:1 or 1.5:1); the amount of organometallic catalyst is 0.05%~0.2% of the total mass of monomers (e.g., 0.05%, 0.1%, 0.15% or 0.2%).

[0037] The chemical reaction principle involved in this step is represented by the following structural formula: ; ; in It is ε-caprolactone.

[0038] S4. Purification: The product obtained in step S3 is precipitated, washed, and vacuum dried to obtain the controllable synthetic polymer bridging agent (if necessary, it can be characterized by nuclear magnetic resonance hydrogen spectroscopy to confirm its molecular structure and block ratio).

[0039] In a preferred embodiment of the underwater anti-dispersion composite material of the present invention, acrylamide monomer, ammonium persulfate initiator, and accelerator constitute an underwater in-situ rapid polymerization system. The accelerator is a compound system of sodium bisulfite and triethanolamine, with a mass ratio of sodium bisulfite to triethanolamine of (2-4):1 (e.g., 2:1, 3:1, or 4:1), preferably 3:1. This redox system can rapidly initiate acrylamide polymerization at room temperature or even lower water temperatures, forming a through-cell polyacrylamide flexible network.

[0040] In a preferred embodiment of the underwater anti-dispersion composite material of the present invention, the network reinforcing agent is sodium carboxymethyl cellulose (CMC) with a degree of substitution of 0.6 to 0.9. If the degree of substitution is below 0.6, its water solubility and thickening ability are insufficient, making it difficult to guarantee anti-dispersion properties; if the degree of substitution is above 0.9, excessive anionic groups will significantly delay the hydration of sulfoaluminate cement, leading to insufficient early strength, and it is prone to excessive reaction with cationic components, affecting fluidity. CMC can dissolve in water to form a high-viscosity solution, further increasing the viscosity of the slurry and assisting in anti-dispersion. More importantly, the carboxyl and hydroxyl groups on its molecular chain can form a multiple hydrogen bond network with the amide groups on the polyacrylamide chain and the surface of cement hydration products, acting as a "molecular glue," enhancing the interfacial bonding between the organic network and the inorganic phase, and improving the overall material integrity.

[0041] In a preferred embodiment of the underwater anti-dispersion composite material of the present invention, the charge regulator is a dimethyl diallyl ammonium chloride-acrylamide copolymer with a cationic charge density of 3.5~5.0 meq / g (e.g., 3.5 meq / g, 4.0 meq / g, 4.5 meq / g, or 5.0 meq / g). If the cationic charge density is lower than 3.5 meq / g, it is insufficient to produce effective charge neutralization and bridging flocculation; if it is higher than 5.0 meq / g, it is easy to cause the surface charge reversal of cement particles and redispersion, or to form polyelectrolyte complex precipitation with CMC, which seriously impairs the rheological properties of the slurry and the casting quality. The role of the charge regulator is to adsorb on the surface of negatively charged cement particles, and through charge neutralization and bridging flocculation, further increase the stability of the slurry, and synergize with the steric hindrance effect of the controllable synthetic polymer bridging agent to ensure excellent underwater anti-dispersion (anti-dispersion loss rate <5%).

[0042] In a preferred embodiment of the underwater anti-dispersion composite material of the present invention, the sulfoaluminate cement exhibits early strength and micro-expansion characteristics, with a specific surface area of ​​380~450 m². 2 / kg, initial setting time not earlier than 15 minutes. The expansion effect of its hydration product, ettringite, can compensate for the shrinkage of organic components and improve volume stability. The fine sand is quartz sand with a fineness modulus of 1.8~2.2 and a mud content of <0.5%.

[0043] This invention also provides a method for preparing the above-mentioned underwater anti-dispersion composite material, comprising the following steps: P1. Preparation of premix: Dissolve the controllable synthetic polymer bridging agent in 60% of the formulation water, stir until completely dissolved, add the network enhancer (CMC), and continue stirring to form a uniform and viscous premix; P2, Inorganic phase composite: The premixed liquid obtained in step P1 is added to sulfoaluminate cement, fine sand and charge regulator, and mechanically stirred to mix evenly to obtain a stable and cohesive inorganic reinforced slurry matrix; P3. Preparation of polymerization initiator solution: Dissolve the acrylamide monomer, ammonium persulfate initiator and accelerator in the remaining 40% of the formulation water, stir evenly to form the acrylamide in-situ polymerization initiator solution; P4. In-situ Composite and Casting: The polymerization initiator obtained in step P3 is rapidly added to the slurry matrix obtained in step P2, and stirred at high speed for 30-60 seconds to obtain a composite slurry with good fluidity and underwater anti-dispersion properties. Underwater casting is then carried out. After casting, the rapid polymerization of acrylamide and the hydration of sulfoaluminate cement proceed simultaneously under the mediation of a controllable synthetic polymer bridging agent, ultimately forming an integrated "anchoring-bridging-interpenetration" reinforcement structure characterized by chemical anchoring, steric hindrance, crystallization crosslinking, hydrogen bond network, and interpenetrating structure.

