Thermal insulation material, method for its production and use
By chemically bonding modified aerogel with modified basalt fiber, the problem of uneven dispersion of inorganic components in organic matrix is solved, a stable composite system is constructed, and the thermal insulation and mechanical properties of thermal insulation materials are improved, making them suitable for building doors and windows.
Patent Information
- Application Number
- CN202610633741.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-09
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-05-09
AI Technical Summary
The inorganic components of existing window and door insulation materials have poor compatibility with the organic matrix interface, which easily leads to uneven dispersion and agglomeration, resulting in reduced insulation performance and decreased mechanical strength, thus failing to meet the requirements of high-efficiency energy-saving buildings.
By chemically bonding modified aerogel and modified basalt fiber, stable inorganic functional units are formed through aminosilane-modified zirconium nitride aerogel and epoxysilane-modified basalt fiber. This improves the dispersion and compatibility of inorganic components in organic systems and constructs a uniform composite system through chemical bonding.
It achieves long-term structural stability and excellent thermal insulation performance of the material, while also providing moderate sound insulation, thus meeting the requirements for building doors and windows.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application belongs to the field of thermal insulation materials technology, and specifically relates to a thermal insulation material, its preparation method and application. Background Technology
[0002] With the continuous improvement of building energy efficiency standards, heat loss control of building doors and windows has become a key aspect of building energy conservation. The performance of thermal insulation materials used in doors and windows directly affects the overall energy consumption level and user comfort of a building. Currently, the thermal insulation materials used in door and window components are mostly organic polymer foam materials. These materials are widely used in building door and window thermal insulation applications due to their convenient molding and good adaptability.
[0003] In practical applications, existing thermal insulation materials for doors and windows still have many insurmountable defects. Traditional foam materials have limited thermal insulation capacity, making it difficult to meet the thermal insulation requirements of high-efficiency energy-saving buildings. Under long-term use or in environments with temperature fluctuations, the thermal insulation performance of the materials is prone to degradation, failing to maintain a stable thermal insulation effect. To improve thermal insulation performance, the industry usually introduces inorganic thermal insulation components into the material system. However, the interfacial compatibility between inorganic components and the organic matrix is poor, easily leading to uneven dispersion and agglomeration. This not only fails to fully utilize the thermal insulation advantages of the inorganic phase but also damages the internal cell structure of the material, resulting in a decline in the overall performance of the material. At the same time, the lack of a stable bond between inorganic components and the organic matrix easily leads to problems such as interface separation and structural loosening after long-term use, significantly reducing the mechanical strength and dimensional stability of the material, making it difficult to meet the mechanical and weather resistance requirements of door and window profiles for long-term use. Summary of the Invention
[0004] This application aims to improve at least one technical problem in the background art.
[0005] The first aspect of this application provides a heat insulation material, the raw materials of which, by weight, include: 80-95 parts of polyester polyol, 40-60 parts of polyether polyol, 40-65 parts of polyisocyanate, 20-50 parts of modified aerogel, 1-5 parts of modified basalt fiber, 0.5-2 parts of catalyst, 2-8 parts of foaming agent, 1-3 parts of foam stabilizer, and 1-4 parts of water. The modified aerogel is obtained by modifying zirconium nitride aerogel with aminosilane. The zirconium nitride aerogel is formed by mixing zirconium source and organic carbon source to form a gel, and then successively subjected to supercritical CO2 drying and carbothermal nitriding. Modified basalt fiber is obtained by modifying short-cut basalt fiber with an epoxy silane coupling agent.
