High-haze optical diffusion film and preparation method thereof
Patent Information
- Application Number
- CN202610691285.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-19
- Publication Date
- 2026-09-08
- Estimated Expiration
- 2046-05-19
AI Technical Summary
然而,其模压工艺需要在上压辊粘附一层“模压用扩散膜”,依然使用二甲苯等有机溶剂,且需要先制成成品膜再进行压辊粘附,工艺繁琐,增加了生产成本和环境负担
1、本发明通过共挤出以及单次涂覆的方式制备了一种由PET基材层和两层扩散层构成的复合光学膜,第一扩散层采用小粒径多孔粒子,第二扩散层则采用较大粒径复合粒子,使入射光光线经历先均匀、后强散的路径,避免了单层强散射导致的光能回反损失,有效提升雾度的同时,使透光率仍在85%左右;
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyester film technology, specifically to a high-haze optical diffusion film and its preparation method. Background Technology
[0002] Currently, the polyester films used in the market are usually made of polyethylene terephthalate (PET), a colorless, transparent, and glossy film with good mechanical properties, high hardness and toughness, excellent puncture and abrasion resistance, and high light transmittance, low haze, and high brightness. Therefore, it is often used to manufacture optical films. Currently, PET optical films are mainly used in downstream markets such as liquid crystal displays and organic light-emitting diode displays, for example, as diffusion films and bulking films.
[0003] The quality and stability of PET film directly affect the performance and application effects of downstream products. Therefore, it is necessary to modify PET film for different application scenarios. For example, diffusion film consists of an anti-adhesion layer, a substrate layer, and a light diffusion layer. Patent CN114578465B discloses a PET-based diffusion film and its preparation method. The PET film includes a three-layer composite structure of A / B / C. One of the core technologies is to form a semi-concave spherical pattern with light diffusion effect on the A layer through a molding process, replacing the traditional coating process. This patent claims to have produced a diffusion film with high light transmittance, haze, and brightness, without the use of organic solvents, making it safe and environmentally friendly. However, its molding process requires adhering a layer of "molding diffusion film" to the upper pressure roller, which still uses organic solvents such as xylene. Furthermore, it requires the finished film to be made first before the pressure roller is adhered, making the process cumbersome and increasing production costs and environmental burden. Patent CN112882142B describes a wear-resistant and light-diffusing film and its preparation method. This method involves forming multiple functional layers by coating the upper and lower surfaces of a PET substrate layer multiple times. The process is lengthy, and the multiple coatings increase the complexity of the equipment and the production cost. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention aims to prepare a high-haze optical diffusion film by simplifying the process and combining double-layer co-extrusion and coating processes.
[0005] To achieve the above objectives, the present invention provides the following technical solution: A high-haze optical diffusion film includes a PET substrate layer, wherein a first diffusion layer is bonded to the upper surface of the PET substrate layer by co-extrusion, and a second diffusion layer is bonded to the lower surface by coating; the first diffusion layer includes a thermoplastic resin and first diffusion particles; the second diffusion layer includes a UV-curable resin, second diffusion particles, silicone-modified nano-ATO antistatic agent, reactive diluent, lubricant, photoinitiator, and crosslinking curing agent. The preparation process of the first diffused particle is as follows: firstly, PS seed microspheres are prepared by dispersion polymerization, then porous microspheres are prepared by swelling polymerization, and finally, nano-silica particles are deposited on its surface to obtain the particle. The second diffused particles are obtained by adsorbing monodisperse PS microspheres in PDADMAC aqueous solution to obtain positively charged PS microspheres, and then electrostatically self-assembling and adsorbing them with SiO2 aqueous dispersion.
[0006] Furthermore, the PET substrate layer is prepared by blending and granulating optical-grade PET chips with 2wt% sodium isophthalate-5-sulfonate using a screw extruder to obtain PET masterbatch.
[0007] Furthermore, the mass ratio of the thermoplastic resin to the first diffusion particles in the first diffusion layer is 100:5~20; its thickness is 5~10 μm; and the thermoplastic resin is PETG resin.
[0008] Furthermore, the preparation process of the first diffusing particle is as follows: S1-1. Add ethanol / deionized water mixed solvent to the reaction flask, add polyvinylpyrrolidone and stir evenly, heat to 70℃, add styrene monomer and azobisisobutyronitrile initiator, polymerize under nitrogen protection for 12h, centrifuge the obtained product, wash with ethanol and dry to obtain seed microspheres, disperse them in polyvinylpyrrolidone aqueous solution and stir evenly for later use. S1-2. Add toluene, styrene, benzoyl peroxide and divinylbenzene to the reaction flask and stir until they are evenly mixed. Emulsify evenly in an aqueous solution containing sodium dodecyl sulfate. Slowly add to the seed microsphere dispersion and stir at room temperature to swell for 12-24 h. Heat to 70℃ and polymerize for 24 h. Centrifuge to collect the microspheres. S1-3. The collected microspheres are redispersed in a mixed solvent of ethanol / deionized water. Tetraethyl orthosilicate and ammonia are added. The mixture is stirred at room temperature to allow the SiO2 generated by the hydrolysis of tetraethyl orthosilicate to be deposited on the surface of the microspheres and the inner wall of the pores. The microspheres are then separated by centrifugation and extracted to obtain the final product.