[0044] The present invention will now be described in detail with reference to embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in the embodiments of the present invention can be combined with each other.

[0045] The sources of the main raw materials used in the following embodiments are as follows: Sodium carboxymethyl cellulose (degree of substitution 0.75), Shanghai Aladdin Biochemical Technology Co., Ltd., Model: 3,4-Dihydroxybenzoic acid, Shanghai Maclean's Biochemical Technology Co., Ltd., Model: 97% (T), Analytical grade AR; N,N'-Dicyclohexylcarbodiimide, Shanghai Maclean's Biochemical Technology Co., Ltd., Model: ≥99%; 4-Dimethylaminopyridine, Guangdong Yuanfeng Chemical Reagent Co., Ltd., Model: 98%, Analytical grade; Undecylbromobromophenol, Tianjin Kebaisi Chemical Co., Ltd., Model: AR≥97%; Sodium methoxide, Shanghai Maclean's Biochemical Technology Co., Ltd., Model: Reagent grade 98%; Ethylene oxide, Shanghai Maclean's Biochemical Technology Co., Ltd., Model: ≥99%; Stannous octoate, Shanghai Maclean's Biochemical Technology Co., Ltd., Model: ≥95%; ε-Caprolactone, Shanghai Aladdin Biochemical Technology Co., Ltd. Sodium bisulfite, Sinopharm Chemical Reagent Co., Ltd., model: purity ≥97%; Triethanolamine; Shanghai Aladdin Biochemical Technology Co., Ltd., model: ≥99% (GC); Acrylamide monomer, Jinan Century Tongda Chemical Co., Ltd., model: content ≥98%; Dimethyl diallyl ammonium chloride-acrylamide copolymer (cationic charge density 4.2 meq / g), Shanghai Maclean Biochemical Technology Co., Ltd.; Ammonium persulfate, Shanghai Maclean Biochemical Technology Co., Ltd., model: reagent grade, 98.5%; Tetramethylethylenediamine, Shanghai Aladdin Biochemical Technology Co., Ltd., model: ≥99%; Sulfoaluminate cement, Tangshan Polar Bear Building Materials Co., Ltd., model: 52.5.

[0046] Example 1 This embodiment provides an underwater anti-dispersion composite material, the composition of which is as follows by weight: 3.5 parts of controllable synthetic polymer bridging agent, 1.2 parts of sodium carboxymethyl cellulose (degree of substitution 0.75), and sulfoaluminate cement (specific surface area 400 m²). 2 / kg, initial setting time 20min) 58 parts, quartz sand (fineness modulus 2.0, mud content <0.3%) 48 parts, acrylamide monomer (purity ≥99.5%) 14 parts, ammonium persulfate 0.45 parts, accelerator (sodium bisulfite:triethanolamine = 3:1, mass ratio) 0.25 parts, dimethyl diallyl ammonium chloride-acrylamide copolymer (cationic charge density 4.2 meq / g) 0.45 parts, water 22 parts.

[0047] The preparation method of the controllable synthetic polymer bridging agent is as follows: S1. Terminal functionalization: Under nitrogen protection, 3,4-dihydroxybenzoic acid (15.4 g, 0.1 mol) and excess undecanoic acid (30.1 g, 0.12 mol) were reacted in 250 mL of dichloromethane with N,N'-dicyclohexylcarbodiimide (22.7 g, 0.11 mol) as the dehydrating agent and 1.2 g of 4-dimethylaminopyridine as the catalyst. The reaction was carried out at 0-5 °C for 2 h and then the temperature was raised to room temperature for 12 h. After the reaction was completed, the solution was filtered, and the filtrate was washed with water, dried, and concentrated. The crude product was dissolved in a small amount of dichloromethane and then wet-loaded onto a chromatography column packed with 200-300 mesh silica gel. The column was eluted with a mixture of petroleum ether and ethyl acetate (volume ratio of 10:1 to 5:1). The composition of the eluent was monitored by thin-layer chromatography (TLC). Fractions containing a single target product spot were collected, combined, and the solvent was removed by rotary evaporation under reduced pressure at 40°C. The product was then dried under vacuum to obtain catechol-based undecyl bromide ester, i.e., the catechol functionalization initiator.

