Metal electrode for metal-air battery and method for manufacturing the same
The metal-air battery electrode was prepared by casting, which solved the problem of balancing electrochemical performance and mechanical strength in active materials with significant volume changes. This method enables low-cost, low-pollution industrial production and improves electrode stability.
Patent Information
- Application Number
- CN202610199933.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-02-11
AI Technical Summary
Existing technologies lack a casting process for iron-based electrodes that can balance good electrochemical performance, mechanical strength, and suitability for industrial production, especially for active materials with significant volume changes in electrolytes.
Metal electrodes for metal-air batteries are prepared using a casting molding method. Through a process of mixing slurry, ball milling, casting, and drying, carbon powder, iron oxide, and bismuth sulfide are used as the main components, combined with polyvinyl butyral (PVB) as a binder to form a uniformly distributed sheet material, ensuring the mechanical integrity and hydrogen evolution reaction performance of the electrode.
It enables low-cost, low-pollution industrial production. The electrode sheet has good flexibility and self-support, buffers volume stress, improves the mechanical integrity and cycle life of the electrode, and inhibits hydrogen evolution, thereby improving the stability of the battery.
Smart Images

Figure CN122202158B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal-air battery technology, and more particularly to a metal electrode for metal-air batteries and its preparation method. More specifically, it is a method for preparing a metal electrode for metal-air batteries by using a casting molding method to dry pressed C / (Fe2O3 or Fe3O4 or Fe) sheet material. Background Technology
[0002] Metal-air batteries (such as iron-air batteries) are becoming a highly promising technology in the new energy field due to their core advantages of high theoretical energy density and the wide availability and environmental friendliness of iron-based materials. Their unique electrochemical system of air cathode and iron anode can efficiently store and release electrical energy through the redox reaction of iron, providing a sustainable solution for diverse power needs such as new energy vehicles, grid-scale energy storage systems, and emergency backup power. They are expected to break through the energy density bottleneck of traditional lithium-ion batteries and become one of the key technologies to promote the upgrading of the global energy structure towards low carbon.
[0003] In the iron electrode preparation stage, the process route can be flexibly adapted according to cost and performance requirements: if the focus is on low-cost mass production, the dry pressing method can be used, which directly forms a film by pressing powder with a metal mold. The process is simple and the equipment investment is low. If higher electrode structure stability and cycle life are pursued, the sintering method can be selected, which enhances the crystallinity and mechanical strength of iron-based materials through high-temperature treatment, but the equipment energy consumption and process cost are relatively high. The tape casting method has both production advantages and advantages. With the help of wet slurry scraping process, it can achieve precise control of micron-level thickness and improve the batch production efficiency through large-scale tape casting equipment. It is suitable for scenarios with high requirements for electrode consistency and provides diversified technical paths for the commercialization of iron-air batteries.
[0004] Casting, as a mature thin-film material preparation technology, is widely used in the fields of ceramics and solid electrolytes, capable of producing thin films with uniform thickness and controllable density. However, applying casting to the preparation of metal electrodes for metal-air batteries, especially for iron-based active materials that exhibit significant volume changes in electrolytes, requires addressing a series of issues, including slurry formulation, electrode structure design, and compatibility with the battery system. Currently, there is a lack of a casting process for iron-based electrodes that can simultaneously achieve good electrochemical performance, mechanical strength, and suitability for industrial production. Summary of the Invention
[0005] In response to the aforementioned technical problems, a metal electrode for metal-air batteries and a method for preparing the same are provided.
[0006] The technical means employed in this invention are as follows:
[0007] A method for preparing a metal electrode for a metal-air battery includes the following steps: preparing a mixed slurry, ball milling, casting, and drying, specifically including the following steps: S1. Iron or iron oxide is mixed with carbon powder and bismuth sulfide in a certain proportion to obtain a mixed powder. S2. Dissolve polyvinyl butyral (PVB) in ethanol to form a binder solution; mix the mixed powder with the binder solution to prepare a mixed slurry; S3. After ball milling the above mixed slurry, cast it into sheet material in a mold using the casting method; S4. Dry the cast sheet material to obtain carbon / iron or iron oxide sheet material; Further, in step S1, the mass ratio of the mixed powder material is calculated as follows: carbon powder to iron or iron oxide powder to bismuth sulfide, which are 5~10% : 85~90% : 5%.