[0009] Furthermore, the preparation process of the first diffusing particle is as follows: S1-1. Add 100 mL of a 1:1 mixture of ethanol and deionized water to a reaction flask, add 1.2 g of polyvinylpyrrolidone and stir until homogeneous. Heat to 70 °C, add 10-20 g of styrene monomer and 0.05-0.2 g of azobisisobutyronitrile initiator, and polymerize under nitrogen protection for 12 h. Centrifuge the obtained product, wash with ethanol and dry to obtain seed microspheres; take 10 g and disperse in 400 mL of an aqueous solution containing 1 wt% PVA, stir until homogeneous and set aside. S1-2. Add 20-30g toluene, 40-50g styrene, 1-3g benzoyl peroxide and 2-4g divinylbenzene to the reaction flask and stir until they are evenly mixed. Then emulsify in 100mL of 0.2wt% sodium dodecyl sulfonate aqueous solution, and then dropwise add to the seed microsphere dispersion. Stir and swell at room temperature for 12-24h, raise the temperature to 70℃, and polymerize under nitrogen protection for 24h. Collect the microspheres by centrifugation and dry at low temperature. S1-3. The collected microspheres (5g) were redispersed in 100 mL of a 1:1 mixture of ethanol and deionized water, 5 mL of tetraethyl orthosilicate and 1 mL of ammonia were added, and the mixture was stirred at room temperature for 6-8 h. After centrifugation and washing with water, the microspheres were placed in a Soxhlet extractor and extracted with anhydrous ethanol. After vacuum drying at 50 °C, porous core-shell composite microspheres, i.e., the first diffusion particles, were obtained.
[0010] Further, the second diffusion layer, by weight fraction, comprises 40-70 parts UV-curable resin, 10-30 parts second diffusion particles, 1-4 parts silicone-modified nano-ATO antistatic agent, 10-30 parts reactive diluent, 0.1-0.5 parts lubricant, 1-3 parts photoinitiator, and 1-5 parts crosslinking curing agent; the dry film thickness is 8-12 μm.
[0011] Furthermore, the organosilicon-modified nano-ATO antistatic agent is obtained by reacting a mixture of methacryloyloxypropyltrimethoxysilane and dodecyl dimethyl (3-trimethoxysilylpropyl)ammonium chloride (Si-QAS) with nano-ATO.
[0012] Furthermore, the reactive diluent is selected from one of isobornyl methacrylate, β-hydroxyethyl methacrylate, and 1,6-hexanediol diacrylate; the lubricant is a fluorocarbon lubricant; the photoinitiator is TPO; and the crosslinking curing agent is dipentaerythritol hexaacrylate.
[0013] Furthermore, the preparation process of the second diffused particle is as follows: S2-1. Take monodisperse PS microspheres with a particle size of 10~20 μm and disperse them in 0.2wt% PDADMAC aqueous solution. Stir at room temperature for 60~120 min, centrifuge, wash with water and dry to obtain positively charged PS microspheres. S2-2. Take nano-SiO2 and ultrasonically disperse it in deionized water. Adjust the pH to 7.5-8.0 with ammonia water and ultrasonically disperse for 30 min to obtain a stable dispersion with a solid content of 1wt%. S2-3. The positively charged PS microspheres are redispersed in deionized water and added dropwise to the stable dispersion in S2-2 while stirring. The mass ratio of SiO2 to PS microspheres is 1:10~15. After the addition is complete, continue stirring at room temperature for 1 hour, centrifuge, wash with water and dry under low temperature vacuum.
[0014] A second objective of this invention is to provide a method for preparing a high-haze optical diffusion film as described above, comprising the following steps: 1) The PET substrate layer raw material and the first diffusion layer raw material are dried separately and then fed into a twin-screw extruder. They are then co-extruded through a multi-layer co-extrusion T-die to form an AB composite film casting. 2) The cast sheet is biaxially stretched and cooled to obtain a film with a total thickness of 50~70μm. The PET substrate layer of the film is then subjected to corona treatment. 3) Preparation of coating solution: Add the second diffusion particles, silicone-modified nano-ATO antistatic agent and lubricant to the reactive diluent in sequence and disperse them evenly at high speed. Then add the UV curing resin, crosslinking curing agent and photoinitiator to the above dispersion slurry and continue to stir evenly. 4) The coating liquid is applied to the surface of the corona-treated PET substrate by slit extrusion coating; the final optical film is obtained by curing under nitrogen protection using a UV curing system.