[0048] The product of step S1 was subjected to 1H NMR spectroscopy, as shown below. Figure 1 As shown in curve ①, the product exhibits a characteristic proton peak of the benzene ring at δ6.8~7.5ppm, and a methylene proton peak connected to the ester group appears near δ4.2ppm, confirming the successful introduction of the catechol structure and the occurrence of the esterification reaction.

[0049] S2. Controlled polymerization of hydrophilic segments: The catechol functionalized initiator (5.0 g) obtained in step S1 and sodium methoxide (0.1 g) were added to a dry high-pressure reactor, and the reactor was evacuated and purged with nitrogen three times. Ethylene oxide (38.6 g) was slowly injected into the reactor, and the reaction was stirred at 100 °C for 10 h. After the reaction was completed, the mixture was cooled to room temperature, the product was dissolved in dichloromethane, washed and neutralized with acidic aqueous solution, and the organic phase was dried over anhydrous sodium sulfate and the solvent was removed by rotary evaporation to obtain the catechol-polyethylene oxide (PEO) intermediate.

[0050] The product of step S2 was subjected to 1H NMR spectroscopy, as shown below. Figure 1 As shown in curve ②, compared with curve ①, the spectrum shows an extremely strong single peak of PEO segment (-CH2CH2O-) at δ3.64ppm, while retaining the characteristic peak of benzene ring, indicating that the hydrophilic segment has successfully initiated polymerization.

[0051] S3. Controllable chain extension of hydrophobic segments: The intermediate obtained in step S2 (30 g, containing approximately 0.01 mol of hydroxyl groups) and ε-caprolactone (34.4 g, 0.3 mol) were added to a dry three-necked flask, and stannous octoate (0.03 g) was added as a catalyst. The reaction was carried out under nitrogen protection in an oil bath at 120 °C for 12 h. After the reaction was complete, the product was dissolved in an appropriate amount of tetrahydrofuran, precipitated in a large amount of cold methanol (0~5 °C), filtered, washed three times with cold methanol, and finally dried under vacuum at 40 °C for 48 h to obtain a white solid product, namely, catechol-polyethylene oxide-polycaprolactone copolymer. The molar number of hydroxyl groups in the intermediate obtained in step S2 was calculated as follows: First, the number-average molecular weight (already calculated later) was determined. Then, in step S3, the molar number of hydroxyl groups used as the macromolecular initiator could be obtained by converting the molecular weight using a weighing method. Since each catechol-polyethylene oxide intermediate molecular chain contains an active hydroxyl group (-OH) at its end, the molar number of the intermediate is equivalent to the molar number of active sites of the macromolecular initiator in the reaction system. The specific calculation steps are as follows: First, weigh the intermediate after purification and thorough vacuum drying, m (g), and then use the formula... The exact number of moles was calculated.

[0052] like Figure 1 As shown in curve ③, a series of new characteristic peaks of PCL segments appeared in the spectrum in the ranges of δ4.06ppm (-CH2O-), 2.30ppm (-COCH2-) and 1.3~1.7ppm, confirming the successful construction of the amphiphilic block copolymer structure of the final product.

[0053] S4. Purification and Characterization: The product obtained in step S3 was precipitated, washed, and vacuum dried; the product was characterized by proton nuclear magnetic resonance spectroscopy, such as... Figure 1 As shown. The dried, controlled-synthetic polymer bridging agent should be sealed and stored away from light for later use.

[0054] in accordance with Figure 1Curve ③ was used for end-group analysis to calculate the degree of polymerization: the integral area of ​​the proton (3H) of the catechol benzene ring at δ 6.8~7.5ppm was set as 3.00 as the internal standard; the integral area of ​​the PEO segment (4H) at δ 3.64ppm was found to be approximately 272.0, and n = 272.0 / 4 ≈ 68 was calculated; the integral area of ​​the PCL segment (2H) at δ 4.06ppm was found to be approximately 60.0, and m = 60.0 / 2 ≈ 30 was calculated.

[0055] Based on this calculation, the molecular weight of the hydrophilic segment PEO in the bridging agent is approximately 3000, the molecular weight of the hydrophobic segment PCL is approximately 3400, and the mass ratio of the hydrophobic segment to the hydrophilic segment is approximately 1.13:1.