[0008] Further, step S1 specifically involves: weighing carbon powder, iron or iron oxide powder, and bismuth sulfide according to a preset ratio, ball milling the carbon powder, iron or iron oxide powder, and bismuth sulfide in a ball mill for 1 ± 0.5 h, and then mixing the ball-milled powders in a centrifuge and stirring for 3 to 4 hours.
[0009] Further, in step S3, the mixed slurry is poured into the casting mold and scraped flat into a wet film using a scraper. The thickness of the metal sheet is controlled to be 1.4~1.6mm by the scraper.
[0010] Further, in step S4, the cast slurry is placed in an oven and dried at 20-25°C for 3-4 hours to prepare a carbon / iron or iron oxide composite electrode sheet.
[0011] The present invention also claims protection for the metal electrode of the metal-air battery prepared based on the above method.
[0012] This invention utilizes a casting process, where the slurry is uniformly spread under the action of a scraper, ensuring a uniform distribution of active materials, conductive agents, and binders in a two-dimensional plane. During drying, the polymer binder (PVB) solidifies to form a continuous three-dimensional network, firmly bonding the iron-based active particles and conductive carbon materials together. This structure gives the dried electrode sheet excellent flexibility and self-support, effectively buffering volumetric stress during charging and discharging. The uniformly solidified binder network suppresses pulverization and detachment of the electrode material, thereby improving the mechanical integrity and cycle life of the electrode. The addition of bismuth sulfide significantly increases the overpotential of the hydrogen evolution reaction, thus inhibiting hydrogen evolution; simultaneously, the dispersibility and surface modification effects of bismuth sulfide also slow down the passivation of the iron electrode.
[0013] Compared with the prior art, the present invention has the following advantages: 1. This invention eliminates the need for complex dry pressing molds and high-temperature sintering equipment. The tape casting process is simple, low-cost, and pollution-free. Furthermore, the tape-cast iron electrode uses PVB as a binder, which can form a network to connect material particles during the processing, thereby giving the electrode sheet better tensile toughness. 2. This invention provides a method for preparing a composite metal electrode for a metal-air battery that is low in production cost and simple in process, and is applicable to industrial production.
[0014] 3. The electrode sheet prepared by this invention has good stability under long-term charge-discharge tests. Attached Figure Description
[0015] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1 This is a microscopic schematic diagram of a metal-air battery.
[0017] Figure 2 This diagram illustrates the charge-discharge cycle in the embodiment. Detailed Implementation
[0018] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention.
[0019] This embodiment discloses a method for preparing a metal electrode for a metal-air battery, comprising the following steps: preparing a mixed slurry, ball milling, casting, and drying, specifically including the following steps: Iron or iron oxide is mixed with carbon powder and bismuth sulfide in a certain proportion to obtain a mixed powder. The mass ratio of the mixed powder is 5~10% for carbon powder, 85~90% for iron or iron oxide powder, and 5% for bismuth sulfide. In this embodiment, the bismuth sulfide is used as a functional additive, and its mechanism of action includes: increasing the hydrogen evolution overpotential of the electrode and inhibiting the generation of hydrogen gas by water decomposition during charging and discharging; its uniform dispersion in the electrode can modify the surface of iron particles and slow down the excessive growth of the iron oxide passivation layer; and its synergistic effect with the PVB binder network can enhance the overall structural toughness of the electrode and buffer the stress of volume change.
[0020] Furthermore, as a specific implementation method, the mass range of carbon powder, iron or iron oxide, and bismuth sulfide used in preparing carbon / iron or iron oxide sheet materials is 3.3g~3.5g, 26g~28g, and 1.65g~1.7g.
[0021] Weigh carbon and iron or iron oxide powder according to the preset ratio, and ball mill the carbon powder and iron or iron oxide powder separately in a ball mill for 1±0.5h. Mix the ball-milled powder and put it into a centrifuge to stir for 3~4 hours. Polyvinyl butyral (PVB) is dissolved in ethanol to form a binder solution; the mixed powder is then mixed with the binder solution to prepare a mixed slurry. The mass ratio of PVB to ethanol in the binder solution is 1:(4~6).