[0015] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention prepares a composite optical film consisting of a PET substrate layer and two diffusion layers by co-extrusion and single coating. The first diffusion layer uses small-diameter porous particles, while the second diffusion layer uses larger-diameter composite particles. This allows the incident light to follow a path that is first uniform and then strongly diffused, avoiding the light energy reflection loss caused by strong scattering in a single layer. This effectively improves the haze while keeping the light transmittance at around 85%. 2. Silicone-modified nano-ATO is used as an antistatic agent for the optical diffusion film. This antistatic agent has good dispersibility in solvent-free coatings and enhances the bonding with the PET substrate layer, so that the film has antistatic properties and its stability under high temperature and high humidity conditions is also improved. 3. The addition of sodium isophthalate-5-sulfonate to the PET substrate layer significantly improves the adhesion to the first diffusion layer of PETG and the second diffusion layer of UV resin; 4. The one-time coating process reduces equipment and production costs. The first layer is co-extruded without solvents, and the second layer is cured with solvent-free UV curing, which significantly reduces the environmental burden. Detailed Implementation
[0016] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0017] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0018] Example: A high-haze optical diffusion film includes a PET substrate layer, wherein a first diffusion layer is bonded to the upper surface of the PET substrate layer by co-extrusion, and a second diffusion layer is bonded to the lower surface by coating; The PET substrate layer is prepared by blending and granulating optical-grade PET chips with 2wt% sodium isophthalate-5-sulfonate using a screw extruder to obtain PET masterbatch; The first diffusion layer comprises PETG resin and first diffusion particles in a mass ratio of 100:5~20; and has a thickness of 5~10μm. The second diffusion layer comprises 40-70 parts of UV-curable resin, 10-30 parts of second diffusion particles, 1-4 parts of silicone-modified nano-ATO antistatic agent, 10-30 parts of reactive diluent, 0.1-0.5 parts of lubricant, 1-3 parts of photoinitiator, and 1-5 parts of crosslinking curing agent; the dry film thickness is 8-12 μm.
[0019] The preparation process of the first diffused particle is as follows: S1-1. Add 100 mL of a 1:1 mixture of ethanol and deionized water to a reaction flask, add 1.2 g of polyvinylpyrrolidone and stir until homogeneous. Heat to 70 °C, add 10-20 g of styrene monomer and 0.05-0.2 g of azobisisobutyronitrile initiator, and polymerize under nitrogen protection for 12 h. Centrifuge the obtained product, wash with ethanol and dry to obtain seed microspheres; take 10 g and disperse in 400 mL of an aqueous solution containing 1 wt% PVA, stir until homogeneous and set aside. S1-2. Add 20-30g toluene, 40-50g styrene, 1-3g benzoyl peroxide and 2-4g divinylbenzene to the reaction flask and stir until they are evenly mixed. Then emulsify in 100 mL of 0.2wt% sodium dodecyl sulfonate aqueous solution, and then dropwise add to the seed microsphere dispersion. Stir and swell at room temperature for 12-24 h, raise the temperature to 70℃, and polymerize under nitrogen protection for 24 h. Collect the microspheres by centrifugation and dry at low temperature. S1-3. The collected microspheres (5g) were redispersed in 100 mL of a 1:1 mixture of ethanol and deionized water, 5 mL of tetraethyl orthosilicate and 1 mL of ammonia were added, and the mixture was stirred at room temperature for 6-8 h. After centrifugation and washing with water, the microspheres were placed in a Soxhlet extractor and extracted with anhydrous ethanol. After vacuum drying at 50 °C, porous core-shell composite microspheres, i.e., the first diffusion particles, were obtained.
[0020] The preparation process of the second diffused particle is as follows: S2-1. Take monodisperse PS microspheres with a particle size of 10~20 μm and disperse them in 0.2wt% PDADMAC aqueous solution. Stir at room temperature for 60~120 min, centrifuge, wash with water and dry to obtain positively charged PS microspheres. S2-2. Take nano-SiO2 and ultrasonically disperse it in deionized water. Adjust the pH to 7.5-8.0 with ammonia water and ultrasonically disperse for 30 min to obtain a stable dispersion with a solid content of 1wt%. S2-3. The positively charged PS microspheres are redispersed in deionized water and added dropwise to the stable dispersion in S2-2 while stirring. The mass ratio of SiO2 to PS microspheres is 1:10~15. After the addition is complete, continue stirring at room temperature for 1 hour, centrifuge, wash with water and dry under low temperature vacuum.