[0006] The thermal insulation material provided in this application uses polyester polyol and polyether polyol as the main organic matrix components, which react with polyisocyanate to form a cross-linked, stable polyurethane skeleton, providing reliable mechanical support and a molding basis for the material. The catalyst, foaming agent, foam stabilizer, and water in the system synergistically regulate the foaming and molding process of the material, forming a uniform and regular cell structure, providing structural assurance for the realization of the material's core thermal insulation performance. The modified aerogel in the thermal insulation material is mainly composed of zirconium nitride aerogel. This aerogel is prepared by gelling zirconium source and organic carbon source, followed by supercritical carbon dioxide drying and carbothermal nitriding processes. It possesses inherent characteristics of high porosity and low thermal conductivity. After modification with aminosilane, stable amino active groups can be loaded on the surface, effectively improving the dispersion and compatibility of the inorganic phase in the organic system. The modified basalt fiber is prepared by modifying short-cut basalt fiber with an epoxy silane coupling agent. The fiber surface has epoxy active groups, mainly participating in the system construction as an auxiliary functional component.
[0007] During the blending and molding process, the amino groups on the surface of the modified aerogel and the epoxy groups on the surface of the modified basalt fiber can undergo ring-opening addition reactions, allowing the two inorganic components to bond together through chemical bonds to form stable inorganic functional units. This avoids the problems of agglomeration or uneven distribution of inorganic fillers. At the same time, the unreacted active groups can further form chemical bonding interfaces with the polyurethane matrix, allowing the inorganic functional phase to be tightly bonded to the organic matrix. This improves the problem of poor compatibility between inorganic fillers and organic matrix, ensuring the long-term stability of the overall structure of the material.
[0008] The thermal insulation material provided in this application focuses on thermal insulation as its core performance. Zirconium nitride aerogel, with its nanoporous structure, effectively hinders solid-state heat conduction and weakens heat radiation transfer. Combined with the closed-cell structure of the polyurethane matrix, this double-blocking of heat transfer paths gives the material outstanding thermal insulation capabilities. Modified basalt fiber primarily plays a supporting role in enhancing structural stability and also attenuates sound wave transmission, providing moderate sound insulation improvement. The addition of fiber components does not affect the integrity of the pores, thus ensuring that the core thermal insulation performance remains undisturbed. The synergistic effect of all components gives the material both excellent thermal insulation performance and good structural stability, meeting the requirements for thermal insulation components in building doors and windows.
[0009] Preferably, the molar ratio of zirconium to carbon in the zirconium source and the organic carbon source is 1:(8-15).
[0010] Preferably, the zirconium source includes at least one of zirconium oxychloride, zirconium nitrate, zirconium acetate, zirconium isopropoxide, and zirconium n-butoxide.
[0011] Preferably, the organic carbon source includes at least one of glucose, sucrose, starch, cellulose, fructose, and urea.
[0012] Preferably, the mass ratio of zirconium nitride aerogel to aminosilane is 1:(0.1-0.5); the aminosilane includes at least one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropyltriethoxysilane.
[0013] The above-mentioned method for preparing modified aerogel includes the following steps: Zirconium source was dissolved in a mixed solution of water and hydrochloric acid, and then an organic carbon source was added. The mixture was aged at a temperature of 60℃-80℃ to obtain a gel. The gel was dried by supercritical CO2 and then heated to 1000℃-1200℃ in a nitrogen atmosphere to perform carbothermal nitridation, thus obtaining zirconium nitride aerogel. Zirconium nitride aerogel and aminosilane were added to ethanol and stirred to obtain modified aerogel.
[0014] Preferably, the length of the chopped basalt fibers is 50μm-80μm.
[0015] Preferably, the mass ratio of chopped basalt fibers to epoxy silane is 1:(0.05-0.3); the epoxy silane includes at least one of γ-epoxypropyl etheroxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-epoxypropyl etheroxypropyltriethoxysilane.
[0016] The above-mentioned method for preparing modified basalt fibers includes the following steps: Short-cut basalt fibers and epoxy silanes were added to ethanol and stirred to obtain modified basalt fibers.
[0017] Preferably, the polyester polyol has a molecular weight of 1000-3000 and a hydroxyl value of 50mgKOH / g-100mgKOH / g.