[0056] The preparation method of the underwater anti-dispersion composite material in this embodiment includes the following steps: P1. Preparation of premixed solution: Weigh out 3.5 parts of the controllable synthetic polymer bridging agent as specified in the formula, add it to 13.2 parts of water (60% of the total water volume), and stir at 500 rpm for 30 minutes at 25°C until completely dissolved, presenting a clear or slightly opalescent solution. Then add 1.2 parts of sodium carboxymethyl cellulose and continue stirring for 30 minutes to form a homogeneous, viscous premix. P2, Inorganic phase composite: Sulfoaluminate cement (58 parts), quartz sand (48 parts), and charge modifier (0.45 parts, dimethyl diallyl ammonium chloride-acrylamide copolymer) were placed in a planetary mixer and pre-dry-mixed for 1 minute. Then, the premixed liquid obtained in step P1 was slowly added to the dry powder mixture, and the mixture was stirred at low speed (150 rpm) for 1 minute, followed by high speed (400 rpm) for 3 minutes to obtain a uniform, cohesive inorganic reinforced slurry matrix. P3. Preparation of polymerization initiator solution: In another container, acrylamide monomer (14 parts), ammonium persulfate (0.45 parts), and accelerator (0.25 parts) are dissolved in the remaining 40% water (i.e., 8.8 parts water), and stirred manually or at low speed until completely dissolved to obtain an in-situ polymerization initiator for acrylamide. P4. In-situ composite and casting: The polymerization initiator liquid obtained in step P3 is quickly poured into the slurry matrix prepared in step P2, and the mixer is immediately started and stirred at high speed (600 rpm) for 45 seconds to obtain a composite material slurry with good fluidity, no stratification, and no bleeding. The slurry is then poured into an underwater test mold (simulating an underwater environment) or subjected to other performance tests.

[0057] The performance of the above composite material was tested. The test methods are detailed in the experimental example. The underwater dispersion loss rate, the bond strength with the underwater saturated dry concrete substrate, the 28-day flexural strength, the degree of improvement in flexural strength, and the chloride ion diffusion coefficient were measured. The data are summarized in Table 1.

[0058] Example 2 The difference between this embodiment and Example 1 is that the amounts of the controllable polymer bridging agent and acrylamide monomer were mainly adjusted, while other components were adjusted accordingly. The composition by weight is as follows: The controlled-synthetic polymer bridging agent consists of 2.0 parts, sodium carboxymethyl cellulose (degree of substitution 0.75) 1.2 parts, sulfoaluminate cement 60 parts, quartz sand 50 parts, acrylamide monomer 10 parts, ammonium persulfate 0.35 parts, accelerator 0.18 parts, dimethyl diallyl ammonium chloride-acrylamide copolymer 0.40 parts, and water 20 parts.

[0059] The preparation method, material preparation and testing method of the controllable synthetic polymer bridging agent are the same as in Example 1.

[0060] Example 3 The difference between this embodiment and Example 1 is that the amount of the controllable synthetic polymer bridging agent and acrylamide monomer is increased, while other components are adjusted accordingly. The composition by weight is as follows: The controlled-synthetic polymer bridging agent consists of 5.0 parts, sodium carboxymethyl cellulose (degree of substitution 0.75) 1.2 parts, sulfoaluminate cement 55 parts, quartz sand 45 parts, acrylamide monomer 18 parts, ammonium persulfate 0.55 parts, accelerator 0.32 parts, dimethyl diallyl ammonium chloride-acrylamide copolymer 0.50 parts, and water 25 parts.

[0061] The preparation method, material preparation and testing method of the controllable synthetic polymer bridging agent are the same as in Example 1.

[0062] Example 4 The difference between this embodiment and Example 1 lies in the change of the relative content of polycaprolactone (PCL) and polyethylene oxide (PEO) segments in the controlled-synthetic polymer bridging agent. In step S3 of the controlled-synthetic polymer bridging agent preparation, the amount of ε-caprolactone added is adjusted. Specifically, the intermediate (30g) obtained in step S2 and 24.0g (approximately 0.2mol) of ε-caprolactone are added to the reaction system, and the bridging agent is obtained through polymerization. The remaining components, proportions, preparation methods, and testing methods are the same as in Example 1.

[0063] Example 5 The difference between this embodiment and Example 1 lies in the change of the relative content of polycaprolactone (PCL) and polyethylene oxide (PEO) segments in the controlled-synthetic polymer bridging agent. In step S3 of the controlled-synthetic polymer bridging agent preparation, the amount of ε-caprolactone added is adjusted. Specifically, the intermediate (30g) obtained in step S2 and 45.0g (approximately 0.39mol) of ε-caprolactone are added to the reaction system, and the bridging agent is obtained through polymerization. The remaining components, proportions, preparation methods, and testing methods are the same as in Example 1.