[0021] The raw materials used in the above embodiments, such as styrene and methyl methacrylate, are conventional reagents, purchased from brands such as Sinopharm Group and Aladdin, and will not be described in detail in this application. Other raw materials are shown in Table 1.
[0022] In addition, it should be noted that the term "parts" as used in this article refers to "parts by weight".
[0023] Table 1
[0024] Example 1: S1, The preparation process of the first diffused particles is as follows: S1-1. Add 100 mL of a 1:1 mixture of ethanol and deionized water to a reaction flask, add 1.2 g of polyvinylpyrrolidone and stir until homogeneous. Heat to 70 °C, add 20 g of styrene monomer and 0.2 g of azobisisobutyronitrile initiator, and polymerize for 12 h under nitrogen protection. Centrifuge the product, wash with ethanol and dry to obtain seed microspheres (average particle size 2.5 μm). Take 10 g and disperse in 400 mL of an aqueous solution containing 1 wt% PVA, stir until homogeneous and set aside. S1-2. Add 20 g toluene, 40 g styrene, 2 g benzoyl peroxide and 2 g divinylbenzene to the reaction flask and stir until they are evenly mixed. Then emulsify in 100 mL of 0.2 wt% sodium dodecyl sulfonate aqueous solution, and then dropwise add to the seed microsphere dispersion. Stir and swell at room temperature for 24 h, raise the temperature to 70 °C, and polymerize under nitrogen protection for 24 h. Collect the microspheres by centrifugation and dry at low temperature. S1-3. 5 g of the collected microspheres were redispersed in 100 mL of a 1:1 (v / v) ethanol / deionized water mixture. 5 mL of tetraethyl orthosilicate and 1 mL of ammonia were added. The mixture was stirred at room temperature for 6–8 h, centrifuged, washed with water, and then placed in a Soxhlet extractor for extraction with anhydrous ethanol. The microspheres were then vacuum dried at 50 °C to obtain porous core-shell composite microspheres, i.e., the first diffused particles, with a particle size of approximately 5.5 μm and a specific surface area ≥40 m². 2 / g.
[0025] S2. The preparation process for the second diffused particles is as follows: S2-1. Disperse monodisperse PS microspheres with a particle size of 15 μm in 200 mL of 0.2 wt% PDADMAC aqueous solution, stir at room temperature for 90 min, centrifuge, wash with water and dry to obtain positively charged PS microspheres. S2-2. Take nano-SiO2 and ultrasonically disperse it in deionized water. Adjust the pH to 7.5-8.0 with ammonia water and ultrasonically disperse for 30 min to obtain a stable dispersion with a solid content of 1wt%. S2-3. The positively charged PS microspheres are redispersed in deionized water and added dropwise to the stable dispersion in S2-2 while stirring. The mass ratio of SiO2 to PS microspheres is 1:10. After the addition is complete, continue stirring at room temperature for 1 hour, centrifuge, wash with water and dry under low temperature vacuum.
[0026] S3. Preparation of organosilicon-modified nano-ATO antistatic agent Take 10 g of nano-ATO and disperse it in 100 mL of anhydrous ethanol, and sonicate for 30 min; dissolve 0.12 g of KH570 and 0.05 g of Si-QAS in 2 mL of ethanol, slowly add them dropwise to the above ATO suspension, reflux for 12 h, centrifuge, wash with ethanol and dry to obtain the final product.
[0027] S4. Preparation of optical film S4-1, PET substrate layer raw material: 100 parts of optical grade PET chips and 2 parts of sodium isophthalate-5-sulfonate are weighed and blended and granulated by screw extruder to obtain PET masterbatch; First diffusion layer raw material: 100 parts of PETG resin and 5 parts of first diffusion particles are weighed; The PET substrate layer raw material and the first diffusion layer raw material are dried separately and fed into a twin-screw extruder, and co-extruded through a multi-layer co-extrusion T-die to form an AB composite film casting sheet; S4-2. The cast sheet is biaxially stretched at a temperature of 80 °C and a stretch ratio of 3.4 in the longitudinal direction, and at a temperature of 110 °C and a stretch ratio of 4.0 in the transverse direction. The heat setting temperature is 220 °C, and the film is cooled and set to obtain a film with a total thickness of 70 μm (the thickness of the first diffusion layer is 5 μm). The PET substrate layer of the film is then subjected to corona treatment. S4-3 Preparation of coating solution: Add 10 parts of second diffusion particles, 3 parts of organosilicon modified nano-ATO antistatic agent, and 0.5 parts of fluorocarbon lubricant to 30 parts of isobornyl methacrylate in sequence and disperse evenly at high speed. Then add 70 parts of UV curing resin, 5 parts of crosslinking curing agent dipentaerythritol hexaacrylate, and 3 parts of photoinitiator TPO to the above dispersion slurry and continue to stir evenly. S4-4. Using a slot extrusion coating method, the coating liquid is applied to the surface of the corona-treated PET substrate; under nitrogen protection, it is cured by a UV curing system to obtain the final optical film.