[0018] Preferably, the polyether polyol has a molecular weight of 1500-3000 and a hydroxyl value of 40mgKOH / g-110mgKOH / g.
[0019] Preferably, the polyisocyanate is one of isophorone diisocyanate, toluene diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate.
[0020] The second aspect of this application provides a method for preparing the aforementioned heat-insulating material, comprising the following steps: Polyester polyol, polyether polyol, modified aerogel, modified basalt fiber, catalyst, foaming agent and foam stabilizer are mixed and then polyisocyanate is added to react and obtain thermal insulation material.
[0021] The third aspect of this application provides the application of the aforementioned thermal insulation materials in thermal insulation components for building doors and windows.
[0022] The beneficial effects of this application are as follows: This application constructs a composite system with a uniform structure and strong interfacial bonding through the synergistic effect of chemical bonding between amino-modified zirconium nitride aerogel and epoxy-modified basalt fiber. This fundamentally avoids problems such as inorganic component agglomeration and interfacial separation, ensuring the long-term stability of the material's internal structure. This system fully leverages the nanoporous thermal insulation advantages of zirconium nitride aerogel, combined with the closed-cell structure of polyurethane foam, to achieve efficient blocking of heat transfer paths, endowing the material with excellent and stable thermal insulation performance. Simultaneously, the reinforcing effect and good interfacial compatibility of the modified basalt fiber enable the material to possess both mechanical properties and aging resistance, meeting the needs of long-term service scenarios. Furthermore, while ensuring core thermal insulation performance, the material also possesses moderate sound absorption capacity, achieving a balanced consideration of thermal insulation, mechanical properties, and sound insulation performance. The overall comprehensive performance is significantly improved, making it well-suited for applications in energy-saving components such as building doors and windows, and possessing broad practical value and promising prospects for promotion. Detailed Implementation
[0023] The present application will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Furthermore, it should be understood that after reading the contents of this application, those skilled in the art can make various alterations or modifications to this application, and these equivalent forms also fall within the scope defined by the appended claims.
[0024] Example 1 A thermal insulation material, the raw materials of which, by weight, comprise: 85 parts of polyester polyol (polyethylene succinate, molecular weight 1800, hydroxyl value 65 mg KOH / g), 50 parts of polyether polyol (polypropylene glycol, molecular weight 2700, hydroxyl value 55 mg KOH / g), 55 parts of polyisocyanate (diphenylmethane diisocyanate), 35 parts of modified aerogel, 3 parts of modified basalt fiber, 1 part of catalyst (dibutyltin dilaurate), 5 parts of foaming agent (1,1,1,3,3-pentafluoropropane), 2 parts of foam stabilizer (polyether modified silicone oil), and 2 parts of deionized water.
[0025] The preparation method of the modified aerogel includes the following steps: Zirconium source (zirconium oxychloride) was dissolved in a mixed solution of deionized water and hydrochloric acid (volume ratio of deionized water to hydrochloric acid was 5:1), and then carbon source (glucose, with a molar ratio of zirconium to carbon in zirconium oxychloride and glucose of 1:10) was added. The gel was aged at 70°C for 12 hours to obtain a gel. The gel was dried by supercritical CO2 (drying temperature 50℃, pressure 12MPa, drying time 6h), and then heated to 1200℃ in a nitrogen atmosphere for carbothermal nitridation (nitrogen flow rate 50mL / min, heating rate 5℃ / min, holding time 3h) to obtain zirconium nitride aerogel. Zirconium nitride aerogel and aminosilane (3-aminopropyltriethoxysilane, with a mass ratio of 1:0.3 between zirconium nitride aerogel and 3-aminopropyltriethoxysilane) were added to ethanol and stirred for reaction (reaction temperature 60℃, reaction time 4h). The solid reactant was filtered and dried under vacuum at 60℃ for 6h to obtain modified aerogel.