[0022] In step S3, the mixed slurry is poured into the casting mold and scraped flat into a wet film using a scraper. The thickness of the metal sheet is controlled to be 1.4~1.6mm by the scraper.
[0023] In this embodiment, the particle size range of the iron or iron oxide powder is 0.5μm to 10μm; the particle size range of the carbon powder is 40nm to 50nm; and the purity of the bismuth sulfide powder is not less than 99.9%.
[0024] The carbon / iron or iron oxide sheet material after casting is dried to obtain a carbon / iron or iron oxide sheet material with high mechanical strength. Specifically, the cast slurry is placed in an oven and dried at a temperature of 20~25℃ for 3~4 hours to prepare the carbon / iron or iron oxide sheet material. The final microstructure of the metal electrode in the prepared metal-air battery is as follows: Figure 1 As shown, in the discharge state, the negative electrode of a metal-air battery releases metal ions into the electrolyte, while the positive electrode (air electrode) absorbs oxygen. These metal ions move in the electrolyte, eventually reaching the positive electrode and reacting with oxygen to form metal oxides and water, releasing electrons and generating electrical energy. The charging process is the reverse of the discharging process. During charging, the metal oxides and water decompose into metal ions and oxygen; the metal ions return to the negative electrode, and the oxygen returns to the positive electrode. This process is reversible, ensuring the battery's cyclical use.
[0025] Example 1 This embodiment discloses a method for preparing a metal electrode for a metal-air battery, comprising the following steps: preparing a mixed slurry, ball milling, casting, and drying, specifically including the following steps: Ferric oxide powder is mixed with carbon powder and bismuth sulfide in a certain proportion to form a mixed powder. The iron powder is spherical with a particle size of 3-5 micrometers, the bismuth sulfide has a purity of 99.9%, and the carbon powder has a particle size of 40-50 nanometers. The mixed powder is calculated by mass ratio, with carbon powder, ferric oxide powder and bismuth sulfide accounting for 10%, 85% and 5% respectively. Weigh carbon powder and iron oxide powder in a preset ratio, and ball mill the carbon powder and iron oxide powder separately in a ball mill for 1 hour. Mix the ball-milled powders and put them into a centrifuge to stir for 3 hours. An adhesive was prepared by mixing 1g of PVB with 5g of ethanol. After the above mixture is ball-milled, the slurry is poured into a casting mold for casting, and the thickness of the metal sheet is 1.4 mm. The drying process for the cast carbon / iron oxide sheet material is as follows: the cast slurry is placed in an oven and dried at a temperature of 20~25℃ for 3 hours to prepare the carbon / iron oxide sheet material.
[0026] The charge-discharge cycle curve of the finally prepared metal-air battery under ideal conditions is as follows: Figure 2 As shown in the figure, the final metal-air battery remains stable after approximately 120 hours of cyclic charge-discharge.
[0027] Example 2 This embodiment discloses a method for preparing a metal electrode for a metal-air battery, comprising the following steps: preparing a mixed slurry, ball milling, casting, and drying, specifically including the following steps: Iron powder, carbon powder, and bismuth sulfide are mixed in a certain proportion to form a mixed powder, with the proportions of carbon powder, iron powder, and bismuth sulfide being 5%, 90%, and 5%, respectively. Furthermore, as a specific implementation method, the mass range of carbon powder and iron powder used to prepare carbon / iron sheet materials is 1.55g, 28g, and 1.55g.
[0028] Weigh carbon powder and iron powder according to the preset ratio, and ball mill the carbon powder and iron powder separately in a ball mill for 1 hour. Then mix the ball-milled powders and put them into a centrifuge to stir for 3 hours. A binder was prepared by mixing 1g of PVB with ethanol. After the above mixture is ball-milled, the mixed powder is poured into a casting mold for casting operation, and the thickness of the metal sheet is 1.5 mm. The drying process for the cast carbon / iron sheet material is as follows: the cast slurry is placed in an oven and dried at a temperature of 20~25℃ for 3 hours to prepare the carbon / iron sheet material.