[0028] Example 2: S1-S3 are the same as in Example 1.
[0029] S4. Preparation of optical film S4-1, PET substrate layer raw material: Weigh 100 parts of optical grade PET chips and 2 parts of sodium isophthalate-5-sulfonate, and granulate them by screw extruder to obtain PET masterbatch; First diffusion layer raw material: Weigh 100 parts of PETG resin and 12 parts of first diffusion particles; Dry the PET substrate layer raw material and the first diffusion layer raw material separately and feed them into a twin-screw extruder, and co-extrude them through a multi-layer co-extrusion T-die to form an AB composite film casting sheet; S4-2. The cast sheet is biaxially stretched at a temperature of 80 °C and a stretch ratio of 3.4 in the longitudinal direction, and at a temperature of 110 °C and a stretch ratio of 4.0 in the transverse direction. The heat setting temperature is 220 °C, and the film is cooled and set to obtain a film with a total thickness of 70 μm. The PET substrate layer of the film is then subjected to corona treatment. S4-3. Preparation of coating solution: Add 20 parts of second diffusion particles, 3 parts of organosilicon modified nano-ATO antistatic agent, and 0.5 parts of fluorocarbon lubricant to 30 parts of isobornyl methacrylate in sequence and disperse evenly at high speed. Then add 70 parts of UV curing resin, 5 parts of crosslinking curing agent dipentaerythritol hexaacrylate, and 3 parts of photoinitiator TPO to the above dispersion slurry and continue to stir evenly. S4-4. Using a slot extrusion coating method, the coating liquid is applied to the surface of the corona-treated PET substrate; under nitrogen protection, it is cured by a UV curing system to obtain the final optical film.
[0030] Example 3: S1-S3 are the same as in Example 1.
[0031] S4. Preparation of optical film S4-1, PET substrate layer raw material: Weigh 100 parts of optical grade PET chips and 2 parts of sodium isophthalate-5-sulfonate, and granulate them by screw extruder to obtain PET masterbatch; First diffusion layer raw material: Weigh 100 parts of PETG resin and 20 parts of first diffusion particles; Dry the PET substrate layer raw material and the first diffusion layer raw material separately and feed them into a twin-screw extruder, and co-extrude them through a multi-layer co-extrusion T-die to form an AB composite film casting sheet; S4-2. The cast sheet is biaxially stretched at a temperature of 80 °C and a stretch ratio of 3.4 in the longitudinal direction, and at a temperature of 110 °C and a stretch ratio of 4.0 in the transverse direction. The heat setting temperature is 220 °C, and the film is cooled and set to obtain a film with a total thickness of 70 μm. The PET substrate layer of the film is then subjected to corona treatment. S4-3. Preparation of coating solution: Add 30 parts of second diffusion particles, 3 parts of organosilicon modified nano-ATO antistatic agent, and 0.5 parts of fluorocarbon lubricant to 30 parts of isobornyl methacrylate in sequence and disperse evenly at high speed. Then add 70 parts of UV curing resin, 5 parts of crosslinking curing agent dipentaerythritol hexaacrylate, and 3 parts of photoinitiator TPO to the above dispersion slurry and continue to stir evenly. S4-4. Using a slot extrusion coating method, the coating liquid is applied to the surface of the corona-treated PET substrate; under nitrogen protection, it is cured by a UV curing system, and the final optical film is obtained with a dry film thickness of 8μm.