[0026] The preparation method of modified basalt fiber includes the following steps: Short-cut basalt fibers (65 μm in length) and epoxy silane (γ-epoxypropyl ether oxypropyl trimethoxysilane, with a mass ratio of short-cut basalt fibers to γ-epoxypropyl ether oxypropyl trimethoxysilane of 1:0.15) were added to ethanol and stirred for reaction (reaction temperature 50 °C, reaction time 3 h). The solid reactant was filtered and dried under vacuum at 60 °C for 6 h to obtain modified basalt fibers.
[0027] The preparation method of this thermal insulation material includes the following steps: Polyester polyol, polyether polyol, modified aerogel, modified basalt fiber, catalyst, foaming agent and foam stabilizer are added to a high-speed mixer and mixed (stirred at 3000 r / min for 10 min). Then, polyisocyanate is added and stirred before being poured into a molding mold. After the reaction is completed, the heat insulation material is obtained.
[0028] Example 2 A thermal insulation material, the raw materials of which, by weight, comprise: 90 parts of polyester polyol (polyethylene succinate, molecular weight 1800, hydroxyl value 65 mg KOH / g), 45 parts of polyether polyol (polypropylene glycol, molecular weight 2700, hydroxyl value 55 mg KOH / g), 50 parts of polyisocyanate (dicyclohexylmethane diisocyanate), 40 parts of modified aerogel, 2 parts of modified basalt fiber, 1.2 parts of catalyst (dibutyltin dilaurate), 4 parts of foaming agent (1,1,1,3,3-pentafluoropropane), 1.5 parts of foam stabilizer (polyether modified silicone oil), and 2.5 parts of deionized water.
[0029] The preparation method of the modified aerogel includes the following steps: Zirconium source (zirconium oxychloride) was dissolved in a mixed solution of deionized water and hydrochloric acid (volume ratio of deionized water to hydrochloric acid was 5:1), and then carbon source (sucrose, the molar ratio of zirconium to carbon in zirconium oxychloride and sucrose was 1:12) was added. The gel was aged at 70°C for 12 hours to obtain a gel. The gel was dried by supercritical CO2 (drying temperature 50℃, pressure 12MPa, drying time 6h), and then heated to 1200℃ in a nitrogen atmosphere for carbothermal nitridation (nitrogen flow rate 50mL / min, heating rate 5℃ / min, holding time 3h) to obtain zirconium nitride aerogel. Zirconium nitride aerogel and aminosilane (3-aminopropyltriethoxysilane, with a mass ratio of zirconium nitride aerogel to 3-aminopropyltriethoxysilane of 1:0.25) were added to ethanol and stirred for reaction (reaction temperature 60℃, reaction time 4h). The solid reactant was filtered and dried under vacuum at 60℃ for 6h to obtain modified aerogel.
[0030] The preparation method of modified basalt fiber includes the following steps: Short-cut basalt fibers (60 μm in length) and epoxy silane (β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, with a mass ratio of short-cut basalt fibers to β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane of 1:0.2) were added to ethanol and stirred for reaction (reaction temperature 50 °C, reaction time 3 h). The solid reactants were filtered and dried under vacuum at 60 °C for 6 h to obtain modified basalt fibers.
[0031] The preparation method of this thermal insulation material includes the following steps: Polyester polyol, polyether polyol, modified aerogel, modified basalt fiber, catalyst, foaming agent and foam stabilizer are added to a high-speed mixer and mixed (stirred at 3000 r / min for 10 min). Then, polyisocyanate is added and stirred before being poured into a molding mold. After the reaction is completed, the heat insulation material is obtained.
[0032] Example 3 A thermal insulation material, the raw materials of which, by weight, comprise: 82 parts of polyester polyol (polyethylene succinate, molecular weight 1800, hydroxyl value 65 mg KOH / g), 50 parts of polyether polyol (polypropylene glycol, molecular weight 2700, hydroxyl value 55 mg KOH / g), 60 parts of polyisocyanate (isophorone diisocyanate), 30 parts of modified aerogel, 4 parts of modified basalt fiber, 0.8 parts of catalyst (dibutyltin dilaurate), 6 parts of foaming agent (1,1,1,3,3-pentafluoropropane), 3 parts of foam stabilizer (polyether modified silicone oil), and 1.5 parts of deionized water.