[0064] Comparative Example 1 The composition of this comparative example is basically the same as that of Example 1, but without the addition of the controlled-synthetic polymer bridging agent (3.5 parts). To maintain approximately the same total volume and consistency, the 3.5 parts of the controlled-synthetic polymer bridging agent were replaced by water by an equal mass, i.e., the total water volume was adjusted to 25.5 parts. The amount of sodium carboxymethyl cellulose remained at 1.2 parts, and the remaining components and amounts were the same as in Example 1, as detailed below: Sodium carboxymethyl cellulose (degree of substitution 0.75) 1.2 parts, sulfoaluminate cement (specific surface area 400 m² / kg, initial setting 20 min) 58 parts, quartz sand (fineness modulus 2.0, mud content <0.3%) 48 parts, acrylamide monomer (purity ≥99.5%) 14 parts, ammonium persulfate 0.45 parts, accelerator (sodium bisulfite:triethanolamine = 3:1, mass ratio) 0.25 parts, dimethyl diallyl ammonium chloride-acrylamide copolymer (cationic charge density 4.2 meq / g) 0.45 parts, water 25.5 parts.

[0065] The preparation and testing methods for this comparative example are the same as those for Example 1.

[0066] Comparative Example 2 The composition of this comparative example is basically the same as that of Example 1, but acrylamide monomer (14 parts), ammonium persulfate (0.45 parts), and accelerator (0.25 parts) are not added. To maintain the fluidity of the slurry, these 14.7 parts by mass are replaced with water, that is, the total water volume is adjusted to 36.7 parts. The remaining components and amounts are the same as in Example 1, as detailed below: 3.5 parts of controllable synthetic polymer bridging agent, 1.2 parts of sodium carboxymethyl cellulose (degree of substitution 0.75), and sulfoaluminate cement (specific surface area 400 m²). 2 / kg, initial setting time 20min) 58 parts, quartz sand (fineness modulus 2.0, mud content <0.3%) 48 parts, dimethyl diallyl ammonium chloride-acrylamide copolymer (cationic charge density 4.2 meq / g) 0.45 parts, water 36.7 parts.

[0067] The preparation and testing methods for this comparative example are the same as those for Example 1 (step P3 only requires the addition of the corresponding amount of water).

[0068] Comparative Example 3 The composition of this comparative example is basically the same as that of Example 1, except that the sulfoaluminate cement (58 parts) is replaced by an equal mass of 42.5 grade ordinary Portland cement (PO 42.5). The remaining components and amounts are the same as in Example 1.

[0069] The preparation and testing methods for this comparative example are the same as those for Example 1.

[0070] Comparative Example 4 The composition of this comparative example is basically the same as that of Example 1, but without the addition of dimethyl diallyl ammonium chloride-acrylamide copolymer (charge regulator, 0.45 parts). To maintain the fluidity of the slurry, this 0.45 parts were replaced by water by an equal mass, i.e., the total water volume was adjusted to 22.45 parts. The remaining components and amounts are the same as in Example 1.

[0071] The preparation and testing methods for this comparative example are the same as those for Example 1.

[0072] Comparative Example 5 The composition of this comparative example is basically the same as that of Example 1, except that the controllable synthetic polymer bridging agent (3.5 parts) is replaced with a simple mixture of physically mixed polyethylene oxide (number average molecular weight 3000, 1.5 parts) and polycaprolactone (number average molecular weight 3500, 2.0 parts), and a small amount (0.1 parts) of dopamine hydrochloride is added to simulate catechol groups. The mass ratio of polycaprolactone (PCL) to polyethylene oxide (PEO) is approximately 1.33:1, and the total mass of 3.5 parts is the same as the number of parts of the controllable synthetic polymer bridging agent in Example 1. The remaining components and amounts are the same as in Example 1.

[0073] The preparation and testing methods are the same as in Example 1 (the stirring time needs to be extended during the preparation of the premix to attempt to dissolve / disperse the mixture).

[0074] The test methods used in the above embodiments and comparative examples are as follows: 1. Underwater anti-dispersion loss rate test: The underwater anti-dispersion loss rate test of mortar was conducted by measuring the mass loss before and after water scouring. A certain weight of freshly mixed mortar was poured directly into a molding mold placed underwater and allowed to stand for 1 minute to allow it to initially set. Then, the mortar was continuously stirred in the water at a rate of 500 rpm for 10 minutes to simulate the scouring effect of a dynamic water environment on the mortar. After the test, the sample was removed, loose particles and adhering moisture were cleaned from the surface, and the remaining mass was weighed. The anti-dispersion loss rate of the mortar under underwater conditions was obtained by calculating the percentage difference in mortar mass before and after scouring relative to the initial mass.