[0032] Example 4: Same as Example 1, except that in S1, the preparation process of the first diffused particle is as follows: S1-1. Add 100 mL of a 1:1 mixture of ethanol and deionized water to a reaction flask, add 1.2 g of polyvinylpyrrolidone and stir until homogeneous. Heat to 70 °C, add 20 g of styrene monomer and 0.2 g of azobisisobutyronitrile initiator, and polymerize for 12 h under nitrogen protection. Centrifuge the product, wash with ethanol and dry to obtain seed microspheres (average particle size 2.5 μm). Take 10 g and disperse in 400 mL of an aqueous solution containing 1 wt% PVA, stir until homogeneous and set aside. S1-2. Add 30 g toluene, 50 g styrene, 2 g benzoyl peroxide and 2 g divinylbenzene to the reaction flask and stir until they are evenly mixed. Then emulsify in 100 mL of 0.2 wt% sodium dodecyl sulfonate aqueous solution, and then dropwise add to the seed microsphere dispersion. Stir and swell at room temperature for 24 h, raise the temperature to 70 °C, and polymerize under nitrogen protection for 24 h. Collect the microspheres by centrifugation and dry at low temperature. S1-3. 5g of the collected microspheres were redispersed in 100 mL of a 1:1 (v / v) ethanol / deionized water mixture. 5 mL of tetraethyl orthosilicate and 1 mL of ammonia were added. The mixture was stirred at room temperature for 6–8 h, centrifuged, washed with water, and then placed in a Soxhlet extractor for extraction with anhydrous ethanol. The microspheres were then vacuum dried at 50 °C to obtain porous core-shell composite microspheres, i.e., the first diffused particles, with a particle size of approximately 7.5 μm and a specific surface area ≥40 m². 2 / g.
[0033] Example 5: Same as Example 1, except for S2. The preparation process for the second diffused particles is as follows: S2-1. Disperse monodisperse PS microspheres with a particle size of 15 μm in 200 mL of 0.2 wt% PDADMAC aqueous solution, stir at room temperature for 90 min, centrifuge, wash with water and dry to obtain positively charged PS microspheres. S2-2. Take nano-SiO2 and ultrasonically disperse it in deionized water. Adjust the pH to 7.5-8.0 with ammonia water and ultrasonically disperse for 30 min to obtain a stable dispersion with a solid content of 1wt%. S2-3. The positively charged PS microspheres are redispersed in deionized water and added dropwise to the stable dispersion in S2-2 while stirring. The mass ratio of SiO2 to PS microspheres is 1:15. After the addition is complete, continue stirring at room temperature for 1 hour, centrifuge, wash with water, and dry under low temperature vacuum.
[0034] Comparative Example 1: Same as Example 1, except that the PET substrate layer is made of pure PET chips.
[0035] Comparative Example 2: Same as Example 1, except that the first diffusing particle is the seed microsphere obtained in step S1-1.
[0036] Comparative Example 3: Same as Example 1, except that the first diffusing particle is the swollen microspheres obtained in step S1-2.
[0037] Comparative Example 4: Same as Example 1, except that the second diffusion particles are 9 parts monodisperse PS microspheres and 1 part nano silica.
[0038] Comparative Example 5: Same as Example 1, except that the second diffusion layer was not coated.
[0039] Comparative Example 6: Same as Example 1, except that the antistatic agent is unmodified nano-ATO.
[0040] Haze and transmittance: The transmittance / haze was measured using a WGT-S type transmittance / haze meter (Shanghai Precision Scientific Instruments Co., Ltd.); three points were taken from the center and edge of each sample, and the average value was taken.
[0041] Surface resistivity: The surface resistance of the second diffusion layer was measured using an ACL-385 surface resistivity tester, with 5 points measured for each sample and the average value taken.
[0042] Stability in high temperature and high humidity environments: The film was placed at 85℃ / 85%RH for 72h, and the surface resistance was measured. The retention rate (resistivity to high temperature and high humidity %) was calculated as (resistivity after treatment / initial resistivity) × 100%.
[0043] Peel strength: Using a universal testing machine, the 180° peel strength between the first diffusion layer and the PET substrate layer was tested according to GB / T 8808-2023. The sample width was 25 mm, the peel speed was 50 mm / min, and the average peak load was taken 5 times. The unit is N / cm.
[0044] Abrasion resistance: The test was conducted according to the test method described in patent CN113881090B. The UV resin layer of the diffusion film was placed statically on the light-emitting surface of the light guide plate, and a 500-gram weight was placed on the optical diffuser. The diffusion film was dragged back and forth several times to examine the damage to the diffusion film and the light guide plate. No visible scratches were considered "excellent", slight scratches were considered "good", and obvious scratches were considered "poor".
[0045] The results are recorded in Table 2.
[0046] Table 2
[0047] The first diffusion layer of this invention uses porous core-shell structured silica-styrene microspheres as diffusion particles. Their internal pore structure enhances scattering ability, improving haze with a low addition amount and reducing negative impacts on transmittance. Using unswollen, dense seed microspheres (Comparative Example 2) weakens scattering ability, resulting in poor haze improvement. Swollen porous PS microspheres (Comparative Example 3) exhibit improved scattering ability, thus achieving better haze than Comparative Example 2, but still lower than Examples 1-5. Furthermore, Comparative Examples 2 and 3 show better transmittance than Examples 1-5. Comparative Examples 4 and 5 examine the second diffusion layer, demonstrating its indispensable contribution to high haze.