[0033] The preparation method of the modified aerogel includes the following steps: Zirconium source (zirconium acetate) was dissolved in a mixed solution of deionized water and hydrochloric acid (volume ratio of deionized water to hydrochloric acid was 5:1), and then carbon source (urea, with a molar ratio of zirconium to carbon in zirconium acetate and urea of 1:9) was added. The gel was aged at 70°C for 12 hours to obtain a gel. The gel was dried by supercritical CO2 (drying temperature 50℃, pressure 12MPa, drying time 6h), and then heated to 1200℃ in a nitrogen atmosphere for carbothermal nitridation (nitrogen flow rate 50mL / min, heating rate 5℃ / min, holding time 3h) to obtain zirconium nitride aerogel. Zirconium nitride aerogel and aminosilane (N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, with a mass ratio of zirconium nitride aerogel to N-(2-aminoethyl)-3-aminopropyltrimethoxysilane of 1:0.35) were added to ethanol and stirred for reaction (reaction temperature 60℃, reaction time 4h). The solid reactant was filtered and dried under vacuum at 60℃ for 6h to obtain modified aerogel.
[0034] The preparation method of modified basalt fiber includes the following steps: Short-cut basalt fibers (70 μm in length) and epoxy silane (γ-epoxypropyl ether oxypropyltriethoxysilane, with a mass ratio of 1:0.1 between the short-cut basalt fibers and γ-epoxypropyl ether oxypropyltriethoxysilane) were added to ethanol and stirred for reaction (reaction temperature 50 °C, reaction time 3 h). The solid reactants were filtered and dried under vacuum at 60 °C for 6 h to obtain modified basalt fibers.
[0035] The preparation method of this thermal insulation material includes the following steps: Polyester polyol, polyether polyol, modified aerogel, modified basalt fiber, catalyst, foaming agent and foam stabilizer are added to a high-speed mixer and mixed (stirred at 3000 r / min for 10 min). Then, polyisocyanate is added and stirred before being poured into a molding mold. After the reaction is completed, the heat insulation material is obtained.
[0036] Comparative Example 1 An insulation material, differing from Example 1 in that the raw materials do not contain modified aerogel. Otherwise, it is the same as Example 1.
[0037] Comparative Example 2 A thermal insulation material, differing from Example 1 in that the modified aerogel in the raw materials is replaced with unmodified zirconium nitride aerogel. Otherwise, it is the same as Example 1.
[0038] Comparative Example 3 An insulation material, differing from Example 1 in that it does not contain modified basalt fiber in its raw materials. Otherwise, it is the same as Example 1.
[0039] Comparative Example 4 An insulation material, differing from Example 1 in that the modified basalt fiber in the raw materials is replaced with short-cut basalt fiber that has not undergone epoxy silane modification. Otherwise, it is the same as Example 1.
[0040] Comparative Example 5 A thermal insulation material differs from Example 1 in that, in the preparation of the modified aerogel, zirconium nitride aerogel is replaced with titanium nitride aerogel. Otherwise, it is the same as Example 1.
[0041] Comparative Example 6 A thermal insulation material, differing from Example 1 in that, in the preparation of the modified aerogel, aminosilane is replaced with methyltrimethoxysilane. Otherwise, it is the same as Example 1.
[0042] Comparative Example 7 A thermal insulation material differs from Example 1 in that, in the preparation of the modified basalt fiber, the epoxy silane is replaced with vinyltrimethoxysilane. Otherwise, it is the same as Example 1.
[0043] Comparative Example 8 An insulating material, differing from Example 1 in that the modified aerogel comprises 10 parts by weight. Otherwise, it is the same as Example 1.