[0075] 2. Bond strength: The bond strength test of mortar was conducted according to JGJ / T 70-2009 standard. Using figure-eight shaped specimens cured as specified, a tensile testing machine was used to apply a uniform load along the bond surface until failure. The maximum load was recorded, and the strength value was calculated. Each group of valid specimens should contain no fewer than six specimens, and the average value was taken as the result. If a single value deviates by more than 20% of the average value, it is discarded, and the average value is recalculated using the remaining values. If fewer than four valid data points are available, the test result is invalid. The result is accurate to 0.01 MPa.

[0076] 3. Flexural strength test: The flexural strength test of cement mortar was conducted according to GB / T 17671-2021, "Test Method for Strength of Cement Mortar (ISO Method)". However, the casting method was slightly modified; specimens were cast underwater and demolded after 1 day, then cured to the specified age. During testing, the specimen was placed sideways on the support rollers of the flexural testing machine and uniformly loaded at a rate of 50±10 N / s until fracture. The failure load was recorded, and the strength value was calculated. The arithmetic mean of three valid specimens in each group was taken as the flexural strength result; if the deviation of a single value from the average value exceeded ±10%, it was discarded, and the average value was taken; if both values ​​exceeded the tolerance, the test was invalid. The calculation result was accurate to 0.1 MPa.

[0077] The degree of improvement in flexural strength was determined by comparison with ordinary underwater concrete of the same strength grade. The specific composition of ordinary underwater concrete of the same strength grade is 58 parts of sulfoaluminate cement, 48 parts of quartz sand, and 22 parts of water. The preparation method is to mix the cement and quartz sand, add water, and stir until uniform. Then, the experiment is carried out according to the normal pouring, curing and testing methods.

[0078] 4. Chloride ion diffusion coefficient test: The chloride ion diffusion coefficient of mortar was tested according to the RCM method in T / CECS 882-2021. Slices of specimens cured to the specified age were vacuum-saturated with salt and placed in a dedicated test tank, with sodium chloride cathodic solution and sodium hydroxide anolyte injected into both sides respectively. A constant DC voltage was applied across the specimens, and the chloride ion diffusion coefficient was calculated by measuring the migration depth of chloride ions within a specified time. Each group of valid specimens contained no fewer than three specimens, and their arithmetic mean was used as the test result. When the deviation of a single measured value from the median value exceeded 15%, the median value was taken as the result; if both the maximum and minimum values ​​exceeded this range, the test group was invalid. The calculation results were accurate to 0.1 × 10⁻⁻¹. 12 m 2 / s.

[0079] The performance test results of Examples 1-5 and Comparative Examples 1-5 are summarized in the table below: Table 1 Summary of Performance Test Results

[0080] As shown in Table 1, compared with Example 1, Example 2 reduced the amount of bridging agent and acrylamide, resulting in a slight decrease in anti-dispersion properties (which are negatively correlated with the underwater anti-dispersion loss rate) and bonding strength, but still maintained an excellent level; the improvement in toughness was reduced.

[0081] Compared with Example 1, Example 3 increases the amount of key organic components, which can further improve anti-dispersion, bonding strength and toughness, but the material cost increases accordingly.

[0082] Compared with Example 1, Example 4 shows a slight decrease in toughening effect (flexural strength) due to the reduction in polycaprolactone (PCL) crystalline micro-regions, but better anti-dispersion performance due to the relatively high content of polyethylene oxide (PEO).

[0083] Compared with Example 1, Example 5 shows that the increased polycaprolactone (PCL) content leads to enhanced hydrophobicity, slight adjustment of the initial cohesiveness of the slurry, and a slight increase in the resistance to dispersion loss. However, the number of physical crosslinking points in the crystallization increases, and the toughness of the material is significantly improved.

[0084] The results of Comparative Example 1 show that, in the absence of specially designed and controllable synthetic polymer bridging agents, effective underwater anti-dispersion and strong adhesion cannot be achieved by relying solely on CMC and charge regulators, and the material properties degrade to the level of ordinary modified mortar.

[0085] The results of Comparative Example 2 show that, in the absence of a flexible interpenetrating network formed by acrylamide polymerization, the toughness (flexural strength) and bond strength of the material are significantly reduced, and the material is more brittle overall.