[0048] In this invention, both the first and second diffusing particles involve PS microspheres and SiO2 components, but their microstructure design and functional positioning are completely different: the first diffusing particle uses a process of swelling polymerization to create pores and depositing SiO2 on the inner wall of the pores, aiming to build an internal porous structure to maximize scattering efficiency, while forming surface roughness to facilitate co-extrusion; the second diffusing particle uses an electrostatic self-assembly process to attach SiO2 to the surface of a dense PS large-particle core, aiming to achieve large-angle scattering through the dense core and provide wear-resistant protection through the shell layer. Comparative Example 5, without the second diffusing layer coating, clearly failed the wear resistance test on the PET substrate layer, showing poor performance; Comparative Example 4 directly uses PS microspheres and silica particles as diffusing particles, which are physically mixed. The free silica particles are prone to agglomeration in the coating liquid, resulting in poor coating surface uniformity and therefore relatively poor wear resistance.
[0049] The organosilicon-modified nano-ATO, used as an antistatic agent, effectively exerted its antistatic properties. Except for comparative examples 5 and 6, the surface resistivity was all above 3 × 10⁻⁶. 9 The magnitude change is negligible; in comparison, unmodified nano-ATO was selected for example, although it was also around 10. 9 The magnitude of the modified nano-ATO is much higher than that of Examples 1-5. In addition, the modified nano-ATO is uniformly dispersed in the coating liquid and can bond well with the PET substrate layer after curing, thus exhibiting high stability. It can also maintain good antistatic effect in high temperature and high humidity environments, with a retention rate of over 90%, while the retention rate of Comparative Example 6 is only 82.3%.
[0050] Comparing Comparative Example 1 with the Example, adding an appropriate amount of sodium isophthalate-5-sulfonate to the PET substrate layer can also improve the interlayer adhesion strength.
[0051] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details.
Claims
1. A high-haze optical diffusion film, comprising a PET substrate layer, characterized in that, The upper surface of the PET substrate layer is bonded with a first diffusion layer by co-extrusion, and the lower surface is bonded with a second diffusion layer by coating. The first diffusion layer includes thermoplastic resin and first diffusion particles. The second diffusion layer includes UV-curable resin, second diffusion particles, silicone-modified nano-ATO antistatic agent, reactive diluent, lubricant, photoinitiator, and crosslinking curing agent. The preparation process of the first diffused particle is as follows: firstly, PS seed microspheres are prepared by dispersion polymerization, then porous microspheres are prepared by swelling polymerization, and finally, nano-silica particles are deposited on its surface to obtain the particle. The second diffused particles are obtained by adsorbing monodisperse PS microspheres in PDADMAC aqueous solution to obtain positively charged PS microspheres, and then electrostatically self-assembling and adsorbing them with SiO2 aqueous dispersion. The PET substrate layer is prepared by blending and granulating optical-grade PET chips with 2wt% sodium isophthalate-5-sulfonate using a screw extruder to obtain PET masterbatch. The mass ratio of the thermoplastic resin to the first diffusion particles in the first diffusion layer is 100:5~20; its thickness is 5~10μm; the thermoplastic resin is PETG resin; The second diffusion layer, by weight fraction, comprises 40-70 parts UV-curable resin, 10-30 parts second diffusion particles, 1-4 parts silicone-modified nano-ATO antistatic agent, 10-30 parts reactive diluent, 0.1-0.5 parts lubricant, 1-3 parts photoinitiator, and 1-5 parts crosslinking curing agent; the dry film thickness is 8-12 μm. The organosilicon-modified nano-ATO antistatic agent is obtained by reacting a mixture of methacryloyloxypropyltrimethoxysilane and dodecyl dimethyl (3-trimethoxysilylpropyl)ammonium chloride with nano-ATO.
2. The high-haze optical diffusion film according to claim 1, characterized in that, The preparation process of the first diffusing particle is as follows: S1-1. Add ethanol / deionized water mixed solvent to the reaction flask, add polyvinylpyrrolidone and stir evenly, heat to 70℃, add styrene monomer and azobisisobutyronitrile initiator, polymerize under nitrogen protection for 12h, centrifuge the obtained product, wash with ethanol and dry to obtain seed microspheres, disperse them in polyvinylpyrrolidone aqueous solution and stir evenly for later use. S1-2. Add toluene, styrene, benzoyl peroxide and divinylbenzene to the reaction flask and stir until they are evenly mixed. Emulsify evenly in an aqueous solution containing sodium dodecyl sulfate. Slowly add to the seed microsphere dispersion and stir at room temperature to swell for 12-24 h. Heat to 70℃ and polymerize for 24 h. Centrifuge to collect the microspheres. S1-3. The collected microspheres are redispersed in a mixed solvent of ethanol / deionized water. Tetraethyl orthosilicate and ammonia are added. The mixture is stirred at room temperature to allow the SiO2 generated by the hydrolysis of tetraethyl orthosilicate to be deposited on the surface of the microspheres and the inner wall of the pores. The microspheres are then separated by centrifugation and extracted to obtain the final product.