[0029] Example 3 This embodiment discloses a method for preparing a metal electrode for a metal-air battery, comprising the following steps: preparing a mixed slurry, ball milling, casting, and drying, specifically including the following steps: Iron oxide, carbon powder, and bismuth sulfide are mixed in a certain proportion to form a mixed powder. The average particle size of the iron oxide powder is 10 micrometers, the purity of the bismuth sulfide is 99.9%, and the particle size of the carbon powder is 40-50 nanometers. The mass ratio of the mixed powder is 10%, 85%, and 5% for carbon powder, iron oxide powder, and bismuth sulfide, respectively. An adhesive was prepared by mixing 1g of PVB with 5g of ethanol. Weigh carbon powder and iron oxide powder in a preset ratio, and ball mill the carbon powder and iron oxide powder separately in a ball mill for 1.5 hours. Then mix the ball-milled powders and put them into a centrifuge to stir for 4 hours. After the above mixture is ball-milled, the mixed powder is poured into a casting mold for casting, and the thickness of the metal sheet is 1.6 mm. The drying of the cast carbon / iron oxide sheet material is specifically as follows: the cast slurry is placed in an oven and dried at a temperature of 25°C for 3 hours to prepare the carbon / iron oxide sheet material. Example 4 This embodiment discloses a method for preparing a metal electrode for a metal-air battery, comprising the following steps: preparing a mixed slurry, ball milling, casting, and drying, specifically including the following steps: Ferric oxide, carbon powder, and bismuth sulfide are mixed in a certain proportion to form a mixed powder. The ferric oxide powder is spherical iron powder with an average particle size of 1 micrometer. The bismuth sulfide has a purity of 99.9%. The carbon powder has a particle size of 40-50 nanometers. The mixed powder is calculated by mass ratio, with carbon powder, ferric oxide powder, and bismuth sulfide accounting for 5%, 90%, and 5%, respectively. Weigh carbon powder and ferric oxide powder in a preset ratio, and ball mill the carbon powder and ferric oxide powder separately in a ball mill for 1.5 hours. Then mix the ball-milled powders and put them into a centrifuge to stir for 4 hours. An adhesive was prepared by mixing 1.5g of PVB with 5g of ethanol. After the above mixture is ball-milled, the mixed powder is poured into a casting mold for casting, and the thickness of the metal sheet is 1.5 mm. The drying of the cast carbon / iron or iron oxide sheet material is specifically as follows: the cast slurry is placed in an oven and dried at a temperature of 25°C for 4 hours to prepare carbon / iron oxide sheet material. Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a metal electrode for a metal-air battery, characterized in that, The process includes the following steps: preparing the mixed slurry, ball milling, casting, and drying, specifically including the following steps: S1. Mix iron or iron oxide with carbon powder and bismuth sulfide in a certain proportion to obtain a mixed powder; S2. Dissolve polyvinyl butyral in ethanol to form a binder solution; mix the mixed powder with the binder solution to prepare a mixed slurry; S3. After ball milling the above mixed slurry, cast it into sheet material in a mold using the casting method; S4. Dry the cast sheet material to obtain carbon / iron or iron oxide sheet material.
2. The method according to claim 1, characterized in that, The mass ratio of the mixed powder material is as follows: carbon powder to iron or iron oxide powder to bismuth sulfide is 5~10% : 85~90% : 5%.
3. The method according to claim 1, characterized in that, Step S1 is as follows: Weigh carbon powder, iron or iron oxide powder, and bismuth sulfide according to the preset ratio, and ball mill the carbon powder, iron or iron oxide powder, and bismuth sulfide in a ball mill for 1 ± 0.5 h. Mix the ball-milled powders and put them into a centrifuge to stir for 3 to 4 hours.
4. The method according to claim 1, characterized in that, In step S3, the mixed slurry is poured into the casting mold and scraped flat into a wet film using a scraper. The thickness of the metal sheet is controlled to be 1.4~1.6mm by the scraper.
5. The method according to claim 1, characterized in that, In step S4, the cast slurry is placed in an oven and dried at 20-25°C for 3-4 hours to obtain a carbon / iron or iron oxide composite electrode sheet.
6. A metal electrode for a metal-air battery, characterized in that, It is prepared by any one of claims 1 to 5.
Citation Information
Patent Citations
Low-cost metal electrode
CN114467208A
Rechargeable battery using iron negative electrode and manganese oxide positive electrode
US20210028452A1