[0086] The results of Comparative Example 3 indicate that ordinary silicate cement has a large shrinkage, and the interaction between early hydration products and the catechol groups of the bridging agent may be weaker than that of sulfoaluminate cement, resulting in a decrease in volume stability, bond strength and final toughness.

[0087] The results of Comparative Example 4 show that, in the absence of electrostatic stabilization and bridging flocculation assistance from charge regulators, relying solely on the steric hindrance of the controllable synthetic polymer bridging agent and the viscosity of CMC, an observable decrease in anti-dispersion (i.e., decreased anti-dispersion due to increased underwater anti-dispersion loss rate) is observed, demonstrating that charge regulators play an indispensable role in optimizing slurry stability.

[0088] The results of Comparative Example 5 show that polymers obtained through simple physical mixing cannot form molecular structures with a clear integrated "anchoring-bridging-toughening" function. Severe phase separation occurred between polyethylene oxide and polycaprolactone, preventing dopamine from effectively positioning and exerting its interfacial anchoring effect. This resulted in significantly inferior anti-dispersion properties, bond strength, and toughness compared to Example 1, demonstrating the necessity of the present invention for the controllable synthesis of bridging agents with specific structures.

[0089] In summary, the underwater anti-dispersion composite materials provided in Examples 1-5 of this invention exhibit superior underwater anti-dispersion properties (loss rate <5%), adhesion strength to wet substrates (>3.5 MPa), material toughness (flexural strength improvement >180%), and impermeability (chloride ion diffusion coefficient <2.5 × 10⁻⁶). -12 m 2 The invention demonstrates excellent performance in various aspects, including dispersion loss, weak interfacial adhesion, and insufficient toughness in underwater repair materials through molecular design and network synergy. The results of Comparative Examples 1-5 clearly show that the controllably synthesized amphiphilic block polymer "catechol-polyethylene oxide (PEO)-polycaprolactone (PCL)" is the core key to achieving multiple performance enhancements; the in-situ polymerization network of acrylamide is crucial for toughening; sulfoaluminate cement is superior to ordinary silicate cement due to its expansion characteristics and better interaction with the bridging agent; and the charge regulator plays an important auxiliary role in combating dispersibility. This invention successfully solves key technical problems such as large dispersion loss, weak interfacial adhesion, and insufficient toughness in underwater repair materials through molecular design and network synergy.

[0090] The present invention also observed the microstructure of Example 1 and Comparative Example 1: Among them, the SEM image of Comparative Example 1 is as follows: Figure 3 As shown, its microstructure is relatively loose and porous, with a large number of exposed needle-like crystals (typical ettringite, a hydration product of sulfoaluminate cement). These crystals are randomly packed, with obvious voids and cracks between the crystals and between the crystals and the matrix. Due to the lack of chemical anchoring and film-forming encapsulation by a controllable synthetic polymer bridging agent, the inorganic hydration products cannot form a tight whole, resulting in many internal defects in the material. Macroscopically, this manifests as low bonding strength and poor anti-dispersion properties (high loss rate).

[0091] The SEM image of Example 1 is as follows: Figure 2 As shown: This sample exhibits a highly dense and continuous microstructure. Compared with Comparative Example 1 ( Figure 3 Compared to the previous method, the number of exposed needle-like crystals is significantly reduced, replaced by a uniformly covered organic polymer film. This indicates that the controllable synthetic polymer bridging agent and the in-situ polymerized acrylamide network of the present invention successfully constructed a dense interpenetrating network structure in the cement matrix.

[0092] This polymer phase not only effectively fills the micropores and reduces the porosity, but also tightly binds the inorganic particles together through chemical bonding and physical encapsulation. This structural feature of "organic membrane encapsulating inorganic phase" is the fundamental reason why the material obtains excellent underwater anti-dispersion properties (loss rate <5%) and high toughness.