[0044] Comparative Example 9 An insulating material, differing from Example 1 in that the modified aerogel comprises 65 parts by weight. Otherwise, it is the same as Example 1.
[0045] Comparative Example 10 An insulation material, differing from Example 1 in that the modified basalt fiber comprises 0.2 parts by weight. Otherwise, it is the same as Example 1.
[0046] Comparative Example 11 An insulation material, differing from Example 1 in that the modified basalt fiber comprises 10 parts by weight. Otherwise, it is the same as Example 1.
[0047] The performance of the thermal insulation materials prepared in Examples 1-3 and Comparative Examples 1-11 was tested, and the test results are shown in Table 1.
[0048] Table 1 Based on the data in Table 1, Comparative Example 1, which does not contain modified aerogel, lacks the nanoporous thermal insulation structure constructed by zirconium nitride aerogel compared to Example 1. This results in a significant decrease in the core thermal insulation capacity. Furthermore, the absence of the interfacial synergistic effect provided by the aerogel also significantly reduces the material's mechanical and sound absorption properties. Comparative Example 2 uses unmodified zirconium nitride aerogel. Compared to Example 1, its aerogel surface lacks reactive functional groups, preventing the formation of a stable interfacial bond with the modified basalt fiber and polyurethane matrix. This leads to poorer dispersion of inorganic components in the matrix and affects the internal pore structure, ultimately impacting the material's thermal insulation, mechanical, and sound absorption properties. Comparative Example 3, which does not contain modified basalt fiber, lacks the structural reinforcement provided by the modified basalt fiber compared to Example 1. This results in a certain degree of reduction in mechanical properties, weakened sound dissipation, and decreased sound absorption performance. Comparative Example 4 used unmodified chopped basalt fibers. Compared to Example 1, the surface of the chopped basalt fibers lacked epoxy active groups that could synergistically bond with the aerogel. The chopped basalt fibers, modified aerogel, and organic matrix were merely physically mixed, making it difficult to form a stable bonding interface. This not only affected the mechanical stability of the material but also reduced the overall thermal insulation and sound absorption effects. Compared to Example 1, Comparative Example 5 replaced zirconium nitride aerogel with titanium nitride aerogel. Titanium nitride aerogel had poor pore uniformity, and after high-temperature treatment, it was prone to pore wall collapse and decreased pore connectivity. This not only prevented the construction of efficient thermal insulation pathways, significantly weakening the core thermal insulation performance, but its weakened skeleton structure also failed to effectively reinforce the polyurethane matrix, leading to a simultaneous decrease in the material's mechanical properties. Comparative Example 6 modified zirconium nitride aerogel with methylsilane. Compared to Example 1, the aerogel surface could not form active sites (amino groups) capable of reacting with epoxy groups, resulting in poor interfacial bonding and disruption of the uniformity of the internal structure of the material. Ultimately, this led to a significant decline in thermal insulation, mechanical, and sound absorption properties. Comparative Example 7 modified basalt fibers with vinylsilane. Compared to Example 1, the active groups on the surface of the basalt fibers could not effectively combine with the amino groups on the surface of the aerogel. The two inorganic functional components were unable to form a stable composite structure, resulting in poor dispersion in the matrix and thus affecting the overall performance of the material.
[0049] In Comparative Example 8, the amount of modified aerogel added was too small, preventing the formation of a continuous and complete porous thermal insulation network within the system. This hindered the full realization of the modified aerogel's heat-blocking effect, and the insufficient amount of functional filler also failed to provide adequate structural support to the matrix. In Comparative Example 9, the excessive amount of modified aerogel made it difficult to disperse uniformly in the organic matrix, resulting in self-agglomeration. This not only damaged the cell structure formed by polyurethane foaming but also increased the probability of interface defects, leading to a decrease in the integrity of the material's internal structure. In Comparative Example 10, the amount of modified basalt fiber added was too small, making it difficult for the modified basalt fiber to form an effective three-dimensional reinforcing network within the system. Its reinforcement effect on the matrix was very limited, and the insufficient fiber also failed to provide enough scattering sites for sound wave dissipation. In Comparative Example 11, the excessive amount of modified basalt fiber caused it to entangle and aggregate, interfering with the normal foaming process, disrupting the regularity of the internal cells, and creating steric hindrance with the modified aerogel. This affected the uniform distribution of inorganic components, ultimately leading to a decrease in the material's mechanical properties.