3. The high-haze optical diffusion film according to claim 2, characterized in that, The preparation process of the first diffusing particle is as follows: S1-1. Add 100 mL of a 1:1 mixture of ethanol and deionized water to a reaction flask, add 1.2 g of polyvinylpyrrolidone and stir until homogeneous. Heat to 70 °C, add 10-20 g of styrene monomer and 0.05-0.2 g of azobisisobutyronitrile initiator, and polymerize under nitrogen protection for 12 h. Centrifuge the obtained product, wash with ethanol and dry to obtain seed microspheres; take 10 g and disperse in 400 mL of an aqueous solution containing 1 wt% PVA, stir until homogeneous and set aside. S1-2. Add 20-30g toluene, 40-50g styrene, 1-3g benzoyl peroxide and 2-4g divinylbenzene to the reaction flask and stir until they are evenly mixed. Then emulsify in 100mL of 0.2wt% sodium dodecyl sulfonate aqueous solution, and then dropwise add to the seed microsphere dispersion. Stir and swell at room temperature for 12-24h, raise the temperature to 70℃, and polymerize under nitrogen protection for 24h. Collect the microspheres by centrifugation and dry at low temperature. S1-3. The collected microspheres (5g) were redispersed in 100 mL of a 1:1 mixture of ethanol and deionized water, 5 mL of tetraethyl orthosilicate and 1 mL of ammonia were added, and the mixture was stirred at room temperature for 6-8 h. After centrifugation and washing with water, the microspheres were placed in a Soxhlet extractor and extracted with anhydrous ethanol. After vacuum drying at 50 °C, porous core-shell composite microspheres, i.e., the first diffusion particles, were obtained.
4. The high-haze optical diffusion film according to claim 1, characterized in that, The reactive diluent is selected from one of isobornyl methacrylate, β-hydroxyethyl methacrylate, and 1,6-hexanediol diacrylate; the lubricant is a fluorocarbon lubricant; the photoinitiator is TPO; and the crosslinking curing agent is dipentaerythritol hexaacrylate.
5. The high-haze optical diffusion film according to claim 1, characterized in that, The preparation process of the second diffused particle is as follows: S2-1. Take monodisperse PS microspheres with a particle size of 10~20 μm and disperse them in 0.2wt% PDADMAC aqueous solution. Stir at room temperature for 60~120 min, centrifuge, wash with water and dry to obtain positively charged PS microspheres. S2-2. Take nano-SiO2 and ultrasonically disperse it in deionized water. Adjust the pH to 7.5-8.0 with ammonia water and ultrasonically disperse for 30 min to obtain a stable dispersion with a solid content of 1wt%. S2-3. The positively charged PS microspheres are redispersed in deionized water and added dropwise to the stable dispersion in S2-2 while stirring. The mass ratio of SiO2 to PS microspheres is 1:10~15. After the addition is complete, continue stirring at room temperature for 1 hour, centrifuge, wash with water and dry under low temperature vacuum.
6. A method for preparing a high-haze optical diffusion film according to any one of claims 1-5, characterized in that, Includes the following steps: 1) The PET substrate layer raw material and the first diffusion layer raw material are dried separately and then fed into a twin-screw extruder. They are then co-extruded through a multi-layer co-extrusion T-die to form an AB composite film casting. 2) The cast sheet is biaxially stretched and cooled to obtain a film with a total thickness of 50~70 μm. The PET substrate layer of the film is then subjected to corona treatment. 3) Preparation of coating solution: The second diffusion particles, silicone-modified nano-ATO antistatic agent and lubricant are added to the reactive diluent in sequence and dispersed at high speed to obtain a dispersion slurry. Then, the UV curing resin, crosslinking curing agent and photoinitiator are added to the above dispersion slurry and stirred evenly. 4) The coating liquid is applied to the surface of the corona-treated PET substrate using a slot extrusion coating method; The final optical film is obtained by curing under nitrogen protection using a UV curing system.
Citation Information
Patent Citations
Friction-resistant light diffusion film and method for manufacturing the same
CN112882142B
A diffusion membrane and its preparation method
CN113881090B
A PET-based diffusion film and its preparation method
CN114578465B
Optical diffusion film and preparation method thereof
CN102540291A
Porous core-shell SiO2 / PS microsphere light diffusion agent, preparation and application