[0093] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An underwater anti-dispersion composite material, characterized in that, By weight, it comprises the following components: 2-5 parts of controllable synthetic polymer bridging agent, 0.8-1.5 parts of network reinforcing agent, 50-65 parts of sulfoaluminate cement, 40-55 parts of fine sand, 10-18 parts of acrylamide monomer, 0.3-0.6 parts of ammonium persulfate initiator, 0.15-0.35 parts of accelerator, 0.3-0.6 parts of charge regulator, and 18-28 parts of water; The network reinforcing agent is sodium carboxymethyl cellulose with a degree of substitution of 0.6 to 0.9; the charge regulator is dimethyl diallyl ammonium chloride-acrylamide copolymer with a cationic charge density of 3.5 to 5.0 meq / g. The controllable synthetic polymer bridging agent is an amphiphilic block copolymer prepared by a sequentially controllable three-step polymerization method, and its molecular structure is as follows: ; In this molecule, the R1 group at one end is a catechol anchoring group, the S2 segment in the middle is a hydrophilic segment of polyethylene oxide, and the S3 segment at the other end is a hydrophobic segment of polycaprolactone; n is an integer between 40 and 100, m is an integer between 10 and 60, and the mass ratio of the hydrophobic segment of polycaprolactone to the hydrophilic segment of polyethylene oxide is (0.8~1.5):1; The underwater anti-dispersion composite material is prepared by a method including the following steps: P1. Preparation of premix: Dissolve the controllable synthetic polymer bridging agent in 60% of the formulation water, stir until completely dissolved, add the network reinforcing agent, and continue stirring to form a uniform and viscous premix; P2, Inorganic phase composite: The premixed liquid obtained in step P1 is added to sulfoaluminate cement, fine sand and charge regulator, and mechanically stirred to mix evenly to obtain an inorganic reinforced slurry matrix; P3. Preparation of polymerization initiator solution: Dissolve the acrylamide monomer, ammonium persulfate initiator and accelerator in the remaining 40% of the formulation water, stir evenly to form the acrylamide in-situ polymerization initiator solution; P4. In-situ composite and casting: Add the polymerization initiator liquid obtained in step P3 to the slurry matrix obtained in step P2, stir for 30-60 seconds to obtain the composite material slurry, and then carry out underwater casting construction.

2. The underwater anti-dispersion composite material as described in claim 1, characterized in that, The three-step polymerization method for the controllable synthesis of polymer bridging agents includes the following preparation steps: S1. Terminal functionalization: Starting with 3,4-dihydroxybenzoic acid, an active bromoalkyl terminus is introduced through esterification to obtain a catechol functionalization initiator. S2. Hydrophilic segment controlled polymerization: Using the product obtained in step S1 as an initiator, in the presence of an alkaline catalyst, the ring-opening polymerization of ethylene oxide monomer is initiated. The polymerization temperature is 80~110℃ and the reaction time is 6~12h to obtain catechol-polyethylene oxide intermediate. S3. Controllable chain extension of hydrophobic segments: Using the intermediate obtained in step S2 as a macromolecular initiator, the ε-caprolactone monomer is initiated to undergo ring-opening polymerization under the action of an organometallic catalyst. The polymerization temperature is 100~130℃ and the reaction time is 8~16h. S4. Purification: The product obtained in step S3 is precipitated, washed, and vacuum dried to obtain the controllable synthetic polymer bridging agent.

3. The underwater anti-dispersion composite material as described in claim 2, characterized in that, In step S1, the molar ratio of 3,4-dihydroxybenzoic acid to bromoalkyl alcohol is 1:(1.1~1.3); the molar ratio of the dehydrating agent N,N'-dicyclohexylcarbodiimide to 3,4-dihydroxybenzoic acid used in the esterification reaction is (1.0~1.2):1; and the amount of the catalyst 4-dimethylaminopyridine used in the esterification reaction is 5%~15% of the molar amount of 3,4-dihydroxybenzoic acid.

4. The underwater anti-dispersion composite material as described in claim 3, characterized in that, In step S2, the molar ratio of the initiator to the ethylene oxide monomer is 1:(40~100), and the amount of alkaline catalyst is 1%~5% of the mass of the initiator. The alkaline catalyst is sodium methoxide or potassium tert-butoxide.

5. The underwater anti-dispersion composite material as described in claim 4, characterized in that, In step S3, the molar ratio of the macromolecular initiator to the ε-caprolactone monomer is 1:(10~60), the amount of organometallic catalyst is 0.05%~0.2% of the total mass of the monomer, and the organometallic catalyst is stannous octoate or aluminum triisopropoxy.

6. The underwater anti-dispersion composite material as described in claim 1, characterized in that, The accelerator is a compound system of sodium bisulfite and triethanolamine, with a mass ratio of sodium bisulfite to triethanolamine of (2~4):

1.

7. The underwater anti-dispersion composite material as described in claim 1, characterized in that, The specific surface area of ​​the sulfoaluminate cement is 380~450 m². 2 / kg, initial setting time not earlier than 15 minutes; the fine sand is quartz sand with a fineness modulus of 1.8~2.2 and a mud content of less than 0.5%.

Citation Information

Patent Citations

  • Phosphonic acid-based water-reducing agent as well as preparation method and application thereof

    CN108129625A

  • Underwater non-dispersible early-strength grouting material and preparation method thereof

    CN120554051A