[0050] The above description is only a preferred embodiment of this application. It should be noted that those skilled in the art can make several improvements and additions without departing from the method of this application, and these improvements and additions should also be considered within the scope of protection of this application.
Claims
1. A heat insulation material, characterized in that, The raw materials, by weight, include: 80-95 parts polyester polyol, 40-60 parts polyether polyol, 40-65 parts polyisocyanate, 20-50 parts modified aerogel, 1-5 parts modified basalt fiber, 0.5-2 parts catalyst, 2-8 parts foaming agent, 1-3 parts foam stabilizer, and 1-4 parts water. The foaming agent is 1,1,1,3,3-pentafluoropropane; The modified aerogel is obtained by modifying zirconium nitride aerogel with aminosilane, wherein the preparation method of the zirconium nitride aerogel includes the following steps: Zirconium source was dissolved in a mixed solution of water and hydrochloric acid, and then an organic carbon source was added. The mixture was aged at a temperature of 60℃-80℃ to obtain a gel. The gel was dried by supercritical CO2 and then heated to 1000℃-1200℃ in a nitrogen atmosphere to perform carbothermal nitridation, thus obtaining the zirconium nitride aerogel. The zirconium nitride aerogel and the aminosilane were added to ethanol and stirred to obtain the modified aerogel. The modified basalt fiber is obtained by modifying short-cut basalt fiber with an epoxy silane coupling agent.
2. The thermal insulation material according to claim 1, characterized in that, The molar ratio of zirconium to carbon in the zirconium source and the organic carbon source is 1:(8-15).
3. The thermal insulation material according to claim 1, characterized in that, The zirconium source includes at least one of zirconium oxychloride, zirconium nitrate, zirconium acetate, zirconium isopropoxide, and zirconium n-butoxide. And / or, the organic carbon source includes at least one of glucose, sucrose, starch, cellulose, fructose and urea.
4. The thermal insulation material according to claim 1, characterized in that, The mass ratio of the zirconium nitride aerogel to the aminosilane is 1:(0.1-0.5); the aminosilane includes at least one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropyltriethoxysilane.
5. The thermal insulation material according to claim 1, characterized in that, The length of the short-cut basalt fibers is 50μm-80μm.
6. The thermal insulation material according to claim 1, characterized in that, The mass ratio of the short-cut basalt fiber to the epoxy silane is 1:(0.05-0.3); the epoxy silane includes at least one of γ-epoxypropyl etheroxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-epoxypropyl etheroxypropyltriethoxysilane.
7. The thermal insulation material according to claim 1, characterized in that, The polyester polyol has a molecular weight of 1000-3000 and a hydroxyl value of 50mgKOH / g-100mgKOH / g; And / or, the polyether polyol has a molecular weight of 1500-3000 and a hydroxyl value of 40mgKOH / g-110mgKOH / g; And / or, the polyisocyanate is one of isophorone diisocyanate, toluene diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate.
8. The method for preparing the thermal insulation material according to any one of claims 1-7, characterized in that, Includes the following steps: The polyester polyol, the polyether polyol, the modified aerogel, the modified basalt fiber, the catalyst, the foaming agent, and the foam stabilizer are mixed and then the polyisocyanate is added to react, thereby obtaining the thermal insulation material.
9. The application of the thermal insulation material as described in any one of claims 1-7 in thermal insulation components for building doors and windows.
Citation Information
Patent Citations
Polyurethane foam heat insulation and decoration integrated board and preparation method thereof